Biomass polymer suspension dispersion system as well as preparation method and application thereof

Through the biomass polymer suspension dispersion system, the problems of low polymer active ingredients and poor environmental friendliness in the development of unconventional oil and gas reservoirs are solved, and efficient and low-damage fracturing fluid preparation is achieved, which meets ultra-low permeability and tight oil and gas development needs and improve environmental friendliness.

CN118956370APending Publication Date: 2024-11-15JIANGSU JINQIAO OIL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411043216.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The ultra-low permeability and low pore characteristics of unconventional oil and gas reservoirs make it difficult to develop. The existing volume fracturing fluid has a small amount of effective components of polymers and is poor in environmentally friendly. The fracturing fluid in the form of emulsion is often used in the aqueous phase. It is easy to form a 'fish eye' in the middle, affecting efficiency.

Method used

Using a biomass polymer suspension dispersion system, including more than 90 wt% of biomass materials and less than 10 wt% of non-biomass materials, modified carboxymethylcellulose sodium, fatty alcohol polyoxyethylene ether, polylactic acid, polyethylene B Components such as glycol diesters, fatty amide propyl betaine and monohydric alcohol ester are prepared through specific preparation methods to ensure that the polymer is suspended and dispersed in water, avoid residue damage and improve environmental friendliness.

Benefits of technology

It realizes efficient fracturing fluid preparation, reduces residue rate and core damage rate in high-temperature and high-pressure environments, improves drag reduction rate and environmental friendliness, meets the needs of ultra-low permeability and tight oil and gas development, and reduces freshwater resources. dependency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956370A_ABST
    Figure CN118956370A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of hydraulic fracturing of unconventional oil and gas fields, and particularly relates to a biomass polymer suspension dispersion system as well as a preparation method and application of the biomass polymer suspension dispersion system. The biomass material comprises modified sodium carboxymethyl cellulose powder, fatty alcohol-polyoxyethylene ether, polylactic acid, polyethylene glycol diester, fatty amide propyl betaine and monohydric alcohol ester, and the non-biomass material comprises a polyacrylamide polymer, persulfate and potassium chloride. The invention has the advantages of excellent performance, ultralow harm and excellent environmental friendliness; the salt resistance is excellent, 0-10 * 10 < 4 > mg / L formation water can be directly used for being directly mixed with the variable-viscosity fracturing fluid, and dependence on fresh water resources is avoided; the requirements of development of ultra-low permeability tight oil gas and shale gas for high displacement, low damage and integrated continuous liquid preparation are met, and the requirement that renewable green materials are utilized for production and processing advocated by the environmental protection policy is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydraulic fracturing of unconventional oil and gas fields, and specifically relates to a biomass polymer suspension dispersion system and a preparation method and application thereof. Background Art

[0002] With the increase in energy demand for economic development, conventional oil and gas resources are no longer sufficient to meet the needs of today's development; therefore, the development of unconventional oil and gas resources has made up for this gap to some extent. However, the physical properties of ultra-low permeability and low porosity of unconventional oil and gas reservoirs make their development difficult, and large-scale "volume fracturing" technology has become an efficient means of developing unconventional oil and gas.

[0003] At present, in order to achieve large-scale volume fracturing construction on site, the "integrated" continuous mixing technology is often used. Different from the traditional pre-mixing and placing the liquid in the storage tank, the "integrated" fracturing technology adopts the on-site ready-to-use method. Since the powder fracturing fluid thickener and additives need a certain amount of time to hydrate and are easy to gather in the water phase to form "fish eyes", the "integrated" continuous mixing fracturing fluid often uses emulsion polymers or a suspension dispersion system in which the polymer is dispersed in the oil phase to prepare fracturing. Field applications have found that the content of effective polymer components in the emulsion polymer system is relatively low, generally not exceeding 30%; while the polyacrylamide polymer suspension dispersion system prepared with mineral oil as the dispersion medium can have an effective solid content of more than 40%. The prepared fracturing fluid has formed residues after gel breaking, and its environmental friendliness is poor. Summary of the invention

[0004] The purpose of the present invention is to provide a biomass polymer suspension dispersion system and a preparation method and application thereof, which can retain the advantages of the polymer suspension dispersion system while avoiding the residue damage caused by the preparation of fracturing fluid and improving the environmental friendliness of the system.

[0005] In order to solve the above technical problems, the present invention provides a biomass polymer suspension dispersion system, including more than 90wt% of biomass materials and less than 10% of non-biomass materials, wherein the biomass materials include modified sodium carboxymethyl cellulose powder, fatty alcohol polyoxyethylene ether, polylactic acid, polyethylene glycol diester, fatty amide propyl betaine and monohydric alcohol ester, and the non-biomass materials include polyacrylamide polymers, persulfate and potassium chloride.

[0006] Furthermore, the modified sodium carboxymethyl cellulose powder accounts for 25% to 45% of the total amount of the biomass polymer suspension dispersion system, has a degree of substitution between 0.3 and 1.8, and a particle size of 80 to 140 meshes. The modified sodium carboxymethyl cellulose powder is one of sodium sulfonate-modified sodium carboxymethyl cellulose, hydroxypropyl-modified sodium carboxymethyl cellulose, and hydroxyethyl sodium carboxymethyl cellulose. The modified sodium carboxymethyl cellulose mainly functions to thicken after being dissolved in water and has strong salt resistance.

[0007] Furthermore, the fatty alcohol polyoxyethylene ether accounts for 5% to 15% of the total amount of the biomass polymer suspension dispersion system, and the fatty alcohol polyoxyethylene ether is one or more of lauric acid polyoxyethylene ether, stearic acid polyoxyethylene ether, palmitic acid polyoxyethylene ether, and oleic acid polyoxyethylene ether; the fatty alcohol polyoxyethylene ether mainly helps the polymer powder to disperse in the monohydric alcohol ester solvent to avoid agglomeration, and increase the speed at which the polymer suspension dispersion system dissolves in water, while playing the role of assisting the drainage of the fracturing fluid.

[0008] Furthermore, the molecular weight of the polylactic acid is 5000-50000; the polyethylene glycol diester is one of polyethylene glycol diethyl ester, polyethylene glycol dibutyl ester, polyethylene glycol diisopropyl ester and polyethylene glycol diisooctyl ester, wherein the degree of polymerization of polyethylene glycol is 200-2000; the mass ratio of the polylactic acid to the polyethylene glycol diester is 1-5:2-3, and the sum of the masses of the polylactic acid and the polyethylene glycol diester accounts for 3%-6% of the total amount of the biomass polymer suspension dispersion system; the polylactic acid and the polyethylene glycol diester are both suspension dispersion system stabilizers, which are used to increase the viscosity of the suspension dispersion system and ensure that the suspension dispersion system does not stratify when standing for a long time.

[0009] Furthermore, the fatty amide propyl betaine accounts for 5% to 10% of the total amount of the biomass polymer suspension dispersion system, and the fatty amide propyl betaine is one of lauryl amide propyl betaine, palmitamide propyl betaine, oleyl amide propyl betaine, and myristic amide propyl betaine; the fatty amide propyl betaine can play a phase transition effect and accelerate the process of contact between the polymer and water in the suspension dispersion system.

[0010] Further, the monohydric alcohol ester is one or more of isooctyl laurate, isooctyl myristate, isooctyl palmitate, isooctyl stearate, isopropyl laurate, and isopropyl myristate, and its viscosity is required to be 4.5 to 6.6 m 2 / s, surface tension range is 24~31mN / m, density is 0.8~0.92g / cm 3 ; The monohydric alcohol ester is the dispersion medium of the suspension dispersion system.

[0011] Furthermore, the molecular weight of the polyacrylamide polymer is 10 million to 15 million, the particle size is 100 to 140 meshes, and the polyacrylamide polymer accounts for 1% to 5% of the total amount of the biomass polymer suspension dispersion system; the polyacrylamide polymer mainly acts as a drag reducer, and its drag reduction rate for mineralized water should be above 80%.

[0012] Furthermore, the persulfate is one of ammonium persulfate, sodium persulfate and potassium persulfate, and the persulfate accounts for 0.5% to 2% of the total amount of the biomass polymer suspension dispersion system; the persulfate is a degumming agent, which destroys the long-chain structure of the high-molecular polymer under high-temperature conditions in the formation; the potassium chloride is an anti-swelling agent, and it accounts for 2% to 5% of the total amount of the biomass polymer suspension dispersion system.

[0013] On the other hand, the present invention also provides a method for preparing a biomass polymer suspension dispersion system. The method for preparing the above-mentioned biomass polymer suspension dispersion system comprises: firstly heating the monohydric alcohol ester to 40-60°C, stirring at high speed, successively adding fatty alcohol polyoxyethylene ether, polylactic acid, polyethylene glycol diester, and fatty amide propyl betaine in proportion until they are completely dissolved, maintaining the stirring speed at above 800r / min, successively adding modified sodium carboxymethyl cellulose powder, polyacrylamide polymer, persulfate and potassium chloride in proportion, stirring for 30min-90min, and obtaining a polymer dispersion system.

[0014] The present invention also provides a method for applying a biomass polymer suspension dispersion system in a variable viscosity fracturing fluid, the method comprising: preparing a fracturing fluid with a water mineralization range of 10×10 4 mg / L, pumping volume is 1~20m 3 / h, and control the dripping rate of the polymer dispersion system at the wellhead according to the displacement, so that the addition amount of the polymer dispersion system in water is 0.02wt%~0.5wt%, among which 0.02wt%~0.06wt% is a low viscosity system, 0.06wt%~0.3wt% is a medium viscosity system, and 0.1wt%~0.5wt% is a high viscosity system.

[0015] The beneficial effects of the present invention are:

[0016] 1. The biomass polymer suspension dispersion system of the present invention uses biomass monohydric alcohol ester as suspension dispersant, polylactic acid and polyethylene glycol diester as stabilizers, fatty alcohol polyoxyethylene ether and fatty amide betaine as auxiliary agents, and suspends and disperses modified sodium carboxymethyl cellulose powder and polyacrylamide powder in monohydric alcohol ester to prepare a biomass suspension dispersion system. Among them, various biomass auxiliary agents have the characteristics of low residue, low damage, zero pollution and mineralization resistance. It can use 10×10 4The fracturing fluid can be directly prepared with formation water with a mineralization degree of 100 mg / L. The high-temperature residue of the fracturing fluid is less than 5 mg / L, the damage rate of the breaker liquid to the tight core is less than 5%, and the drag reduction rate can reach up to 81%. This technology not only meets the needs of ultra-low permeability tight oil and gas and shale gas development for high displacement, low damage, and integrated continuous preparation, but also complies with the environmental protection policy's advocacy of using renewable green materials for production and processing. The residue rate of the present invention is extremely low under high temperature and high pressure conditions, and the damage to the low permeability reservoir is extremely small.

[0017] 2. The present invention can retain the advantages of the polymer suspension dispersion system while avoiding the residue damage caused by the preparation of the fracturing fluid and improving the environmental friendliness of the system. It has excellent performance, ultra-low damage and excellent environmental friendliness.

[0018] 3. The salt tolerance of the present invention is excellent and can be directly used in 0-10×10 4 mg / L formation water is directly mixed with viscous fracturing fluid to get rid of dependence on fresh water resources.

[0019] 4. The drag reduction rate of the present invention is high. After the modified sodium cellulose is fully dissolved, the high viscosity system is heated to 160°C and 170s. -1 At the shear rate, after 2h of shearing, the apparent viscosity is maintained above 50mPa·s, that is, it still has good sand carrying performance in high temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solution of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 The variation of the pressure difference at both ends of the circulation pipeline of the friction meter with time after adding the water phase to the biomass polymer suspension dispersion system prepared in Example 1;

[0022] Figure 2 The variation law of drag reduction rate with increasing displacement after adding water phase to the biomass polymer suspension dispersion system prepared in Example 1;

[0023] Figure 3 The apparent viscosity of the biomass polymer suspension dispersion system changes with time after adding water phase at different temperatures;

[0024] Figure 4 The high viscosity fracturing fluid prepared for biomass polymer suspension dispersion system was tested for heat and shear resistance at 160℃ and 170s-1;

[0025] Figure 5The damage rate of high-viscosity fracturing fluid degelling fluid to the core changes with the injection multiples at different temperatures. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] The preparation method of the biomass polymer suspension dispersion system is as follows:

[0029] S1: 25 parts of isooctyl laurate and 20 parts of isopropyl laurate are placed in a reaction kettle and heated to 60°C;

[0030] S2: 3 parts of myristyl alcohol polyoxyethylene ether, 2 parts of polylactic acid (molecular weight 10000), 2 parts of polyethylene glycol diisooctyl ester (degree of polymerization 1000), and 3 parts of cocamidopropyl betaine were added to a reactor, stirred at a mechanical speed of 800 r / min for 30 min until they were completely dissolved, and then the system temperature was reduced to 40° C.;

[0031] S3: Increase the mechanical stirring speed to 1000r / min, evenly mix 3 parts of potassium chloride solid powder (200 mesh), 2 parts of ammonium persulfate powder (200 mesh), 5 parts of polyacrylamide drag reducer powder (molecular weight 10 million, particle size 120 mesh) and sulfonic acid modified sodium carboxymethyl cellulose powder (substitution degree 0.9, molecular weight 5 million, particle size 140 mesh), and slowly add them into the reactor to fully suspend and disperse the powder in the monohydric alcohol ester system, and continue stirring for 90 minutes to obtain a bio-based suspension dispersion system.

[0032] Example 2

[0033] The mineral composition of water produced from Well A in a certain formation in the Ordos Basin was tested, and its mineralization is shown in Table 1.

[0034] Table 1 Water production from well A in a certain area of ​​the Ordos Basin

[0035]

[0036] The bio-based suspension dispersion system prepared in Example 1 was dissolved in the simulated produced water of Well A to prepare a fracturing fluid, and a fracturing fluid friction meter was used to analyze and test the time for the viscous fracturing fluid to exert the best drag reduction and the highest drag reduction rate. The test method is as follows:

[0037] S1: Add 10L of simulated produced water from well A in a certain formation in the Ordos Basin into the circulation tank of the fracturing fluid friction tester, and start the mechanical stirring in the tank at a stirring speed of 100r / min;

[0038] S2: Set the circulation displacement to 35L / min, circulate the simulated formation water in the pipeline, and drip 10g of the bio-based suspension dispersion system into the circulation tank;

[0039] S3: Record the pressure difference change at both ends of the circulation pipeline until the pressure difference stabilizes. Calculate the drag reduction rate under the displacement according to the following formula. The test results are as follows: Figure 1 .

[0040]

[0041] Among them, ΔP0 is the pressure drop of pure water, Pa; ΔP1 is the stable pressure drop after adding the dispersed system, Pa.

[0042] like Figure 1 As shown, the test results show that after adding the bio-based suspended dispersion system prepared in Example 1 to the simulated produced water of Well A for 48 seconds, the pressure difference of the circulation pipeline can be stabilized, that is, the maximum drag reduction rate is achieved, and the drag reduction rate can reach 76%. The results show that the polyacrylamide polymer drag reducer in the suspended dispersion system exerts the best effect within 48 seconds.

[0043] Adjust the displacement of the fracturing fluid friction meter and test the drag reduction rate of the medium viscosity fracturing fluid in the displacement range of 20 to 45 L / min. The test results are as follows: Figure 2 As shown, the drag reduction rate increases with the increase of displacement, and tends to be stable when the displacement reaches 40L / min, and the drag reduction rate can reach 79.8%.

[0044] Example 3

[0045] Take a 1000mL beaker, add 500mL of simulated produced water from well A in a certain formation in the Ordos Basin mentioned in Example 2, place the beaker in a water bath and set it to a certain temperature for heating, use mechanical stirring to continuously stir at a speed of 1000r / min, add 6g of the biomass suspension dispersion system prepared in Example 1 to the beaker, prepare a high-viscosity fracturing fluid, and then stir it every 30s for 170s. -1 The apparent viscosity under the conditions, the test results are as follows Figure 3 .

[0046] like Figure 3As shown in the figure, the reason why the apparent viscosity of high-viscosity fracturing fluid increases with time is that the hydration of modified sodium carboxymethyl cellulose takes a certain amount of time. At low temperature of 20°C, it takes 270 seconds to achieve complete hydration, and the apparent viscosity reaches a stable level of 245 mPa·s; at 40°C, it takes 120 seconds to achieve complete hydration, and the apparent viscosity reaches a stable level of 239 mPa·s.

[0047] Example 4

[0048] The high viscosity fracturing fluid prepared in Example 3 was subjected to temperature and shear resistance test analysis using a high temperature and high pressure rheometer, with the target temperature set at 160°C and the shear rate set at 170s. -1 , continue shearing for 120 minutes, observe the apparent viscosity remaining, the test results are as follows Figure 4 shown.

[0049] like Figure 4 As shown, the high viscosity fracturing fluid prepared in Example 3 was heated at 160°C and a shear rate of 170s -1 Under the same conditions, after continuous shearing for 120 min, the apparent viscosity was maintained above 50 mPa·s, showing excellent temperature resistance.

[0050] Example 5

[0051] The gel breaking conditions of the high viscosity fracturing fluid prepared in Example 3 at 60°C, 90°C, 120°C and 160°C are shown in Table 2.

[0052] Table 2 Gel breaking of high viscosity fracturing fluid prepared in Example 3 at different temperatures

[0053]

[0054] As shown in Table 2, the degelling liquid for preparing the high-viscosity fracturing fluid in Example 3 has a surface tension lower than 28 mN / m, an interfacial tension lower than 0.1 mN / m, and a residue content lower than 5 mg / L.

[0055] Example 6

[0056] The debonding liquid in Example 5 was used to conduct a displacement test on the core to evaluate its damage rate to the core. The evaluation method is: the core is an artificial core with a porosity of 8.7% and a permeability of 0.9 mD. The test method is to drive saturated sodium chloride brine into the artificial core at a certain temperature to achieve equilibrium, and obtain the original permeability K0 according to the Darcy formula, and then calculate the permeability K1 after the debonding liquid is balanced at the corresponding temperature, and calculate the core damage rate (η) according to the following formula.

[0057]

[0058] The relationship between core damage rate and injection multiple is as follows: Figure 5 As shown, the test results show that the damage rate of the degelling fluid produced in Example 5 to the low-permeability core is less than 5%, reflecting that the fracturing fluid prepared by the bio-based suspension dispersion system has excellent cleanliness and low damage.

[0059] The above disclosures are only several preferred embodiments of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A biomass polymer suspension dispersion system, It is characterized in that It includes more than 90wt% of biomass materials and less than 10% of non-biomass materials, wherein the biomass materials include modified sodium carboxymethyl cellulose powder, fatty alcohol polyoxyethylene ether, polylactic acid, polyethylene glycol diester, fatty amide propyl betaine and monohydric alcohol ester, and the non-biomass materials include polyacrylamide polymers, persulfate and potassium chloride.

2. A biomass polymer suspension dispersion system according to claim 1, It is characterized in that The modified sodium carboxymethyl cellulose powder accounts for 25% to 45% of the total amount of the biomass polymer suspension dispersion system, has a degree of substitution between 0.3 and 1.8, and a particle size of 80 to 140 meshes. The modified sodium carboxymethyl cellulose powder is one of sodium sulfonate modified sodium carboxymethyl cellulose, hydroxypropyl modified sodium carboxymethyl cellulose, and hydroxyethyl sodium carboxymethyl cellulose.

3. A biomass polymer suspension dispersion system according to claim 1, It is characterized in that The fatty alcohol polyoxyethylene ether accounts for 5% to 15% of the total amount of the biomass polymer suspension dispersion system, and the fatty alcohol polyoxyethylene ether is one or more of lauric acid polyoxyethylene ether, stearic acid polyoxyethylene ether, palmitic acid polyoxyethylene ether, and oleic acid polyoxyethylene ether.

4. A biomass polymer suspension dispersion system according to claim 1, It is characterized in that The molecular weight of the polylactic acid is 5000-50000; the polyethylene glycol diester is one of polyethylene glycol diethyl ester, polyethylene glycol dibutyl ester, polyethylene glycol diisopropyl ester and polyethylene glycol diisooctyl ester, wherein the degree of polymerization of polyethylene glycol is 200-2000; the mass ratio of the polylactic acid to the polyethylene glycol diester is 1-5:2-3, and the sum of the masses of the polylactic acid and the polyethylene glycol diester accounts for 3%-6% of the total amount of the biomass polymer suspension dispersion system.

5. The biomass polymer suspension dispersion system according to claim 1, It is characterized in that The fatty amide propyl betaine accounts for 5% to 10% of the total amount of the biomass polymer suspension dispersion system, and the fatty amide propyl betaine is one of lauramide propyl betaine, palmitamide propyl betaine, oleamide propyl betaine and myristic amide propyl betaine.

6. A biomass polymer suspension dispersion system according to claim 1, It is characterized in that The monohydric alcohol ester is one or more of isooctyl laurate, isooctyl myristate, isooctyl palmitate, isooctyl stearate, isopropyl laurate, and isopropyl myristate, and its viscosity is required to be between 4.5 and 6.6 m 2 / s, surface tension range is 24~31mN / m, density is 0.8~0.92g / cm 3 .

7. The biomass polymer suspension dispersion system according to claim 1, It is characterized in that The molecular weight of the polyacrylamide polymer is 10 million to 15 million, the particle size is 100 to 140 meshes, and the polyacrylamide polymer accounts for 1% to 5% of the total amount of the biomass polymer suspension dispersion system.

8. The biomass polymer suspension dispersion system according to claim 1, It is characterized in that The persulfate is one of ammonium persulfate, sodium persulfate and potassium persulfate, and the persulfate accounts for 0.5% to 2% of the total amount of the biomass polymer suspension dispersion system; the potassium chloride accounts for 2% to 5% of the total amount of the biomass polymer suspension dispersion system.

9. A method for preparing a biomass polymer suspension dispersion system, comprising preparing the biomass polymer suspension dispersion system according to any one of claims 1 to 8, It is characterized in that The method comprises: firstly heating the monohydric alcohol ester to 40-60°C, stirring at high speed, successively adding fatty alcohol polyoxyethylene ether, polylactic acid, polyethylene glycol diester and fatty amide propyl betaine in proportion until they are completely dissolved, maintaining the stirring speed at above 800r / min, successively adding modified sodium carboxymethyl cellulose powder, polyacrylamide polymer, persulfate and potassium chloride in proportion, stirring continuously for 30min-90min, and obtaining a polymer dispersion system.

10. A method for applying a biomass polymer suspension dispersion system in a variable viscosity fracturing fluid, It is characterized in that The method comprises: preparing a fracturing fluid with a water salinity range of 10×10 4 mg / L, pumping volume is 1~20m 3 / h, and control the dripping rate of the polymer dispersion system at the wellhead according to the displacement, so that the addition amount of the polymer dispersion system in water is 0.02wt%~0.5wt%, among which 0.02wt%~0.06wt% is a low viscosity system, 0.06wt%~0.3wt% is a medium viscosity system, and 0.1wt%~0.5wt% is a high viscosity system.