Sulfhydrylated polymer nanogel as well as preparation method and application thereof
Through the preparation of thiolated polymer nanogels, the problem of high cost and poor stability in mercury repair in water is solved, efficient and low-cost mercury removal is achieved, and high efficiency is maintained under different pH and ionic environments.
Patent Information
- Application Number
- CN202411121113.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The prior art has problems such as high cost, complex synthesis process, large amount of toxic reagents and poor chemical stability of nanoadsorbent materials in water, which is difficult to meet the needs of rapid and high-standard repair.
Using the preparation method of thiolated polymer nanogels, the nanogels with a large amount of thiol functional groups are formed by radical polymerization of chloromethylstyrene monomers and hydrosulfide modification. The nanogels are prepared by using the microemulsion polymerization strategy to ensure that Its stability and selectivity.
It realizes efficient removal of mercury in water with low cost, simple preparation, non-toxic reagents, good stability and selectivity, and maintains high adsorption efficiency within the pH 2-12 range. The removal rate of mercury exceeds 99 after 10 recycles. %.
Smart Images

Figure CN118955775A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, relates to materials for efficiently removing mercury from water, and particularly relates to a thiol polymer nanogel and a preparation method and application thereof. Background Art
[0002] Mercury has attracted widespread global attention due to its high toxicity, high diffusion and high bioaccumulation. Anthropogenic sources of mercury include gold mining, fossil fuel combustion, metal production, cement production, waste incineration, chlor-alkali industry, etc. Countries are constantly working to reduce mercury emissions, such as adopting cleaner or alternative processes, developing new mercury capture technologies to reduce mercury emissions, and setting strict mercury emission standards. The mobility and diffusion of mercury are closely related to the movement of natural water. Since water is essential to life and makes an important contribution to the cycle of mercury in the environment, the remediation of mercury pollution in water is a key issue.
[0003] The international community has set strict limits on the concentration of mercury in water. For example, the U.S. Environmental Protection Agency stipulates that the upper limit of mercury in drinking water is 2 μg / L, and the limit concentration of mercury in industrial wastewater is 10 μg / L. Currently, the methods for remediating mercury in water include precipitation, flocculation, adsorption, ion exchange and solvent extraction. Among them, the adsorption method has the characteristics of simplicity, high efficiency, easy operation, no by-products, and regeneration, and has received widespread attention in the field of mercury remediation in water.
[0004] However, traditional adsorbents such as activated carbon, zeolite, mesoporous silica and resin lack sufficient mercurophilic functional groups, and have defects such as slow kinetics, low capacity, poor selectivity and large material consumption in the removal of mercury from water, making it difficult to meet the needs of rapid and high-standard remediation of mercury-contaminated water bodies. Researchers have attempted to improve the mercury removal efficiency by modifying the surface of traditional materials with soft base ligands such as sulfur / selenium, but due to the number of intrinsic active functional groups and pore distribution defects of traditional materials, the number of soft base functional ligands modified on the surface is relatively small, and the adsorption efficiency of traditional materials for mercury after modification is limited. In addition, the surface-modified chemical reagents will block some pores and inhibit the diffusion of mercury into the material, resulting in slow mercury removal kinetics.
[0005] In recent years, some nanomaterials such as graphene, metal organic frameworks (MOFs), porous organic polymers (POPs), covalent organic frameworks (COFs), and nano-metal sulfides have been developed for the remediation of mercury in water. Through reasonable pore size regulation and functional ligand modification, these nanomaterials show high affinity and high enrichment efficiency for mercury in water. For example, Ma et al. constructed a thiol-functionalized COFs mercury "nano-trap". Based on its high density of strong mercury chelating groups, large surface area and stable molecular skeleton, this nanomaterial shows ultra-high removal efficiency for mercury in water, with a maximum adsorption capacity of more than 1000 mg / g, and can reduce the mercury concentration in water to below 0.4 μg / L. Zhang et al. prepared a MOF-808-SH by replacing the polyacid ligands on MOF-808 with thioglycolic acid, which has ultra-fast adsorption kinetics for the removal of mercury in water, with a rate constant of k As high as 36.89 g / (mg·min), which is dozens of times faster than the existing mercury adsorbents. Although great progress has been made in the research of nano-adsorbent materials in the field of mercury remediation in water, there are still many key problems: first, the cost is high, because the precursor modules / monomers for constructing nano-materials such as POPs and COFs are expensive; second, the synthesis process is complicated, and the amount of toxic reagents used is large. For example, graphene synthesis requires a large amount of acid and oxidant, and the polymerization of COFs and POPs requires a large amount of organic solvent as a medium; third, some nano-adsorbent materials have poor chemical stability, such as MOFs in water, especially in alkaline solutions, poor stability, nano-metal sulfides dissolve in acid and are accompanied by the release of heavy metals, etc. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a thiol polymer nanogel and a preparation method thereof. The preparation method of the present invention is simple, low-cost, does not use toxic reagents, and the prepared thiol polymer nanogel has good stability and selectivity and can efficiently remove mercury in water.
[0007] The technical solution of the present invention is achieved in this way: The invention discloses a method for preparing a thiolated polymer nanogel. The method comprises the following steps: a mixed liquid obtained by dissolving a halogenated olefin monomer, a crosslinking agent and an initiator is used as an oil phase, an aqueous solution of a surfactant is used as an aqueous phase, the oil phase is added to the aqueous phase under nitrogen protection, and stirred to obtain an oil-in-water type microemulsion, and then heated to initiate free radical polymerization to obtain a halogenated polymer nanogel, and then under nitrogen protection, a sulfhydride reacts with the halogenated polymer nanogel to thiolate the halogenated polymer nanogel, thereby obtaining the thiolated polymer nanogel.
[0008] Furthermore, the method specifically includes the following steps: (1) Dissolving a halogenated olefin monomer, a crosslinking agent and an initiator in a mixed manner to obtain an oil phase, dissolving a surfactant in water to obtain an aqueous phase, then adding the oil phase to the aqueous phase, introducing nitrogen to exclude air, and stirring for 10-60 min to obtain an oil-in-water microemulsion; the molar ratio of the halogenated olefin monomer, the crosslinking agent and the initiator in the oil phase is 100:0.1:1-100:1:1: the mass concentration of the surfactant in the aqueous phase is 0.4%; and the volume ratio of the oil phase to the aqueous phase is 1:10; (2) heating the oil-in-water microemulsion to 60-80 °C, reacting for 4 h, and then centrifuging, washing and drying to obtain the halogenated polymer nanogel; (3) Under nitrogen protection, the halogenated polymer nanogel and the hydrogen sulfide are dissolved in anhydrous ethanol, and then reacted at 75°C to convert the halogenated hydrocarbons of the halogenated polymer nanogel into thiol groups. After the reaction is completed, the thiolated polymer nanogel is obtained by centrifugation, washing and drying. In specific applications, the anhydrous ethanol must ensure that the hydrogen sulfide is completely dissolved so as to have a good dispersion effect with the halogenated polymer nanogel. The amount of anhydrous ethanol used is 18 to 25 times the total mass of the hydrogen sulfide and the halogenated polymer nanogel.
[0009] Furthermore, in step (3), a phase transfer catalyst is added during the reaction of the hydrosulfide and the halogenated polymer nanogel, wherein the phase transfer catalyst is tetrabutylammonium bromide, and the amount of the phase transfer catalyst is 0.4-1 wt% of the total mass of the hydrosulfide and the halogenated polymer nanogel.
[0010] Furthermore, the halogenated olefin monomer is chloromethylstyrene.
[0011] Furthermore, the crosslinking agent is one or more of divinylbenzene, allyl methacrylate and triallyl isocyanurate, preferably divinylbenzene.
[0012] Furthermore, the initiator is one or more of azobisisobutyronitrile, benzoyl peroxide, potassium persulfate and methyl ethyl ketone peroxide, preferably azobisisobutyronitrile.
[0013] Furthermore, the surfactant is one or more of sodium dodecyl sulfate, Tween 80 and dodecyltrimethylammonium bromide, preferably sodium dodecyl sulfate.
[0014] Furthermore, the hydrosulfide is one of sodium hydrosulfide and potassium hydrosulfide; and the mass ratio of the hydrosulfide to the halogenated polymer nanogel is 2-6:1.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention adopts chloromethylstyrene as a monomer to directly initiate free radical copolymerization to prepare chlorinated polymer nanogel, so that the surface of the chlorinated polymer nanogel has a large number of active functional groups -Cl, and chloromethylstyrene has a benzene ring, so that the molecular skeleton of the chlorinated polymer nanogel has good stability, and then reacts with excess hydrogen sulfide, and the active functional group -Cl is completely converted into a thiol group, so that the thiol polymer nanogel has a large number of thiol groups and structural stability, which is conducive to the efficient removal of mercury in water.
[0016] 2. The present invention adopts a microemulsion polymerization strategy. The halogenated olefin monomers in the oil phase can be evenly and stably dispersed in the water phase under the action of the surfactant to form small oil droplets of extremely small volume, and then react. Each small oil droplet serves as a reaction site, so that the obtained nanogel has a small particle size and uniform distribution, a large specific surface area, and good dispersibility, so that the thiol functional groups are fully exposed, which is beneficial to improving the mercury adsorption efficiency.
[0017] 3. The thiol polymer nanogel prepared by the present invention has good adsorption efficiency for mercury in the pH range of 2-12 and good chemical stability. After being recycled for 10 times, the removal rate of Hg exceeds 99%. It also has good selectivity and resistance to ion interference. + Mg 2+ , Ca 2+ , Cu 2+ , Pb 2+ Various cations and Cl - 、SO4 2- 、NO3 - 、HPO4 2- When multiple anions coexist, mercury can still be removed efficiently and selectively.
[0018] 4. The raw materials used in the present invention are all commercial olefin monomers, which are low in cost, simple in preparation method, mild in reaction conditions, thorough in polymerization process, and high in monomer utilization rate, reaching 95.2%; and no toxic organic solvents are involved in the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 - Actual picture of PVB-SH in Example 1.
[0020] Figure 2 - SEM image and particle size distribution of PVB-Cl in Example 1.
[0021] Figure 3 - SEM image and particle size distribution of PVB-SH in Example 1.
[0022] Figure 4 -XPS spectra of PVB-Cl and PVB-SH in Example 1.
[0023] Figure 5 -Specific surface area and pore size distribution of PVB-Cl and PVB-SH in Example 1.
[0024] Figure 6 - Kinetic test of mercury adsorption by PVB-Cl and PVB-SH in Example 1.
[0025] Figure 7 -The removal efficiency of mercury by PVB-SH under different pH conditions in Example 1.
[0026] Figure 8 -Isotherm characteristics of mercury adsorption on PVB-SH at different temperatures in Example 1.
[0027] Fig. 9 -Effect of coexisting metal cations on mercury adsorption by PVB-SH in Example 1.
[0028] Fig.10 - Adsorption distribution coefficient of PVB-SH for different metal ions in Example 1.
[0029] Fig.11 -Effect of coexisting anions on mercury adsorption by PVB-SH in Example 1.
[0030] Fig.12 -Pictures of PVB-SH before and after long-term immersion in different corrosive solutions in Example 1 and its effect on mercury removal efficiency.
[0031] Fig.13 -XPS spectrum analysis of PVB-SH after immersion in different etching solutions in Example 1.
[0032] Fig.14 - Mercury removal efficiency of PVB-SH after different regeneration times in Example 1.
[0033] Fig.15 -SEM image and XPS spectrum of PVB-SH after 10 regenerations in Example 1. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0035] Example 1 A method for preparing thiol-modified polymer nanogel: (1) Dissolve 0.12 g of sodium dodecyl sulfate in 30 mL of deionized water and stir to dissolve to obtain an aqueous phase; mix and dissolve 0.0288 mL of crosslinker divinylbenzene (0.2 mmol), 0.04 g of initiator azobisisobutyronitrile and 2.82 mL of functional monomer chloromethylstyrene (20 mmol) to obtain an oil phase; pour the oil phase into the aqueous phase and stir rapidly at 1000 rpm for 30 min under nitrogen protection to obtain an oil-in-water microemulsion; (2) The oil-in-water microemulsion was heated to 75°C and reacted for 4 h. After cooling to room temperature, the solid was collected by centrifugation, washed with deionized water, and dried to obtain 2.84 g of chlorinated polymer nanogel PVB-Cl with a yield of 95.17%.
[0036] (3) Then, 0.5 g of PVB-Cl, 1.5 g of NaHS and 0.3 g of tetrabutylammonium bromide (phase transfer catalyst) were weighed and dissolved in 50 mL of anhydrous ethanol. Nitrogen was introduced to remove air, and then the mixture was stirred at 75 °C for 24 h. After the reaction, the solid was collected by centrifugation, washed with deionized water and dried to obtain 0.12 g of light yellow thiol-modified polymer nanogel PVB-SH (such as Figure 1 as shown).
[0037] Example 2 This embodiment is the same as embodiment 1, except that the amount of the cross-linking agent divinylbenzene in this embodiment is 0.00288 g.
[0038] Example 3 This example is the same as Example 1, except that the amount of sodium hydrosulfide in this example is 3 g.
[0039] Example 4 This example is the same as Example 1, except that the amount of sodium hydrosulfide in this example is 2 g.
[0040] Example 5 This example is the same as Example 1, except that the amount of sodium hydrosulfide in this example is 1 g.
[0041] Example 6 This embodiment is the same as embodiment 1, except that the amount of the cross-linking agent divinylbenzene in this embodiment is 0.0144 g.
[0042] Comparative Example 1 This embodiment is the same as embodiment 1, except that 2-ethyl chloromethylacrylate is used instead of chloromethylstyrene in this embodiment.
[0043] Comparative Example 2 This example is the same as Example 1, except that the amount of the cross-linking agent divinylbenzene in this example is 0.144 g.
[0044] Comparative Example 3 This example is the same as Example 1, except that the amount of the cross-linking agent divinylbenzene in this example is 0.288 g.
[0045] Comparative Example 4 This example is the same as Example 1, except that the amount of sodium hydrosulfide in this example is 0.5 g.
[0046] 1. The SEM images and particle size distribution diagrams of PVB-Cl and PVB-SH in Example 1 are as follows: Figure 1 and Figure 2 As shown in the figure, the SEM image shows that the chlorinated polymer nanogel PVB-Cl has uniformly distributed nanoparticles. The particle size of the chlorinated polymer nanogel PVB-Cl was counted using Nano Measure software, and the average particle size of PVB-Cl was 40.69 nm. The microscopic morphology of the PVB-SH nanogel obtained by NaHS treatment did not change significantly, and the average particle size was slightly larger than that of PVB-Cl, about 41.94 nm. The chemical composition of PVB-Cl and PVB-SH nanogels was analyzed by X-ray photoelectron spectroscopy (XPS). The results showed that PVB-Cl was mainly composed of three elements: C, O and Cl. After NaSH treatment, the characteristic peak of Cl 2p at 200.3 eV disappeared, and a new characteristic peak of S 2p appeared at 163.7 eV, corresponding to the -SH composition; the XPS C1s fine structure spectrum also showed that after NaHS treatment, the C-Cl peak in PVB-Cl disappeared, and a new C-SH characteristic peak appeared ( Figure 4 ), these results all prove that NaHS treatment successfully converts Cl in PVB-Cl into -SH. The specific surface area analysis results show that both PVB-Cl and PVB-SH have large specific surface areas, among which PVB-Cl has a specific surface area of 81.52 m 2 / g, porosity is about 0.7411 cm 3 / g, and the average pore size is 36.78 nm. After being treated with NaHS, the specific surface area of PVB-SH is slightly reduced to 73.22 m 2 / g, the porosity is reduced to 0.2729cm 3 / g, the average pore size is reduced to 15.92nm ( Figure 5 ), the main reason is that the Cl atom is replaced by the larger -SH, but PVB-SH still has a large specific surface area, which is conducive to the full exposure of the -SH functional group and improves the removal efficiency of mercury in water.
[0047] 2. Mercury adsorption test of PVB-Cl and PVB-SH in Example 1 (1) Differences in the adsorption efficiency of mercury between PVB-Cl and PVB-SH The amount of adsorbent added was 0.2 g / L, the mercury concentration was 10 mg / L, the test temperature was 25°C, and the solution pH was adjusted to 5. The adsorption test showed that PVB-Cl hardly adsorbed mercury. After 360 minutes of adsorption, the removal rate of mercury in water by PVB-Cl was only 0.5%. PVB-Cl can quickly and efficiently remove mercury from water. Within 0.5 minutes of adsorption, the mercury concentration in the solution quickly decreased from 10.03 mg / L to 1.21 mg / L, and the removal rate was 87.94%; after 10 minutes, the mercury concentration decreased to 0.19 mg / L, and the removal rate reached 98.10%; after 240 minutes of adsorption, the residual mercury concentration in the solution decreased to below 0.002 mg / L, which is lower than the limit value of mercury content in drinking water specified by the US Environmental Protection Agency ( Figure 6 ).
[0048] (2) Effect of pH on mercury adsorption by PVB-SH The amount of adsorbent added was 0.2 g / L, the mercury concentration was 10 mg / L, the test temperature was 25°C, and the adsorption time was 24 h. Changes in the pH value in the solution can change the surface charge of the adsorbent and the adsorbate, thereby affecting the adsorption. Adsorption tests under different pH conditions are as follows: Figure 7 As shown in the figure, PVB-SH has a very high adsorption efficiency for mercury in the pH range of 2-11, the mercury residual concentration is less than 1 μg / L, and the removal rate exceeds 99.99%. When the pH is 12, the removal efficiency of mercury decreases to 89.96%.
[0049] (3) Mercury removal efficiency of PVB-SH at different temperatures The adsorbent addition amount was 0.2 g / L, the mercury concentration was 5-300 mg / L, the adsorption time was 24 h, the solution pH was 5, and the test temperatures were 25°C, 35°C and 45°C. The test results are as follows Figure 8 As shown in Figure 2, at 25 °C, the adsorption efficiency of PVB-SH nanogel on mercury gradually increased with the increase of mercury concentration. c e In the range from 0 to 50 mg / L, the adsorption of mercury by PVB-SH increased rapidly from 0 to 258.45 mg / g. c eWith further increase, the mercury adsorption slowly increased until it reached equilibrium, and the maximum adsorption was 342.02 mg / g. Temperature increase promoted mercury adsorption. When the temperature increased from 25°C to 45°C, the maximum adsorption of mercury by PVB-SH increased to 380.55 mg / g, indicating that the adsorption of mercury by PVB-SH was an endothermic reaction. The disorder of the solid-liquid system was thermodynamically favorable, and the adsorption could be promoted by increasing the temperature.
[0050] (4) Effect of coexisting ions For the interference test of coexisting metal ions, the amount of adsorbent added was 0.2 g / L, the concentration of each heavy metal was 10 mg / L, the adsorption time was 24 h, the solution pH was 5, and the test temperature was 25 °C. Fig. 9 As shown, in Na + , Ca 2+ Mg 2+ , Pb 2+ , Cu 2+ 、Cd 2+ 、Ni 3+ 、Zn 2+ and Mn 2+ When 9 common metal ions coexist, PVB-SH can still effectively remove mercury from water, with a removal rate of 99.98%. PVB-SH exhibits extremely high selectivity for the adsorption of mercury, with a distribution coefficient of K d Up to 3.07×10 7 , which is 3 orders of magnitude higher than other metal ions ( Fig.10 ).
[0051] In the coexistence anion interference test, the amount of adsorbent added was 0.2 g / L, the concentration of each anion was 10-1000 mg / L, the adsorption time was 24 h, the solution pH was 5, and the test temperature was 25°C. Fig.11 As shown in the figure, under low anion coexistence conditions (10 mg / L), PVB-SH has little effect on the removal of mercury, and the removal rate is greater than 99.9%. When high anions coexist (1000 mg / L), the removal efficiency of PVB-SH for mercury is reduced, but still higher than 96%. The coexistence ion interference test structure shows that PVB-SH has good resistance to metal cation and common anion interference in the removal of mercury.
[0052] (5) Stability analysis 50 mg of PVB-SH was immersed in 10 mL of tap water, 1 mmol / L NaOH, 10 mmol / L NaOH, 0.1 mol / L NaCl, 1 mol / L NaCl, 0.1mol / L HCl and 1 mol / L HCl for 45 days, and then the removal efficiency of mercury was tested. The results showed that PVB-SH still maintained a high removal efficiency for mercury after long-term exposure to tap water and corrosive solutions such as acids, alkalis and salts, with a removal rate of over 99.9% ( Fig.12 ). XPS chemical composition analysis showed that the elemental composition and thiol functional groups of PVB-SH did not change significantly after long-term exposure to tap water and corrosive fluid, indicating that PVB-SH has strong stability ( Fig.13 ).
[0053] (6) Renewability The good chemical stability of PVB-SH gives it excellent regeneration. After adsorbing mercury, PVB-SH can be efficiently regenerated in an acidic solution of thiourea, such as Fig.14 As shown in the figure, after 10 regenerations, the removal efficiency of PVB-SH for mercury was almost not significantly reduced, and the removal rate reached 99.58%. After 10 regenerations, the microstructure and chemical composition of PVB-SH were significantly changed ( Fig.15 ), demonstrating its good reproducibility and structural stability.
[0054] 3. The thiol polymer nanogel PVB-SH prepared in Examples 1 to 5 and Comparative Examples 1 to 5 was used as an adsorbent to adsorb mercury. The amount of adsorbent added was 0.2 g / L, the mercury concentration was 5-300 mg / L, the adsorption time was 24 h, the solution pH was 5, and under the conditions of 25°C, when the adsorption equilibrium was reached, the maximum adsorption amount of mercury by the thiol polymer nanogel PVB-SH prepared in each example was as follows: It can be seen from the above table that (1) excess sodium hydrosulfide is beneficial to increasing the adsorption capacity of mercury by the adsorbent, and at the same time, the adsorption capacity of mercury by the adsorbent increases with the increase of the mass of sodium hydrosulfide. Figure 4 It can be seen that when the chlorinated hydrocarbons in Example 1 are completely converted into thiol groups, when the mass ratio of sodium hydrosulfide to PVB-Cl is greater than 3:1, the mercury adsorption amount is slightly increased because sodium hydrosulfide has a certain degradation effect on the thiolated polymer nanogel PVB-SH, which can increase its specific surface area and porosity. It has been found that when the mass ratio of sodium hydrosulfide to PVB-Cl exceeds 6:1, the solubility of sodium hydrosulfide reaches a supersaturated state, and the adsorption amount of mercury by the obtained thiolated polymer nanogel PVB-SH no longer increases significantly.
[0055] (2) Excessive cross-linking agent will affect the adsorption effect of the adsorbent on mercury. This is because excessive cross-linking agent will hinder the diffusion of mercury into the adsorbent, thereby affecting the amount of mercury adsorbed.
[0056] Finally, it should be noted that the above embodiments of the present invention are only examples for illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a thiol-modified polymer nanogel, characterized in that: The mixed liquid obtained by dissolving a halogenated olefin monomer, a crosslinking agent and an initiator is an oil phase, and the aqueous solution of a surfactant is an aqueous phase. Under the protection of nitrogen, the oil phase is added to the aqueous phase and stirred to obtain an oil-in-water type microemulsion, and then heated to initiate free radical polymerization to obtain a halogenated polymer nanogel. Under the protection of nitrogen, a sulfhydride reacts with the halogenated polymer nanogel to thiolate the halogenated polymer nanogel, thereby obtaining a thiolated polymer nanogel.
2. The method for preparing a thiol-modified polymer nanogel according to claim 1, characterized in that: The specific steps include: (1) Dissolving a halogenated olefin monomer, a crosslinking agent and an initiator in a mixed manner to obtain an oil phase, dissolving a surfactant in water to obtain an aqueous phase, then adding the oil phase to the aqueous phase, introducing nitrogen to exclude air, and stirring for 10-60 min to obtain an oil-in-water microemulsion; the molar ratio of the halogenated olefin monomer, the crosslinking agent and the initiator in the oil phase is 100:0.1:1-100:1:1: the mass concentration of the surfactant in the aqueous phase is 0.4%; and the volume ratio of the oil phase to the aqueous phase is 1:10; (2) heating the oil-in-water microemulsion to 60-80 °C, reacting for 4 h, and then centrifuging, washing and drying to obtain the halogenated polymer nanogel; (3) Under nitrogen protection, the halogenated polymer nanogel and the hydrogen sulfide are dissolved in anhydrous ethanol, and then reacted at 75°C to convert the halogenated hydrocarbons of the halogenated polymer nanogel into thiol groups. After the reaction is completed, the thiol-containing polymer nanogel is obtained by centrifugation, washing and drying.
3. The method for preparing a thiol-modified polymer nanogel according to claim 2, characterized in that: In step (3), a phase transfer catalyst is added during the reaction of the hydrosulfide and the halogenated polymer nanogel. The phase transfer catalyst is tetrabutylammonium bromide. The amount of the phase transfer catalyst is 0.4-1 wt% of the total mass of the hydrosulfide and the halogenated polymer nanogel.
4. A method for preparing a thiol-modified polymer nanogel according to claim 1, 2 or 3, characterized in that: The halogenated olefin monomer is chloromethylstyrene.
5. The method for preparing a thiol-modified polymer nanogel according to claim 1, 2 or 3, characterized in that: The crosslinking agent is one or more of divinylbenzene, allyl methacrylate and triallyl isocyanurate, preferably divinylbenzene.
6. A method for preparing a thiol-modified polymer nanogel according to claim 1, 2 or 3, characterized in that: The initiator is one or more of azobisisobutyronitrile, benzoyl peroxide, potassium persulfate and methyl ethyl ketone peroxide, preferably azobisisobutyronitrile.
7. A method for preparing a thiol-modified polymer nanogel according to claim 1, 2 or 3, characterized in that: The surfactant is one or more of sodium dodecyl sulfate, Tween 80 and dodecyltrimethylammonium bromide, preferably sodium dodecyl sulfate.
8. The method for preparing a thiol-modified polymer nanogel according to claim 1, 2 or 3, characterized in that: The hydrosulfide is one of sodium hydrosulfide and potassium hydrosulfide; the mass ratio of the hydrosulfide to the halogenated polymer nanogel is 2-6:
1.
9. A thiol-polymer nanogel, characterized in that: The nanogel is prepared by the method for preparing a thiol-polymer nanogel according to any one of claims 1 to 8.
10. Use of the thiol polymer nanogel according to claim 9 in removing mercury from water.
Citation Information
Patent Citations
Preparation method of composite separating film filled by interpenetrating polymer network hydrogel
CN105289316A
PROCESS FOR THE PRODUCTION OF SULPHUR-CONTAINING ADSORBENTS
DD139430A1
Mercapto group-containing polymer
JP1998077311A
Vinyl chloride-based copolymer porous body and method for producing same
US20150057380A1
Dispersant system for making polyvinyl chloride which produces low color chlorinated polyvinyl chloride
US5006607A