Polyurethane polyurea foaming material as well as preparation method and application thereof

Through specific formulas and process steps, polyurethane polyurea foaming material is prepared, which solves the problems of high production costs and easy delamination, cracking and powdering of polyurethane polyurea materials, and achieves the effects of low cost, excellent performance and wide application.

CN118955850APending Publication Date: 2024-11-15JIANGSU CHANGSHUN POLYMER MATERIAL INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411148750.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing polyurethane polyurea materials are costly and are prone to stratification, cracking and powdering, and the process is complex and costly, which limits its application scope.

Method used

Component A including amino polyether polyol, terminal hydroxy polyether polyol, chain extender, silicone oil, catalyst, chemical foaming agent, physical foaming agent and filler are combined with modified isocyanate and linear polyether polyol Component B of the polyurethane polyurea foam material is prepared through specific ratios and process steps to ensure that the material does not delaminate, crack or powder during the production process, and improve its physical properties.

Benefits of technology

It has realized low cost and excellent performance polyurea foaming material, suitable for hard and soft foams, meets the requirements of spraying equipment, has a wide range of formulation design freedom and significant physical performance improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005002985060000041
    Figure BDA0005002985060000041
  • Figure BDA0005002985060000051
    Figure BDA0005002985060000051
  • Figure BDA0005002985060000061
    Figure BDA0005002985060000061
Patent Text Reader

Abstract

The invention relates to a polyurethane polyurea foaming material as well as a preparation method and application thereof, and mainly solves the problems of high production cost and layering, cracking and pulverization in the production process of a polyurethane polyurea material in the prior art. According to the technical scheme, the novel polyurethane polyurea foaming material comprises a component A and a component B, the weight ratio of the component A to the component B is 1: (0.3-3), and the component A comprises the following components in parts by weight: 0-50 parts of amino polyether polyol, 0-80 parts of hydroxyl-terminated polyether polyol, 0-30 parts of a chain extender, 1-3 parts of silicone oil, 0.1-2 parts of a catalyst, 0.2-2 parts of a chemical foaming agent, 5-25 parts of a physical foaming agent and 0-50 parts of filler; wherein the hydroxyl-terminated polyether polyol and the chain extender cannot be zero at the same time; according to the technical scheme, the problems are well solved, and the polyurethane foam can be applied to the industrial application of hard and soft polyurea foam.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyurea foaming materials, in particular to a polyurethane polyurea foaming material and a preparation method and application thereof. Background Art

[0002] Polyurea is a material generated by the reaction of all or part of an amino compound component (component A) with an isocyanate-terminated compound (component B). Since the polyurea material has a higher urea content, the material molecules have stronger hydrogen bonding than traditional polyurethanes, and the hard segment strength of the polyurethane material is greater, thus showing a series of excellent physical and mechanical properties. However, the usual amino polyethers are expensive and have fewer types and specifications, thus limiting the development and application of polyurea foam products. The polyurea material developed by the present invention improves the corresponding strength and physical properties while introducing common hydroxyl polyethers, so that the prepared polyurea foam and formula have strong practicality, and ultimately improve the performance and strength. However, the introduction of hydroxyl groups will form a large reactivity difference when reacting with amino groups and isocyanates in the system, which easily leads to stratification, cracking and powdering of the foam. The polyurea foam material prepared by the present invention prevents stratification, cracking and powdering of the polyurea foam material while improving the strength.

[0003] Chinese patent CN112831024A discloses a safe polyimide-polyurea thermal insulation foam and preparation method, and describes the polyimide-polyurea foam prepared based on polyurethane free foaming technology using aromatic polycarboxylic acid ester solution and excess isocyanate as the main raw materials. For example, phthalic acid and isocyanate can undergo condensation reaction to generate corresponding urea compounds. The reaction mechanism is as follows: First, the -N=C=O group in the isocyanate will electrophilically attack the carboxyl group (-COOH) on the benzene ring to form a protected imine intermediate. Subsequently, a nucleophilic addition reaction occurs inside the imine molecule to produce a new CN bond, and an alcohol molecule (ROH) is separated at the same time, and finally, a urea compound (CO-NH-COR) is obtained. However, the general carboxylic acid system will reduce the reactivity of the system, and the patent uses dimethyl phthalate, and the production and use links have certain limitations in terms of safety and environmental protection.

[0004] Chinese patent CN105418881A discloses a polyurea foam material and a preparation method thereof. The polyurea foam material is made of expandable microspheres, isocyanate and diamine. Method: The foamable expandable microspheres are mixed with diamine, and the mixture is mixed under vacuum conditions to obtain a mixture; then isocyanate is added to the mixture, and after mixing under vacuum conditions, the mixture is injected into a mold to form a polyurea foam material. The foam is prepared by the expansion of expandable microspheres under the condition of a temperature of 80°C to 210°C. This method can achieve a good reduction in density and maintain strength of the foamed polyurea layer. However, the process is essentially to first synthesize a traditional plastic polyurea elastomer and then foam it at high temperature. The process is relatively complicated, the process cost is high, and it is suitable for systems with a certain degree of extensibility in the structure.

[0005] Chinese patent CN114920975A discloses a polyurea foam material and a preparation method thereof, a polyurea foam material and a preparation method thereof, the polyurea foam is prepared from component A and component B, in terms of weight, component A includes 100 parts of polyamino compound, 0.5-25 parts of foaming agent, 0.05-0.2 parts of catalyst, 1-2 parts of foam stabilizer, component B includes: 20-45 parts of isocyanate compound, the foaming agent is one of physical foaming agent or chemical foaming agent or a mixture of the two, when only physical foaming agent is added, the added weight is 1-15 parts, when only chemical foaming agent is added, the added weight is 0.5-10 parts. The preparation method of the present invention can prepare polyurea foam with a density as low as 0.03g / cm3. In its patent, amino-terminated polyether is used, and physical and chemical foaming agents are added. The limitation of this patent is that the amino polyether used is relatively expensive and the specifications are not widely available, and most of them are linear difunctional structures. Secondly, the system lacks a chain extender as a hard end, and can only rely on the reaction of isocyanate and water, and this reaction rate is much lower than the reaction rate of isocyanate and amino polyether. These have greatly limited the performance and application range of its products, making its performance low, and the product is limited to relatively soft products. Furthermore, the ratio of 100 parts of component A and 20-45 parts of component B in the public information also limits the application and process requirements such as spray foam that require a volume ratio of 1:1.

[0006] Combined with some of the previous literature, since the reactivity of amino resins and amino chain extenders with isocyanic acid is extremely fast, far exceeding the reaction speed of isocyanic acid and water, therefore, adding traditional water to the system does not play the role of the reactive foaming of common polyurethane foams. This is also the reason why the spray-type full polyurea elastomer itself can be sprayed and cured on the water surface. Under this restriction, previous work used carboxyl substances as reactive foaming agents to react with isocyanates to produce carbon dioxide foaming, or to achieve it using physical foaming agents. Although water is used in CN114920975A, it essentially wants to use isocyanates and amino polyethers to react first to form a terminal isocyanate structure, and then react with excess water to foam. This method has poor foaming performance and is difficult to control the process. Low density is achieved by expanding microspheres or even by some hollow fillers, which is out of the traditional polyurethane foam process and the corresponding process cost is relatively high. Summary of the invention

[0007] One of the technical problems to be solved by the present invention is that the existing technology has the problem that the production cost of polyurethane polyurea materials is high and delamination, cracking and powdering may occur during the production process. A new polyurethane polyurea foaming material is provided, which has the advantages of low cost and no delamination, cracking and powdering after the introduction of traditional hydroxy polyether polyols and hydroxy chain extenders during the production process.

[0008] The second technical problem to be solved by the present invention is to provide a method for preparing a polyurethane polyurea foam material corresponding to the first technical problem to be solved.

[0009] The third technical problem to be solved by the present invention is to provide an application of a polyurethane polyurea foam material corresponding to the first technical problem to be solved.

[0010] In order to solve one of the above technical problems, the technical solution adopted by the present invention is as follows: a polyurethane polyurea foaming material, characterized in that it comprises component A and component B, the weight ratio of component A to component B is 1:0.3-3 in parts by weight, the component A comprises the following components: 0-50 parts of amino polyether polyol, 0-80 parts of terminal hydroxyl polyether polyol, 0-30 parts of chain extender, 1-3 parts of silicone oil, 0.1-2 parts of catalyst, 0.2-2 parts of chemical foaming agent, 5-25 parts of physical foaming agent, 0-50 parts of filler, wherein the terminal hydroxyl polyether polyol and the chain extender cannot be zero at the same time; the component B is a modified isocyanate, and the component B comprises the following components: 40-60 parts of isocyanate and 30-65 parts of linear polyether polyol.

[0011] In the above technical scheme, the functionality of the amino polyether polyol is 2, and the molecular weight ranges from 300 to 3000; the terminal hydroxyl polyether polyol is a soft foam polyether with EO partial end capping and a functionality of 2 to 3 and a hydroxyl value of 24 to 100 mgKOH / g.

[0012] In the above technical scheme, the amino polyether polyol is selected from Jeffamine D-2000, Jeffamine D-1000, Jeffamine D-5000, and Jeffamine D-400; the hydroxyl-terminated soft foam polyether polyol is selected from at least one of CHED-28, CHE-330N, NJ-405, and NJ-4110.

[0013] In the above technical scheme, the chain extender is selected from at least one of Ethacure 100, Ethacure 300, glycerol or diethylene glycol; the silicone oil is selected from at least one of DC193 or Ak 8804; the catalyst is selected from at least one of BICAT8118, DABCO T-120 or JEFFCAT ZR-70; the chemical foaming agent is selected from at least one of water or formic acid, the physical foaming agent is selected from at least one of 141B, 245fa, HFO or methyl acetate, and the filler is selected from at least one of color paste or flame retardant.

[0014] In the above technical solution, the isocyanate is selected from at least one of polymeric MDI, MDI-50 or M20S, and the linear polyether polyol is selected from a difunctional polyether polyol with a molecular weight of 500 to 5000.

[0015] To solve the second technical problem above, the technical solution adopted by the present invention is as follows: A method for preparing the above polyurethane polyurea foam material comprises the following steps:

[0016] (1) preparing component A: at room temperature, add 0-50 parts of amino polyether polyol, 0-80 parts of terminal hydroxyl polyether polyol, 0-30 parts of chain extender, 1-3 parts of silicone oil, 0.1-2 parts of catalyst, 0.2-2 parts of chemical foaming agent, 5-25 parts of physical foaming agent, and 0-50 parts of filler in container A by weight, wherein the terminal hydroxyl polyether polyol and the chain extender cannot be zero at the same time, and stir evenly to obtain component A;

[0017] (2) preparing component B: adding 40 to 60 parts of isocyanate and 30 to 65 parts of linear polyether polyol by weight into container B at a temperature of 60 to 80° C., stirring and reacting to obtain component B;

[0018] (3) Component A and component B are mixed uniformly in a weight ratio of 1:0.3 to 3 to obtain a polyurethane polyurea foam material.

[0019] To solve the third technical problem, the present invention adopts the following technical solution: a polyurethane polyurea foam material in hard and soft polyurea foam industrial applications

[0020] The present invention provides a polyurethane polyurea foaming material. When hydroxyl and water are introduced into the formula, when hydroxyl polyether and water and amino polyether each account for a considerable proportion, due to the large difference in the reactivity of each isocyanate, the foam will be delaminated, cracked and powdered. To solve this phenomenon, partially EO-terminated and multifunctional polyethers, EDA / TDA-initiated polyethers, and sucrose-initiated multifunctional polyols are used to narrow the reactivity gap with amino groups and water, and a strong gel catalyst is used to enhance the gel reaction during the foaming process, thereby obtaining the required polyurea foam. The system of the present invention can realize polyurea foams including hard and soft ones in a large range, and better meet the A / B component weight ratio of 1:0.3 to 3 required by spraying equipment, and has a very wide degree of freedom in formula design. Since the product contains a certain amount of urea groups, the polyurea foam prepared thereby can achieve the advantages of stronger physical properties and application characteristics compared with ordinary polyurethane foams. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 DMA curves of polyurea soft foam and common soft foam;

[0022] Figure 2 DMA curves of polyurea rigid foam and common rigid foam;

[0023] in, Figure 1 The dotted line in the figure is the data result of polyurea soft foam of Example 1, and the solid line is the data result of common soft foam of Comparative Example 3; Figure 2 The dotted line in the figure is the data result of the polyurea rigid foam of Example 4, and the solid line is the data result of the ordinary rigid foam of Comparative Example 4. DETAILED DESCRIPTION

[0024] The present invention is further described below by way of examples, but is not limited to these examples.

[0025] Table 1 List of raw materials

[0026]

[0027]

[0028] B component 1#

[0029] Take a dry and clean three-necked reaction flask, add 46 parts of MDI-50 and 54 parts of CHE-220, stir evenly and pass nitrogen protection, heat to 75°C in an oil bath, react for 2 hours, and after the NCO value reaches the predetermined target range after detection and confirmation, cool and seal for storage to obtain component B 1.

[0030] B Component 2#

[0031] Take a dry and clean three-necked reaction flask, add 55 parts of M20S, 20.7 parts of MDI-50, and 24.3 parts of CHE-220 in sequence, stir evenly and pass nitrogen protection, heat to 75°C in an oil bath, react for 2 hours, and after the NCO value reaches the predetermined target range after detection and confirmation, cool and seal for storage to obtain B component 2#.

[0032] Example 1

[0033] Prepare component A: 68.80 parts of CHE-330N, 10 parts of Ethacure 100, 2.5 parts of glycerol, 2 parts of DC193, 0.2 parts of Dabco T-120, and 0.5 parts of Jeffcat ZR-70 are stirred for about 5 minutes to make them uniform, then 15 parts of HFC-245fa which has been pre-refrigerated (2-5°C) are added and stirred for about 1 minute, and then poured into a sealed bottle and stored at room temperature;

[0034] Preparation of component B: Take a dry and clean three-necked reaction flask, add 46 parts of MDI-50 and 54 parts of CHE-220, stir evenly and pass nitrogen protection, heat to 75°C in an oil bath, react for 2 hours, and after the NCO value reaches the predetermined target range after detection and confirmation, cool and seal for storage to obtain component B 1#;

[0035] Pour the measured components A and B into a cup at room temperature, use a laboratory stirrer to quickly stir for 5 seconds at 2000 rpm to mix the components evenly, and pour into a preheated mold (30-40°C). Demould after 30 minutes to obtain the desired sample; the performance test results of the prepared polyurethane polyurea foam material product are shown in Table 4.

[0036] Examples 2 to 7 and Comparative Examples 1 to 5

[0037] Examples 2 to 7 and Comparative Examples 1 to 5 follow the steps of Example 1, except that the reaction raw materials and raw material ratios are different, as shown in Table 2 and Table 3; the performance test results of the obtained polyurethane polyurea foam material products are shown in Table 4 and Table 5.

[0038] Table 2 Raw material components of polyurea soft foaming materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0039] raw material Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 CHE-220 / / / / / / CHED-28 / / / / 30.00 / CHE-330N 68.80 66.30 58.80 68.35 44.00 73.3 JeffamineD-2000 / 10.00 10.00 / / / Ethacure100 10.00 10.00 10.00 15.00 18.00 glycerin 2.50 / 2.50 / / 2.00 Diethylene glycol / / / / / 6.00 DC193 2.00 2.00 2.00 / / 2.00 AK8804 / / / 1.50 1.50 BICAT8118 / / / 0.15 / / DabcoT-120 0.20 0.2 0.2 / 0.60 0.20 Jeffcat ZR-70 0.50 0.5 0.5 / 0.40 0.50 HFC-245fa 15.00 10.00 15.00 15.00 5.00 15.00 water 1.00 1.0 1.0 0 0.50 1.00 Amount of component A 100 100 100 100 100 100 B component 1# 108.00 82.50 108.00 63.50 89.00 108.00

[0040] Table 3 Raw material components of polyurea rigid foaming materials obtained in Examples 4 to 7 and Comparative Examples 4 to 5

[0041] raw material Example 4 Example 5 Example 6 Example 7 Comparative Example 4 Comparative Example 5 CHE-220 19.00 15.00 NJ-405 15.00 15.00 15.00 15.00 15.00 15.00 NJ-4110 41.90 51.90 56.90 36.50 41.90 51.50 JeffamineD-2000 15.00 / / 15.00 / / Ethacure100 10.00 15.00 10.00 10.00 / / Diethylene glycol / / / / 6.00 / DC193 2.00 2.00 2.00 2.00 2.00 2.00 DabcoT-120 0.20 0.20 0.20 0.20 0.20 0.20 Jeffcat ZR-70 0.50 0.50 0.50 0.50 0.50 0.50 HFC-245fa 15.00 15.00 15.00 20.00 15.00 15.00 water 0.40 0.40 0.40 0.80 0.40 1.00 B Component 2# 108.00 128.00 125.00 108.00 108.00 108.00

[0042] Table 4 Performance indicators of Examples 1 to 3 and Comparative Examples 1 to 3

[0043]

[0044]

[0045] Table 5 Performance indicators of Examples 4 to 7 and Comparative Examples 4 to 5

[0046]

[0047] Since it is difficult to achieve consistency in the density of the sample, the test results have a large deviation. Therefore, a typical foam with a similar formula is taken for DMA testing to obtain the modulus and temperature curve of the material. The results are as follows:

[0048] Depend on Figure 1 and Figure 2 As shown in the DMA curve, the present invention introduces a polyurea segment with strong polarity into the hard segment of the polyurea foam material, so the obtained polyurea soft foam and polyurea hard foam have significant advantages in modulus within the working temperature range compared with ordinary polyurethane soft foam and hard foam with similar formula. At the same time, the formula adjustment is wide, covering soft foam and hard foam, reflecting practicality.

Claims

1. A polyurethane polyurea foam material, characterized in that: The invention comprises component A and component B, wherein the weight ratio of component A to component B is 1:0.3-3 in parts by weight, wherein component A comprises the following components: 0-50 parts of amino polyether polyol, 0-80 parts of terminal hydroxyl polyether polyol, 0-30 parts of chain extender, 1-3 parts of silicone oil, 0.1-2 parts of catalyst, 0.2-2 parts of chemical foaming agent, 5-25 parts of physical foaming agent, and 0-50 parts of filler, wherein the terminal hydroxyl polyether polyol and the chain extender cannot be zero at the same time; and component B is a modified isocyanate, wherein component B comprises the following components: 40-60 parts of isocyanate and 30-65 parts of linear polyether polyol.

2. The polyurethane polyurea foam material according to claim 1, characterized in that: The functionality of the amino polyether polyol is 2, and the molecular weight ranges from 300 to 3000; the terminal hydroxyl polyether polyol is a soft foam polyether with EO partly terminated and the functionality is 2 to 3, and the hydroxyl value is 24 to 100 mgKOH / g.

3. The polyurethane polyurea foam material according to claim 1, characterized in that: The amino polyether polyol is selected from Jeffamine D-2000, Jeffamine D-1000, Jeffamine D-5000, and Jeffamine D-400; the hydroxyl-terminated polyether polyol is selected from at least one of CHED-28, CHE-330N, NJ-405, and NJ-4110.

4. The polyurethane polyurea foam material according to claim 1, characterized in that: The chain extender is selected from at least one of Ethacure 100, Ethacure 300, glycerol or diethylene glycol; the silicone oil is selected from at least one of DC193 or Ak8804; the catalyst is selected from at least one of BICAT 8118, DABCO T-120 or JEFFCAT ZR-70; the chemical foaming agent is selected from at least one of water or formic acid, the physical foaming agent is selected from at least one of 141B, 245fa, HFO or methyl acetate, and the filler is selected from at least one of color paste or flame retardant.

5. The polyurethane polyurea foam material according to claim 1, characterized in that: The isocyanate is selected from at least one of polymeric MDI, MDI-50 or M20S, and the linear polyether polyol is selected from bifunctional polyether polyol with a molecular weight of 500 to 5000.

6. A method for preparing the polyurethane polyurea foam material according to any one of claims 1 to 6, comprising the following steps: (1) preparing component A: at room temperature, add 0-50 parts of amino polyether polyol, 0-80 parts of terminal hydroxyl polyether polyol, 0-30 parts of chain extender, 1-3 parts of silicone oil, 0.1-2 parts of catalyst, 0.2-2 parts of chemical foaming agent, 5-25 parts of physical foaming agent, and 0-50 parts of filler in container A by weight, wherein the terminal hydroxyl polyether polyol and the chain extender cannot be zero at the same time, and stir evenly to obtain component A; (2) preparing component B: adding 40 to 60 parts by weight of isocyanate and 30 to 65 parts by weight of linear polyether polyol to container B at a temperature of 60 to 80°C, and stirring to obtain component B; (3) Component A and component B are uniformly mixed in a weight ratio of 1:0.3-3 to obtain a polyurethane polyurea foam material.

7. The polyurethane polyurea foam material according to claim 1 is used in industrial applications of hard and soft polyurea foams.