Unsaturated silane-glycidyl azide polymer co-coated aluminum lithium alloy powder and preparation method thereof
Through unsaturated silane-polyazide glycidyl ether co-coated technology and precious metal catalyst adhesion, the problems of low combustion efficiency and poor stability of aluminum-lithium alloy powder in solid propellants are solved, and the combustion calorific value and stability are significantly improved. Improves the overall performance of propellant.
Patent Information
- Application Number
- CN202411023326.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The application of traditional aluminum powder in solid propellants has problems such as high ignition temperature, long delay time, slow combustion speed and surface agglomeration, resulting in low combustion efficiency; while the high reactivity of aluminum-lithium alloy powder leads to structural defects such as pore cracks, which affects stability. Sex and compatibility.
Unsaturated silane-polyazide glycidyl ether co-coating technology is used to form a dense coating layer on the surface of aluminum-lithium alloy powder through chemical grafting, and precious metal catalysts are attached to improve stability and energy levels.
It significantly improves the combustion calorific value and stability of aluminum-lithium alloy powder, enhances storage performance and combustion performance, avoids structural defects and surface falloff, and improves the combustion efficiency of propellants.
Smart Images

Figure CN118955230A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder and a preparation method thereof, belonging to the technical field of energetic materials. Background Art
[0002] Metal fuel is one of the important components of modern solid propellants. Metal fuel can increase the explosion heat and detonation velocity of propellants. At the same time, the metal oxide particles generated by combustion play a role in suppressing oscillating combustion. Aluminum powder has been widely used in solid propellants due to its high density, low oxygen consumption and high combustion enthalpy, and has a significant effect on improving specific impulse.
[0003] However, the use of aluminum powder in propellants also has some disadvantages. When using traditional micron aluminum powder, due to its high ignition temperature and long ignition delay time, it is easy to agglomerate on the surface to form large aluminum droplets during the combustion process, and the combustion speed is slow and incomplete, which significantly reduces the combustion efficiency of the powder. Therefore, in order to improve the combustion performance of solid propellants, metal fuels need to be selected and adjusted according to specific needs and conditions to give full play to their advantages and avoid their disadvantages as much as possible.
[0004] Compared with other aluminum-based alloy fuels, the application of aluminum-lithium alloy powder in propellants has significant advantages. First of all, as an ideal alloy fuel, aluminum-lithium alloy powder has the characteristics of high heat release and micro-explosion during combustion, which can significantly improve the combustion efficiency of the propellant. Compared with traditional aluminum powder, aluminum-lithium alloy powder has a higher ignition success rate and a relatively low ignition temperature. However, the high reactivity of aluminum-lithium alloy powder also causes structural defects such as pores and cracks caused by its reaction with propellant components. In order to solve this problem, we can use surface coating technology to improve the stability and compatibility of aluminum-lithium alloy powder. On this basis, high-energy substances are coated to increase their energy levels. Summary of the invention
[0005] In view of this, the object of the present invention is to provide an unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder and a preparation method thereof.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows.
[0007] An unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder, wherein the surface of the aluminum-lithium alloy powder is coated with an unsaturated silane coupling agent, polyazide glycidyl ether is grafted on the unsaturated silane coupling agent to form a second coating layer, and a noble metal catalyst is also attached to the aluminum-lithium alloy powder; the atomic radius of the noble metal catalyst is
[0008] Preferably, the coating thickness of the unsaturated silane coupling agent is 30-40 nm, the coating thickness of the polyazide glycidyl ether is 15-20 nm, and the attachment amount of the noble metal catalyst is less than 3% of the mass of the aluminum-lithium alloy powder.
[0009] Preferably, the unsaturated silane coupling agent is one or more of 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane and vinyltri(2-methoxyethoxy)silane.
[0010] Preferably, the molecular weight of the polyazide glycidyl ether is 3500-4500.
[0011] Preferably, the noble metal catalyst is one or more of platinum, palladium, ruthenium and silver.
[0012] Preferably, the mass fraction of aluminum in the aluminum-lithium alloy powder is 93% to 95%, and the mass fraction of lithium is 5% to 7%.
[0013] Preferably, the particle size of the aluminum-lithium alloy powder is 5 μm to 50 μm.
[0014] A method for preparing unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to the present invention, the method steps comprising:
[0015] (1) hydrolyzing an unsaturated silane coupling agent in an alcohol solution for 20 to 30 minutes to obtain a hydrolyzed silane coupling agent solution;
[0016] (2) adding aluminum-lithium alloy powder to an organic solvent and dispersing the powder uniformly, then adding a hydrolyzed silane coupling agent solution, stirring for 30 to 50 minutes, forming a dense coating layer on the surface of the aluminum-lithium alloy powder, centrifuging, washing, and drying to obtain an unsaturated silane coupling agent-coated aluminum-lithium alloy powder;
[0017] (3) adding the aluminum-lithium alloy powder coated with an unsaturated silane coupling agent into an organic solvent and dispersing the powder evenly, adding a noble metal catalyst, heating the mixture to 65 to 85° C., dropping an organic solution of polyazide glycidyl ether, stirring the mixture at this temperature for 40 to 60 minutes, centrifuging, washing, and drying the mixture to obtain an aluminum-lithium alloy powder co-coated with unsaturated silane and polyazide glycidyl ether.
[0018] Preferably, the added amount of the unsaturated silane coupling agent is 10% to 30% of the mass of the aluminum-lithium alloy powder, the added amount of the noble metal catalyst is 0.5% to 3% of the mass of the aluminum-lithium alloy powder, and the added amount of the polyazide glycidyl ether is 8% to 15% of the mass of the aluminum-lithium alloy powder.
[0019] Preferably, the organic solvent is one or more of tetrahydrofuran, ethyl acetate and acetone.
[0020] Preferably, in step (1), the pH of the alcohol solution is 4 to 5. More preferably, the alcohol is ethanol and / or methanol. Hydrolysis in an alcohol solution with a pH of 4 to 5 can effectively promote the hydrolysis reaction and provide a reaction environment for subsequent steps.
[0021] Application of unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder as metal fuel in solid propellant.
[0022] Beneficial Effects
[0023] The present invention adopts unsaturated silane-polyazide glycidyl ether co-coating, and unsaturated silane-polyazide glycidyl ether is co-coated by chemical grafting. The coating layer is more solid, and precious metals are attached to the surface, which not only improves the stability of aluminum-lithium alloy powder but also increases the energy of aluminum-lithium alloy powder. The combustion calorific value of the co-coated aluminum-lithium alloy powder is significantly improved compared with the original powder and the aluminum-lithium alloy powder coated with a single silane coupling agent. The addition of polyazide glycidyl ether introduces high-energy groups on the surface of the alloy powder, and the high-energy groups bring about a significant increase in calorific value; at the same time, the precious metals attached to the surface can also further improve the combustion performance of the aluminum-lithium alloy powder, which is beneficial to the application of the aluminum-lithium alloy powder in propellants. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a comparison chart of scanning electron microscope photos of the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder (a) and the aluminum-lithium alloy original powder (b) described in Example 1, the aluminum-lithium alloy powder in Comparative Example 1 (c), and the aluminum-lithium alloy powder in Comparative Example 2 (d).
[0025] Figure 2 This is a comparison chart of the stability of the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether in Example 1 (right) and the initial aluminum-lithium alloy powder (left) in the liquid phase.
[0026] Figure 3 This is the infrared spectrum analysis of the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether in Example 1, the original aluminum-lithium alloy powder, and the single-coated unsaturated silane aluminum-lithium alloy powder.
[0027] Figure 4 This is a depth profile of silicon and nitrogen elements in the aluminum-lithium alloy powder in Example 1. DETAILED DESCRIPTION
[0028] The present invention will be further described in detail below in conjunction with specific embodiments.
[0029] In the following examples or comparative examples, the molecular weight of polyazide glycidyl ether is 3656.
[0030] Example 1
[0031] Take an appropriate amount of methanol and add it to a small beaker, adjust the pH to 4, add 0.5g of 3-methacryloxypropyltrimethoxysilane to the solution, and stir for 20 minutes. Add 70ml of ethyl acetate to a three-necked flask, then add 5g of aluminum-lithium alloy powder (lithium content is 6%, particle size is 30μm), mix well, add 3-methacryloxypropyltrimethoxysilane hydrolysis solution drop by drop, stir for 40 minutes, so that the unsaturated silane is fully coated on the surface of the aluminum-lithium alloy, centrifuge, wash and dry under vacuum conditions, add to a three-necked flask containing 70ml of ethyl acetate, add 0.05g of platinum catalyst, heat to 70°C, add 5g of polyazido glycidyl ether ethyl acetate solution (mass fraction of polyazido glycidyl ether is 10%), stir for 50 minutes, centrifuge, wash and dry under vacuum conditions to obtain an unsaturated silane-polyazido glycidyl ether co-coated aluminum-lithium alloy powder.
[0032] Comparative Example 1
[0033] Take an appropriate amount of methanol and add it to a small beaker, adjust the pH to 4, add 0.2g of propyltrimethoxysilane to the solution, and stir for 20 minutes. Add 30ml of ethyl acetate to a three-necked flask, then add 2g of aluminum-lithium alloy powder (lithium content is 6%, particle size is 30μm), mix well, add propyltrimethoxysilane hydrolysis solution drop by drop, stir for 30 minutes, so that the silane is fully coated on the surface of the aluminum-lithium alloy, centrifuge, wash and dry under vacuum conditions, add to a three-necked flask containing 30ml of ethyl acetate, add 0.02g of platinum catalyst, heat to 70°C, add 2g of polyazido glycidyl ether ethyl acetate solution (mass fraction of polyazido glycidyl ether is 10%), stir for 30 minutes, centrifuge, wash and dry under vacuum conditions to obtain a coated aluminum-lithium alloy powder.
[0034] Comparative Example 2
[0035] Take an appropriate amount of methanol and add it to a small beaker, adjust the pH to 4, add 0.2g of 3-methacryloxypropyltrimethoxysilane to the solution, and stir for 20 minutes. Add 30ml of ethyl acetate to a three-necked flask, then add 2g of aluminum-lithium alloy powder (lithium content is 6%, particle size is 30μm), mix well, add 3-methacryloxypropyltrimethoxysilane hydrolysis solution drop by drop, stir for 30 minutes, so that the unsaturated silane is fully coated on the surface of the aluminum-lithium alloy, centrifuge, wash and dry under vacuum conditions, add to a three-necked flask containing 30ml of ethyl acetate, heat to 70°C, add 2g of polyazido glycidyl ether ethyl acetate solution (mass fraction of polyazido glycidyl ether is 10%), stir for 30 minutes, centrifuge, wash and dry under vacuum conditions to obtain a coated aluminum-lithium alloy powder.
[0036] Comparative Example 3
[0037] Take an appropriate amount of methanol and add it to a small beaker, adjust the pH to 4, add 0.2g of 3-methacryloxypropyltrimethoxysilane to the solution, and stir for 20 minutes. Add 30ml of ethyl acetate to a three-necked flask, add 2g of aluminum-lithium alloy powder (lithium content is 6%, particle size is 30μm), mix well, add 3-methacryloxypropyltrimethoxysilane hydrolysis solution drop by drop, stir for 30 minutes, so that the unsaturated silane is fully coated on the surface of the aluminum-lithium alloy, centrifuge, wash and dry under vacuum conditions, add to a three-necked flask containing 30ml of ethyl acetate, add 0.02g of boron trifluoride triethanolamine, heat to 70°C, add 2g of polyazido glycidyl ether ethyl acetate solution (mass fraction of polyazido glycidyl ether is 10%), stir for 30 minutes, centrifuge, wash and dry under vacuum conditions to obtain a coated aluminum-lithium alloy powder.
[0038] Electron microscopic image of the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether described in Example 1 after being placed for 7 days ( Figure 1 a) and the electron microscope image of the aluminum-lithium alloy powder after 7 days of storage ( Figure 1 b) Electron microscopic image of the aluminum-lithium alloy powder in Comparative Example 1 after 7 days of storage ( Figure 1 c) Electron microscopic image of the aluminum-lithium alloy powder in Comparative Example 2 after 7 days of storage ( Figure 1 d) for comparison, such as Figure 1 As shown, after comparison, it is found that the coating layer of the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether described in Example 1 is still dense. The original aluminum-lithium alloy powder has been completely oxidized, and the coating layers of the aluminum-lithium alloy powders in Comparative Example 1 and Comparative Example 2 have fallen off to varying degrees. This shows that the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder prepared in Example 1 has better storage performance than the aluminum-lithium alloy powder coated with unsaturated silane coupling agent and the aluminum-lithium alloy powder without catalyst-coated polyazide glycidyl ether.
[0039] The unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder described in Example 1 and the initial aluminum-lithium alloy powder were placed in hot water at 70°C for comparison. Figure 2 As shown in the figure, from the picture (right) of the co-coated aluminum-lithium alloy powder in this embodiment after being placed in 70°C hot water for 3 hours, it can be seen that the alloy powder did not react with water. From the picture (left) of the initial aluminum-lithium alloy powder in water, it can be seen that it reacted violently. This shows that the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether in Example 1 has a certain stability in a liquid environment.
[0040] The aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether described in Example 1, the original aluminum-lithium alloy powder, and the aluminum-lithium alloy powder coated in Comparative Example 3 were measured for combustion heat using an oxygen-nitrogen calorimeter. As shown in Table 1, the combustion heat value of the co-coated lithium alloy powder described in Example 1 is significantly higher than that of the original powder and the aluminum-lithium alloy powder without a specific catalyst. This shows that the addition of polyazide glycidyl ether introduces high-energy groups on the surface of the alloy powder, and the high-energy groups bring about a significant increase in calorific value. The aluminum-lithium alloy powders in Example 1 and Comparative Example 3 were scanned using an energy spectrometer. As shown in Table 2, the presence of platinum elements shows that the specific metal catalyst used in Example 1 will adhere to the aluminum-lithium alloy powder during the reaction, and the attachment of the metal catalyst can increase the combustion heat. It shows that the unsaturated silane-polyazide glycidyl ether co-coating method described in the present invention not only improves the stability of the aluminum-lithium alloy powder but also increases the energy of the aluminum-lithium alloy powder.
[0041] Table 1
[0042]
[0043] Table 2
[0044]
[0045] In order to confirm that the unsaturated silane and polyazide glycidyl ether described in Example 1 are coated on the aluminum-lithium alloy powder, the powder and the original powder are subjected to FTIR test results as shown in the following figure: Figure 3 As shown in Figure 2, there is a carbon-carbon double bond (1630 cm -1 ) and carbon-oxygen double bonds (1582 cm -1 ) characteristic peak, proving that silane coupling grafted on the alloy powder surface, the carbon-carbon double bond characteristic peak on the co-coated aluminum-lithium alloy disappeared, and the azide group (2316cm -1 ) and carbon-nitrogen peaks (1142 cm -1 ), proving that polyazide glycidyl ether was successfully coated on the alloy powder coated with silane coupling agent. From the depth profile curve, it can be seen that Figure 4 As shown, the mass of the unsaturated silane used for the unsaturated silane-polyazide glycidyl ether co-coating of the aluminum-lithium alloy powder in Example 1 is 10% of the mass of the aluminum-lithium alloy powder, and the coating layer thickness is about 35nm. The mass of the polyazide glycidyl ether is 10% of the mass of the aluminum-lithium alloy powder, and the coating layer thickness is about 15nm.
[0046] Example 2
[0047] Take an appropriate amount of ethanol and add it to a small beaker, adjust the pH to 4.5, add 0.5g of 3-methacryloxypropyltriethoxysilane to the solution, and stir for 25 minutes. Add 70ml of ethyl acetate to a three-necked flask, then add 5g of aluminum-lithium alloy powder (lithium content is 6%, particle size is 30μm), mix well, add 3-methacryloxypropyltriethoxysilane hydrolysis solution drop by drop, stir for 40 minutes, so that the unsaturated silane is fully coated on the surface of the aluminum-lithium alloy, centrifuge, wash and dry under vacuum conditions, add to a three-necked flask containing 70ml of ethyl acetate, add 0.05g of platinum catalyst, heat to 75°C, add 7.5g of polyazido glycidyl ether ethyl acetate solution (mass fraction of polyazido glycidyl ether is 10%), stir for 45 minutes, centrifuge, wash and dry under vacuum conditions to obtain an unsaturated silane-polyazido glycidyl ether co-coated aluminum-lithium alloy powder.
[0048] The coating layer of the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether described in this embodiment is still dense after being placed for 7 days.
[0049] After the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder of this embodiment was placed in hot water at 70°C for 3 hours, the alloy powder did not react with water. This shows that the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder of this embodiment is also stable in a liquid environment.
[0050] The unsaturated silane and polyazide glycidyl ether described in this example are coated on the aluminum-lithium alloy powder. The characteristic peaks of the azide group and the carbon-nitrogen peaks appear in the infrared spectrum, proving that the polyazide glycidyl ether is successfully coated on the alloy powder coated with the silane coupling agent. The spectrum results also show the presence of platinum.
[0051] The combustion calorific value of the co-coated lithium alloy powder in this embodiment is significantly higher than that of the original aluminum-lithium alloy powder. The addition of polyazide glycidyl ether introduces high-energy groups on the surface of the alloy powder, which significantly increase the calorific value, and the attachment of the metal catalyst can increase the combustion heat.
[0052] Example 3
[0053] Take an appropriate amount of methanol and add it to a small beaker, adjust the pH to 5, add 0.2g of vinyl trimethoxysilane to the solution, and stir for 30 minutes. Add 30ml of acetone to a three-necked flask, then add 2g of aluminum-lithium alloy powder (lithium content is 6%, particle size is 30μm), mix well, add vinyl trimethoxysilane hydrolysis solution drop by drop, stir for 30 minutes, so that the unsaturated silane is fully coated on the surface of the aluminum-lithium alloy, centrifuge, wash, centrifuge, and dry, add it to a three-necked flask containing 30ml of tetrahydrofuran, add 0.02g of ruthenium catalyst, heat to 65°C, add 1.6g of polyazido glycidyl ether tetrahydrofuran solution (the mass fraction of polyazido glycidyl ether is 10%), stir for 40 minutes, centrifuge, wash, centrifuge, and dry to obtain an unsaturated silane-polyazido glycidyl ether co-coated aluminum-lithium alloy powder.
[0054] The coating layer of the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether described in this embodiment is still dense after being placed for 7 days.
[0055] After the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder of this embodiment was placed in hot water at 70°C for 3 hours, the alloy powder did not react with water. This shows that the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder of this embodiment is also stable in a liquid environment.
[0056] The unsaturated silane and polyazide glycidyl ether described in this example are coated on the aluminum-lithium alloy powder. The characteristic peaks of the azide group and the carbon-nitrogen peaks appear in the infrared spectrum, proving that the polyazide glycidyl ether is successfully coated on the alloy powder coated with the silane coupling agent. The spectrum results also show the presence of ruthenium.
[0057] The combustion calorific value of the co-coated lithium alloy powder in this embodiment is significantly higher than that of the original aluminum-lithium alloy powder. The addition of polyazide glycidyl ether introduces high-energy groups on the surface of the alloy powder, which significantly increase the calorific value, and the attachment of the metal catalyst can increase the combustion heat.
[0058] Example 4
[0059] Take an appropriate amount of ethanol and add it to a small beaker, adjust the pH to 4.5, add 1g of vinyl triethoxysilane to the solution, and stir for 30 minutes. Add 100ml of acetone to a three-necked flask, then add 10g of aluminum-lithium alloy powder (lithium content is 6%, particle size is 30μm), mix well, add vinyl triethoxysilane hydrolysis solution drop by drop, stir for 45 minutes, so that the unsaturated silane is fully coated on the surface of the aluminum-lithium alloy, centrifuge, wash, centrifuge, and dry, add it to a three-necked flask containing 100ml of tetrahydrofuran, add 0.01g of silver catalyst, heat to 65°C, add 15g of polyazido glycidyl ether tetrahydrofuran solution (the mass fraction of polyazido glycidyl ether is 10%), stir for 40 minutes, centrifuge, wash, centrifuge, and dry to obtain an unsaturated silane-polyazido glycidyl ether co-coated aluminum-lithium alloy powder.
[0060] The coating layer of the aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether described in this embodiment is still dense after being placed for 7 days.
[0061] After the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder of this example was placed in hot water at 70°C for 3 hours, the alloy powder did not react with water. This shows that the unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder of this example is also stable in a liquid environment.
[0062] The unsaturated silane and polyazide glycidyl ether described in this example are coated on the aluminum-lithium alloy powder. The characteristic peaks of the azide group and the carbon-nitrogen peaks appear in the infrared spectrum, proving that the polyazide glycidyl ether is successfully coated on the alloy powder coated with the silane coupling agent. The spectrum results also show the presence of silver.
[0063] The combustion calorific value of the co-coated lithium alloy powder in this embodiment is significantly higher than that of the original aluminum-lithium alloy powder. The addition of polyazide glycidyl ether introduces high-energy groups on the surface of the alloy powder, which significantly increase the calorific value, and the attachment of the metal catalyst can increase the combustion heat.
[0064] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. An unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder, characterized in that: The surface of the aluminum-lithium alloy powder is coated with an unsaturated silane coupling agent, and polyazide glycidyl ether is grafted on the unsaturated silane coupling agent to form a second coating layer. At the same time, a noble metal catalyst is attached to the aluminum-lithium alloy powder; the atomic radius of the noble metal catalyst is 2. The unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to claim 1, characterized in that: The coating thickness of the unsaturated silane coupling agent is 30-40 nm, the coating thickness of the polyazide glycidyl ether is 15-20 nm, and the attachment amount of the noble metal catalyst is less than 3% of the mass of the aluminum-lithium alloy powder.
3. The unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to claim 1, characterized in that: The unsaturated silane coupling agent is one or more of 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane and vinyltri(2-methoxyethoxy)silane.
4. The unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to claim 1, characterized in that: The molecular weight of the polyazide glycidyl ether is 3500-4500.
5. The unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to claim 1, characterized in that: The noble metal catalyst is one or more of platinum, palladium, ruthenium and silver.
6. The unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to claim 1, characterized in that: The mass fraction of aluminum in the aluminum-lithium alloy powder is 93% to 95%, and the mass fraction of lithium is 5% to 7%; the particle size of the aluminum-lithium alloy powder is 5 μm to 50 μm.
7. A method for preparing an aluminum-lithium alloy powder co-coated with unsaturated silane-polyazide glycidyl ether according to any one of claims 1 to 6, characterized in that: The method steps include: (1) hydrolyzing an unsaturated silane coupling agent in an alcohol solution for 20 to 30 minutes to obtain a hydrolyzed silane coupling agent solution; (2) adding aluminum-lithium alloy powder to an organic solvent and dispersing the powder uniformly, then adding a hydrolyzed silane coupling agent solution, stirring for 30 to 50 minutes, forming a dense coating layer on the surface of the aluminum-lithium alloy powder, centrifuging, washing, and drying to obtain an unsaturated silane coupling agent-coated aluminum-lithium alloy powder; (3) adding the aluminum-lithium alloy powder coated with an unsaturated silane coupling agent into an organic solvent and dispersing the powder evenly, adding a noble metal catalyst, heating the mixture to 65 to 85° C., dropping an organic solution of polyazide glycidyl ether, stirring the mixture at this temperature for 40 to 60 minutes, centrifuging, washing, and drying the mixture to obtain an aluminum-lithium alloy powder co-coated with unsaturated silane and polyazide glycidyl ether.
8. The method for preparing an unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to claim 7, characterized in that: The added amount of the unsaturated silane coupling agent is 10% to 30% of the mass of the aluminum-lithium alloy powder, the added amount of the noble metal catalyst is 0.5% to 3% of the mass of the aluminum-lithium alloy powder, and the added amount of the polyazide glycidyl ether is 8% to 15% of the mass of the aluminum-lithium alloy powder.
9. The method for preparing an unsaturated silane-polyazide glycidyl ether co-coated aluminum-lithium alloy powder according to claim 7, characterized in that: The organic solvent is one or more of tetrahydrofuran, ethyl acetate and acetone; the pH of the alcohol solution is 4-5; preferably, the alcohol is ethanol and / or methanol.
10. Use of the aluminum-lithium alloy powder co-coated with the unsaturated silane-polyazide glycidyl ether as claimed in any one of claims 1 to 6 as a metal fuel in a solid propellant.
Citation Information
Patent Citations
Preparation method of high-stability and high-compatibility modified aluminum lithium alloy powder
CN114539009A
Preparation method of heat-resistant liquid high-stability modified aluminum lithium alloy powder
CN114589302A
Fluoroalkyl silane-catechol co-coated aluminum-lithium alloy powder, preparation method and application of fluoroalkyl silane-catechol co-coated aluminum-lithium alloy powder
CN118271142A
Sodium carboxymethyl cellulose-glycidyl azide polymer co-coated aluminum lithium alloy powder and preparation method thereof
CN118496047A
2-ferrocenylpropyl)dimethylsilane, method for preparing the same, and method for preparing hydroxy-terminated poly butadiene containing the same
KR1020100136810A