Experimental method for obtaining dynamic fracture toughness of double-material sample

By combining a uniaxial bidirectional electromagnetic Hopkinson bar loading system with experimental-numerical simulation, the accuracy problem of dynamic fracture toughness testing of dual-material specimens was solved, and the evaluation of pure I-type opening and energy absorption capacity of the adhesive interface was realized.

CN118961467APending Publication Date: 2024-11-15NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411325755.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Most existing methods for testing the dynamic fracture toughness of dual-material specimens are based on quasi-static loading and lack high-speed dynamic testing methods. Furthermore, existing methods often result in inaccurate results.

Method used

A uniaxial bidirectional electromagnetic Hopkinson bar loading system was used to perform bidirectional dynamic synchronous loading on dual-material specimens. Combining experimental and numerical simulation methods, the bending stiffness matching design was used to ensure that the specimens had the same bending deformation during loading. The fracture toughness value was calculated using a combination of experimental and numerical simulation methods.

Benefits of technology

It achieves pure I-type opening of bimaterial specimens, improves the accuracy of dynamic fracture toughness testing, and can more accurately evaluate the energy absorption and fracture propagation capacity of the adhesive interface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961467A_ABST
    Figure CN118961467A_ABST
Patent Text Reader

Abstract

The invention discloses an experimental method for obtaining dynamic fracture toughness of a double-material sample, and belongs to the technical field of material dynamic fracture toughness tests.The experimental method comprises the steps that the double-material sample formed by gluing double materials is designed based on a bending rigidity matching method, so that equivalent bending deformation of the double-material sample in the loading process is guaranteed; the method comprises the following steps: establishing a single-axis bidirectional electromagnetic Hopkinson pull rod loading system, fixing a double-material sample on the single-axis bidirectional electromagnetic Hopkinson pull rod loading system, and carrying out bidirectional dynamic synchronous loading on the double-material sample to realize synchronous opening of the double-material sample, so as to obtain pure I-type opening; the loading speed of the bi-material sample, the time-varying curve of the displacement of the incident bar and the dynamic fracture starting time of the bi-material sample are collected, and the fracture toughness value of the cementing interface of the bi-material sample is more accurately calculated by adopting an experiment-numerical simulation combined method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material dynamic fracture toughness testing, and in particular relates to an experimental method for obtaining dynamic fracture toughness of a double-material sample. Background Art

[0002] The dual-material bonding interface, also known as the bonding interface, is an interface composed of two materials with different physical and chemical properties, such as metal-metal, composite-composite, and metal-composite interfaces. The meaning of dynamic mode I fracture toughness is: the opening type (i.e., the mode in which the crack is parallel to the loading direction and away from the loading edge) fracture toughness during the fracture extension process of the material interface or crack under dynamic loading conditions. According to the fracture behavior of the interface, it can be divided into: opening type (type I), sliding type (type II), tearing type (type III) and mixed type fracture. Among them, type I is the most common, most dangerous, and most deeply studied interface fracture type in engineering, because it is one of the main causes of low stress fracture. The opening type I fracture toughness of the bonding interface is one of the main forms of cracking of the bonding interface, and it is also one of the key parameters for evaluating bonding performance.

[0003] Dual-material bonded structures are widely used in aerospace and other fields, and often serve in complex environments such as high-speed impact. Determining the type I fracture toughness of materials under dynamic loading conditions is of great significance for understanding the fracture behavior of materials under dynamic loading conditions such as high-speed collision and explosion, as well as for related engineering design and safety assessment. However, most of the current tests on dual-material bonding interfaces at home and abroad are quasi-static loading, and there is still a lack of high-speed dynamic test methods. For example, ISO 25217 for composite bonded structures, and its determination method refers to the test method for type I fracture toughness between composite layers, but this test method does not specify a standard process for dual-material bonding. For example, the existing invention patent - a damage evolution characterization method for coupled failure behavior of heterogeneous adhesive joints, although a test method for dual-material bonding is proposed, the method is complicated and requires multiple sets of tests on bonding of homogeneous materials of equal thickness. In addition, the dual cantilever beam specimens of equal thickness generate shear force during the opening process due to the different bending stiffness of the specimens, which introduces type II fracture and causes inaccurate test results. British scholar Liβner M used a wedge-shaped double cantilever beam (WDCB) specimen to conduct a dynamic loading experiment in a Hopkinson bar (SHPB) system and obtained the dynamic fracture toughness of the dual-material bonding interface. However, this experiment introduced friction and eccentricity of the loading rod, which led to inaccurate results. Summary of the invention

[0004] The present invention aims to provide an experimental method for obtaining dynamic fracture toughness of a dual-material specimen, which solves the problem that most existing test methods for obtaining dynamic fracture toughness of dual-material specimens are quasi-static loading and have defects in high-speed dynamic test methods.

[0005] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is as follows:

[0006] An experimental method for obtaining dynamic fracture toughness of a dual-material specimen is provided, comprising:

[0007] Step 1, preparing a dual material sample;

[0008] Step 2: Build a uniaxial bidirectional electromagnetic Hopkinson rod loading system, and fix the bi-material specimen on the uniaxial bidirectional electromagnetic Hopkinson rod loading system;

[0009] Step 3, starting the uniaxial bidirectional electromagnetic Hopkinson rod loading system to perform bidirectional dynamic synchronous loading on the bi-material specimen;

[0010] Step 4, the uniaxial bidirectional electromagnetic Hopkinson rod loading system collects the loading speed of the bi-material sample, the displacement change curve of the incident rod in the uniaxial bidirectional electromagnetic Hopkinson rod loading system over time, and the dynamic fracture starting time of the bi-material sample;

[0011] Step 5: According to the displacement-time curve of the incident rod in the uniaxial bidirectional electromagnetic Hopkinson rod loading system and the dynamic fracture initiation time of the bi-material specimen, the fracture toughness value of the bonding interface of the bi-material specimen is calculated by combining the experimental and numerical simulation methods.

[0012] Further, in step 1, the dual-material specimen includes an upper beam plate and a lower beam plate made of different materials and bonded to each other; the bending stiffness of the upper beam plate and the lower beam plate is the same, that is:

[0013] E1I1=E2I2

[0014]

[0015] Among them, E1 is the bending modulus of the upper beam plate; I1 is the moment of inertia of the upper beam plate; E2 is the bending modulus of the lower beam plate; I2 is the moment of inertia of the lower beam plate; h1 is the thickness of the upper beam plate; h2 is the thickness of the lower beam plate.

[0016] Through the above arrangement, it is ensured that the bi-material specimen has the same bending deformation during the opening process, thereby obtaining a pure I-type opening.

[0017] Further, in step 2, the uniaxial bidirectional electromagnetic Hopkinson rod loading system includes a first incident rod, a second incident rod, an oscilloscope, a flash lamp, a high-speed camera and a computer;

[0018] The first incident rod and the second incident rod are arranged coaxially with a horizontal interval, and one end of each of the first incident rod and the second incident rod is provided with a stress wave generator, and each stress wave generator includes a primary coil and a secondary coil; the two stress wave generators are controlled by an electromagnetic control circuit; a strain gauge is provided at the middle position of the circumferential outer wall of each of the first incident rod and the second incident rod;

[0019] The bi-material sample is arranged between the first incident rod and the second incident rod, the two outer end surfaces of the bi-material sample are respectively bonded and fixed to one end of the first incident rod and the second incident rod, and a fracture strain gauge is arranged on the side of the bi-material sample;

[0020] The flash lamp and the high-speed camera are arranged on the side of the double-material sample; the oscilloscope is electrically connected with the fracture strain gauge, the flash lamp, the computer, the high-speed camera and the two strain gauges.

[0021] The uniaxial bidirectional electromagnetic Hopkinson rod loading system uses the stress pulse wave generated by electromagnetic energy conversion technology; the pulse is generated by closing the discharge switch, and there is almost no time delay between the triggering and closing of the discharge switch and the generation of the stress wave, so the precise time of the pulse generation can be easily controlled by the electromagnetic control circuit. This advantage ensures the synchronization of symmetrical loading of the dual-material specimen under dynamic loading.

[0022] Furthermore, in step 3, after the dual-material sample is completed, the voltage value and capacitance value in the electromagnetic control circuit are set according to the requirements of the loading rate of the dual-material sample, and the electromagnetic control circuit is charged to the set value, and the discharge switch is started to discharge the main coil of the stress generator until the capacitor voltage drops to 0V. The secondary coil will generate a loading stress wave under the action of the electromagnetic repulsion force, and the stress wave is simultaneously transmitted to the dual-material sample through the first incident rod and the second incident rod, and the dual-material sample is subjected to bidirectional dynamic synchronous loading.

[0023] Furthermore, the calculation formula for the loading speed of the dual-material specimen is:

[0024]

[0025] V1(t)=C0(ε 1,inc (t)-(ε 1,ref (t))

[0026] V2(t)=-C0(ε 2,inc (t)-(ε 2,ref (t))

[0027] V=V1(t)+V2(t)

[0028] Among them, ε is the strain signal, k value is the sensitivity coefficient of the selected strain gauge, U0 is the Wheatstone bridge voltage, ΔU is the voltage value output by the corresponding acquisition channel over time; C0 is the elastic wave velocity of the incident rod, ε 1,inc (t) and ε 2,inc (t) are the incident waves of the first incident bar and the second incident bar, ε 1,ref (t) and ε 2,ref (t) are the reflected waves of the first incident rod and the second incident rod, respectively; V is the loading speed of the bi-material specimen, V1(t) and V2(t) are the loading speeds of the first incident rod and the second incident rod, respectively;

[0029] The dynamic fracture initiation time of the bi-material specimen was determined by fracture strain gauge and high-speed camera, and the initiation fracture time was t f CPG and t f HSP In the present application, the time point at which the step of the fracture strain gauge occurs substantially coincides with the time point at which the crack of the adhesive layer is started as captured by the high-speed camera.

[0030] Furthermore, in step 5, the method of combining experiment and numerical simulation includes:

[0031] Step 5.1, integrating and calculating the loading speeds of the first incident rod and the second incident rod to obtain the displacement curves of the first incident rod and the second incident rod ends over time, and also determining the crack initiation time of the adhesive layer crack according to the fracture strain gauge and the high-speed camera;

[0032] The expression of the first incident rod displacement versus time curve is:

[0033]

[0034] The expression of the second incident rod displacement versus time curve is:

[0035]

[0036] Where C0 is the elastic wave velocity of the incident rod, ε 1,inc (t) and ε 2,inc (t) are the incident waves of the first incident bar and the second incident bar, ε 1,ref (t) and ε 2,ref (t) are the reflected waves of the first incident rod and the second incident rod, respectively;

[0037] Step 5.2, establish a dual-material specimen simulation model in the finite element software, and use the displacement curves of the first incident rod and the second incident rod ends over time as boundary conditions of the simulation model to perform displacement loading on the simulation model;

[0038] Step 5.3: Output the relative displacement and nodal force of the crack tip node of the adhesive layer in the numerical simulation results;

[0039] Step 5.4: The relative displacement and node force of the crack tip node of the adhesive layer output in the numerical simulation results are used to calculate the change curve of fracture toughness over time. The dynamic fracture starting time t f CPG and t f HSP Determine the dynamic fracture toughness value of the bonding interface of the bi-material specimen.

[0040] In the above technical solution, the influence of inertia effect on the bi-material specimen under dynamic loading is considered, and an experimental-numerical hybrid method is used to more accurately obtain the dynamic fracture toughness of the bi-material specimen.

[0041] Furthermore, in step 5.4, the dynamic mode I fracture toughness value of the bonding interface of the bi-material specimen is calculated using the modified virtual crack closure method, and the calculation formula is:

[0042]

[0043] Among them, G Ⅰ is the dynamic mode I fracture toughness value of the bonding interface of the bi-material specimen; F y1 When the fracture is of mode I, the node force at the crack tip of the adhesive layer, Δv 3,4 is the relative displacement of the crack tip node of the adhesive layer during mode I fracture, b is the width of the bi-material specimen, and Δa is the unit size of the grid for the bi-material specimen simulation model.

[0044] The beneficial effects of the present invention are as follows: the experimental method for obtaining dynamic fracture toughness of the dual-material specimen in the present invention is mainly used to test the interface dynamic fracture toughness of two different materials (including metal and metal, composite material and composite material, metal and composite material, etc.) that are bonded, solidified or connected in other ways to form a structural member, so as to evaluate the energy that the interface can absorb during the fracture process and its ability to resist fracture extension. Based on a uniaxial bidirectional electromagnetic Hopkinson rod loading system, a uniaxial bidirectional synchronous loading method can be used to achieve synchronous opening of the dual-material specimen, and at the same time, the dual-material specimen bonded by the dual materials is designed based on the bending stiffness matching method to ensure equal bending deformation of the dual-material specimen during the loading process, thereby obtaining a pure I-type opening, and more accurately calculating the fracture toughness value of the bonding interface of the dual-material specimen by using a combination of experimental and numerical simulation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 Flowchart of the experimental method to obtain the dynamic fracture toughness for a bi-material specimen.

[0046] Figure 2 It is a structural schematic diagram of a uniaxial bidirectional electromagnetic Hopkinson rod loading system.

[0047] Figure 3 Schematic diagram of the structure of the dual-material specimen.

[0048] Figure 4 Schematic diagram of the dual-material specimen simulation model.

[0049] Among them, 1. double material specimen; 101. upper beam plate; 102. lower beam plate; 2. first incident rod; 3. second incident rod; 4. oscilloscope; 5. flash; 6. high-speed camera; 7. computer; 8. stress wave generator; 801. main coil; 802. secondary coil; 9. electromagnetic control circuit; 10. strain gauge; 11. fracture strain gauge. DETAILED DESCRIPTION

[0050] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0051] like Figure 1 As shown, the present invention provides an experimental method for obtaining dynamic fracture toughness of a dual-material specimen 1, which comprises:

[0052] Step 1, preparing a dual material sample 1;

[0053] Step 2: build a uniaxial bidirectional electromagnetic Hopkinson rod loading system, and fix the bi-material sample 1 on the uniaxial bidirectional electromagnetic Hopkinson rod loading system;

[0054] Step 3, starting the uniaxial bidirectional electromagnetic Hopkinson rod loading system to perform bidirectional dynamic synchronous loading on the bi-material sample 1;

[0055] Step 4, the uniaxial bidirectional electromagnetic Hopkinson rod loading system collects the loading speed of the bi-material sample 1, the curve of the displacement of the incident rod in the uniaxial bidirectional electromagnetic Hopkinson rod loading system changing with time, and the dynamic fracture starting time of the bi-material sample 1;

[0056] Step 5: According to the displacement-time curve of the incident rod in the uniaxial bidirectional electromagnetic Hopkinson rod loading system and the dynamic fracture initiation time of the bi-material specimen 1, the fracture toughness value of the bonding interface of the bi-material specimen 1 is calculated by using a combined experimental-numerical simulation method.

[0057] Specifically, Figure 3As shown, in step 1, the dual-material specimen 1 includes an upper beam plate 101 and a lower beam plate 102 made of different materials and bonded to each other; the upper beam plate 101 and the lower beam plate 102 have the same bending stiffness, that is:

[0058] E1I1=E2I2

[0059]

[0060] Among them, E1 is the bending modulus of the upper beam plate 101; I1 is the moment of inertia of the upper beam plate 101; E2 is the bending modulus of the lower beam plate 102; I2 is the moment of inertia of the lower beam plate 102; h1 is the thickness of the upper beam plate 101; h2 is the thickness of the lower beam plate 102.

[0061] Through the above arrangement, it is ensured that the bi-material specimen 1 has the same bending deformation during the opening process, thereby achieving pure I-type opening.

[0062] like Figure 2 As shown, in step 2, the uniaxial bidirectional electromagnetic Hopkinson rod loading system includes a first incident rod 2, a second incident rod 3, an oscilloscope 4, a flash lamp 5, a high-speed camera 6 and a computer 7;

[0063] The first incident rod 2 and the second incident rod 3 are arranged coaxially with a horizontal interval, and one end of the first incident rod 2 and the second incident rod 3 is provided with a stress wave generator 8, and each stress wave generator 8 includes a primary coil 801 and a secondary coil 802; the two stress wave generators 8 are controlled by an electromagnetic control circuit 9; a strain gauge 10 is provided at the middle position of the circumferential outer wall of the first incident rod 2 and the second incident rod 3;

[0064] The bi-material sample 1 is arranged between the first incident rod 2 and the second incident rod 3 , and the two outer end faces of the bi-material sample 1 are respectively bonded and fixed to one end of the first incident rod 2 and the second incident rod 3 , and a fracture strain gauge 11 is arranged on the side of the bi-material sample 1 .

[0065] The flash lamp 5 and the high-speed camera 6 are arranged on the side of the bi-material sample 1 ; the oscilloscope 4 is electrically connected to the fracture strain gauge 11 , the flash lamp 5 , the computer 7 , the high-speed camera 6 and the two strain gauges 10 .

[0066] The uniaxial bidirectional electromagnetic Hopkinson rod loading system utilizes the stress pulse wave generated by electromagnetic energy conversion technology; the pulse is generated by closing the discharge switch, and there is almost no time delay between the triggering and closing of the discharge switch and the generation of the stress wave, so the precise time of the pulse generation can be easily controlled by the electromagnetic control circuit 9. This advantage ensures the synchronization of the symmetrical loading of the bimaterial specimen 1 under dynamic loading.

[0067] Specifically, two strain gauges 10 are connected to the oscilloscope 4 in the form of a Wheatstone bridge connection, wherein the first incident rod 2 and the second incident rod 3 are made of titanium alloy, with an elastic modulus of 110 GPa, an elastic wave velocity of 4849.5 m / s, a diameter of 18 mm, and a length of 3500 mm; the resistance of the strain gauge 10 is 1000 Ω, and the sensitivity coefficient is 1.92. In addition, a high-speed camera 6 is set up to record the deformation of the sample and the start time of the crack extension of the adhesive layer. The frame rate of the high-speed camera 6 is set to 400,000 fps, and the total number of frames shot is 180, so the corresponding shooting time is 450 μs. When the high-speed camera 6 starts shooting, it will pass the feedback signal to the oscilloscope 4, and a high-intensity flash 5 is also needed for fill light, which is triggered by the output signal of the oscilloscope 4. A fracture strain gauge 11 is also pasted at the preset crack on the side of the sample to monitor the start of the crack in the adhesive layer, and the signal is also recorded by the oscilloscope 4.

[0068] In step 3, after the bi-material sample 1 is completed, the voltage value and capacitance value in the electromagnetic control circuit 9 are set according to the requirements of the loading rate of the bi-material sample 1, and the electromagnetic control circuit 9 is charged to the set value, and the discharge switch is started to discharge the main coil 801 of the stress generator until the capacitor voltage drops to 0V, and the secondary coil 802 will generate a loading stress wave under the action of the electromagnetic repulsion force. The stress wave is simultaneously transmitted to the bi-material sample 1 through the first incident rod 2 and the second incident rod 3, and the bi-directional dynamic synchronous loading is performed on the bi-material sample 1.

[0069] Furthermore, the calculation formula for the loading speed of the dual-material specimen 1 is:

[0070]

[0071] V1(t)=C0(ε 1,inc (t)-(ε 1,ref (t))

[0072] V2(t)=-C0(ε 2,inc (t)-(ε 2,ref (t))

[0073] V=V1(t)+V2(t)

[0074] Wherein, ε is the strain signal, k value is the sensitivity coefficient of the selected strain gauge 10, U0 is the Wheatstone bridge voltage, ΔU is the voltage value output by the corresponding acquisition channel over time; C0 is the elastic wave velocity of the incident rod, ε 1,inc (t) and ε 2,inc (t) are the incident waves of the first incident rod 2 and the second incident rod 3, ε 1,ref (t) and ε 2,ref(t) are the reflected waves of the first incident rod 2 and the second incident rod 3, respectively; V is the loading speed of the bi-material specimen 1, V1(t) and V2(t) are the loading speeds of the first incident rod 2 and the second incident rod 3, respectively;

[0075] The dynamic fracture initiation time of the bi-material specimen 1 is determined by the fracture strain gauge 11 and the high-speed camera 6 as t f CPG and t f HSP In the present application, the time point at which the step of the fracture strain gauge 11 occurs substantially coincides with the time point at which the crack of the adhesive layer is started as captured by the high-speed camera 6 .

[0076] Furthermore, in step 5, the method of combining experiment and numerical simulation includes:

[0077] Step 5.1, integrating and calculating the loading speeds of the first incident rod 2 and the second incident rod 3, obtaining the displacement curves of the ends of the first incident rod 2 and the second incident rod 3 over time, and also determining the crack initiation time of the adhesive layer crack according to the fracture strain gauge 11 and the high-speed camera 6;

[0078] The expression of the displacement curve of the first incident rod 2 over time is:

[0079]

[0080] The expression of the displacement curve of the second incident rod 3 over time is:

[0081]

[0082] Where C0 is the elastic wave velocity of the incident rod, ε 1,inc (t) and ε 2,inc (t) are the incident waves of the first incident rod 2 and the second incident rod 3, ε 1,ref (t) and ε 2,ref (t) are the reflected waves of the first incident rod 2 and the second incident rod 3, respectively;

[0083] Step 5.2: Figure 4 As shown, a simulation model of a dual-material specimen 1 is established in the finite element software, and the displacement curves of the ends of the first incident rod 2 and the second incident rod 3 over time are used as boundary conditions of the simulation model to perform displacement loading on the simulation model;

[0084] Step 5.3: Output the relative displacement and nodal force of the crack tip node of the adhesive layer in the numerical simulation results;

[0085] Step 5.4: The relative displacement and node force of the crack tip node of the adhesive layer output in the numerical simulation results are used to calculate the change curve of fracture toughness over time. The dynamic fracture starting time t f CPG and t f HSP Determine the dynamic fracture toughness value of the bonding interface of bi-material specimen 1.

[0086] In the above technical solution, considering the influence of inertia effect on the bi-material specimen 1 under dynamic loading, an experimental-numerical hybrid method is used to more accurately obtain the dynamic fracture toughness of the bi-material specimen 1.

[0087] Furthermore, in step 5.4, the dynamic mode I fracture toughness value of the bonding interface of the bi-material specimen 1 is calculated using the modified virtual crack closure method, and the calculation formula is:

[0088]

[0089] Among them, G Ⅰ is the dynamic mode I fracture toughness value of the bonding interface of bi-material specimen 1; F y1 When the fracture is of mode I, the node force at the crack tip of the adhesive layer, Δv 3,4 is the relative displacement of the crack tip node of the adhesive layer during mode I fracture, b is the width of the bi-material specimen, and Δa is the unit size of the grid for the bi-material specimen simulation model.

[0090] In summary, the experimental method for obtaining dynamic fracture toughness of the bi-material specimen 1 in the present invention is mainly used to test the dynamic fracture toughness of the interface of two different materials (including metal and metal, composite material and composite material, metal and composite material, etc.) that are bonded, solidified or connected in other ways to form a structural member, so as to evaluate the energy that the interface can absorb during the fracture process and its ability to resist fracture propagation. Based on a uniaxial bidirectional electromagnetic Hopkinson rod loading system, a uniaxial bidirectional synchronous loading method can be used to achieve synchronous opening of the bi-material specimen 1. At the same time, the bi-material specimen 1 formed by bi-material bonding is designed based on a bending stiffness matching method to ensure equal bending deformation of the bi-material specimen 1 during loading, thereby obtaining a pure I-type opening, and more accurately calculating the fracture toughness value of the bonding interface of the bi-material specimen 1 by using a combination of experimental and numerical simulation methods.

Claims

1. An experimental method for obtaining dynamic fracture toughness of a bi-material specimen. It is characterized in that include: Step 1, preparing a dual material sample; Step 2: Build a uniaxial bidirectional electromagnetic Hopkinson rod loading system, and fix the bi-material specimen on the uniaxial bidirectional electromagnetic Hopkinson rod loading system; Step 3, starting the uniaxial bidirectional electromagnetic Hopkinson rod loading system to perform bidirectional dynamic synchronous loading on the bi-material specimen; Step 4, the uniaxial bidirectional electromagnetic Hopkinson rod loading system collects the loading speed of the bi-material sample, the displacement change curve of the incident rod in the uniaxial bidirectional electromagnetic Hopkinson rod loading system over time, and the dynamic fracture starting time of the bi-material sample; Step 5: According to the displacement-time curve of the incident rod in the uniaxial bidirectional electromagnetic Hopkinson rod loading system and the dynamic fracture initiation time of the bi-material specimen, the fracture toughness value of the bonding interface of the bi-material specimen is calculated by combining the experimental and numerical simulation methods.

2. The experimental method for obtaining dynamic fracture toughness of a dual-material specimen according to claim 1, It is characterized in that In step 1, the dual-material specimen includes an upper beam plate and a lower beam plate made of different materials and bonded to each other; the upper beam plate and the lower beam plate have the same bending stiffness, that is: E 1 I 1 =E 2 I 2 Among them, E 1 is the bending modulus of the upper beam plate; I 1 is the moment of inertia of the upper beam plate; E 2 is the bending modulus of the lower beam plate; I 2 is the moment of inertia of the lower beam plate; h 1 is the thickness of the upper beam plate; h 2 is the thickness of the lower beam slab.

3. The experimental method for obtaining dynamic fracture toughness of a dual material specimen according to claim 2, It is characterized in that In step 2, the uniaxial bidirectional electromagnetic Hopkinson rod loading system includes a first incident rod, a second incident rod, an oscilloscope, a flash lamp, a high-speed camera and a computer; The first incident rod and the second incident rod are arranged coaxially with a horizontal interval, and one end of the first incident rod and the second incident rod is provided with a stress wave generator, each of the stress wave generators includes a primary coil and a secondary coil; the two stress wave generators are controlled by an electromagnetic control circuit; a strain gauge is provided at the middle position of the circumferential outer wall of the first incident rod and the second incident rod; The bi-material sample is arranged between the first incident rod and the second incident rod, the two outer end surfaces of the bi-material sample are respectively bonded and fixed to one end of the first incident rod and the second incident rod, and a fracture strain gauge is arranged on the side of the bi-material sample; The flash lamp and the high-speed camera are arranged on the side of the double-material sample; the oscilloscope is electrically connected with the fracture strain gauge, the flash lamp, the computer, the high-speed camera and the two strain gauges.

4. The experimental method for obtaining dynamic fracture toughness of a dual material specimen according to claim 1, It is characterized in that In step 3, after the dual-material sample is completed, the voltage value and capacitance value in the electromagnetic control circuit are set according to the requirements of the loading rate of the dual-material sample, and the electromagnetic control circuit is charged to the set value, and the discharge switch is started to discharge the main coil of the stress generator until the capacitor voltage drops to 0V. The secondary coil will generate a loading stress wave under the action of the electromagnetic repulsion force. The stress wave is transmitted to the dual-material sample through the first incident rod and the second incident rod at the same time, and the dual-material sample is subjected to bidirectional dynamic synchronous loading.

5. The experimental method for obtaining dynamic fracture toughness of a dual material specimen according to claim 3, It is characterized in that The calculation formula for the loading speed of the dual material specimen is: V 1 (t)=C 0 (ε 1,inc (t)-(ε 1,ref (t)) V 2 (t)=-C 0 (ε 2,inc (t)-(ε 2,ref (t)) V=V 1 (t)+V 2 (t) Among them, ε is the strain signal, k value is the sensitivity coefficient of the selected strain gauge, U 0 is the Wheatstone bridge voltage, ΔU is the output voltage value of the corresponding acquisition channel over time; C 0 is the elastic wave velocity of the incident rod, ε 1,inc (t) and ε 2,inc (t) are the incident waves of the first incident bar and the second incident bar, ε 1,ref (t) and ε 2,ref (t) are the reflected waves of the first incident rod and the second incident rod respectively; V is the loading speed of the bi-material sample, V 1 (t) and V 2 (t) are the loading speeds of the first incident rod and the second incident rod, respectively; The dynamic fracture initiation time of the bi-material specimen was determined by fracture strain gauge and high-speed camera, and the initiation fracture time was t f CPG and t f HSP .

6. The experimental method for obtaining dynamic fracture toughness of a dual material specimen according to claim 3, It is characterized in that In step 5, the combined experimental-numerical simulation method includes: Step 5.1, integrating and calculating the loading speeds of the first incident rod and the second incident rod, obtaining the displacement curves of the first incident rod and the second incident rod ends over time, and also determining the crack initiation time of the adhesive layer crack according to the fracture strain gauge and the high-speed camera; The expression of the first incident rod displacement versus time curve is: The expression of the second incident rod displacement versus time curve is: Among them, C 0 is the elastic wave velocity of the incident rod, ε 1,inc (t) and ε 2,inc (t) are the incident waves of the first incident bar and the second incident bar, ε 1,ref (t) and ε 2,ref (t) are the reflected waves of the first incident rod and the second incident rod, respectively; Step 5.2, establish a dual-material specimen simulation model in the finite element software, and use the displacement curves of the first incident rod and the second incident rod ends over time as boundary conditions of the simulation model to perform displacement loading on the simulation model; Step 5.3: Output the relative displacement and nodal force of the crack tip node of the adhesive layer in the numerical simulation results; Step 5.4: The relative displacement and node force of the crack tip node of the adhesive layer output in the numerical simulation results are used to calculate the change curve of fracture toughness over time. The dynamic fracture starting time t f CPG and t f HSP Determine the dynamic fracture toughness value of the bonding interface of the bi-material specimen.

7. The experimental method for obtaining dynamic fracture toughness of a dual-material specimen according to claim 6, It is characterized in that In step 5.4, the dynamic mode I fracture toughness value of the bonding interface of the bi-material specimen is calculated using the modified virtual crack closure method. The calculation formula is: Among them, G Ⅰ is the dynamic mode I fracture toughness value of the bonding interface of the bi-material specimen; F y1 When the fracture is of mode I, the node force at the crack tip of the adhesive layer, Δv 3,4 is the relative displacement of the crack tip node of the adhesive layer during mode I fracture; b is the width of the bi-material specimen; Δa is the unit size of the grid for the bi-material specimen simulation model.

Citation Information

Cited By

  • High-temperature uniaxial bidirectional electromagnetic Hopkinson rod experiment system and method

    CN119804182A

  • Method for constructing CFRP laminated material simulation model based on DIC and synchrotron radiation

    CN119864111A