Polypropylene-based insulation material, preparation method thereof and high-voltage direct-current polypropylene insulation cable

By using modified nano-oxides and nucleating agents in polypropylene-based insulation materials, the problems of space charge accumulation and insufficient mechanical strength in high-voltage DC cables have been solved, resulting in improved high breakdown field strength and high temperature resistance, making them suitable for new energy power systems.

CN118978764APending Publication Date: 2024-11-19ZHUHAI POWER SUPPLY BUREAU GUANGDONG POWER GIRD CO +2
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411066272.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When cross-linked polyethylene is used as the insulation material in existing high-voltage DC cables, there are problems such as space charge accumulation, insulation aging, insufficient mechanical strength and poor temperature resistance, which make it difficult to meet the needs of new energy power systems.

Method used

Polypropylene-based insulation material is used. By adding modified nano-oxides and nucleating agents, the charge distribution is regulated, the surface electron transport characteristics are improved, and the crystallization process is promoted. Thermoplastic elastomers are added to improve mechanical properties, and silane coupling agents are used to modify nano-oxides to enhance interfacial compatibility.

Benefits of technology

It effectively suppresses space charge accumulation, improves breakdown field strength, enhances mechanical properties and temperature resistance, is suitable for high-temperature environments, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention relates to the technical field of electric power engineering materials, in particular to a polypropylene-based insulation material, a preparation method thereof and a high-voltage direct-current polypropylene insulation cable. The polypropylene-based insulating material provided by the invention is prepared from the following raw materials in parts by weight: 65 to 85 parts of polypropylene resin, 25 to 50 parts of thermoplastic elastomer, 3 to 6 parts of modified nano oxide, 1 to 2 parts of compatilizer and 0.5 to 5 parts of nucleating agent, wherein the polypropylene resin is isotactic polypropylene, and the isotacticity of the isotactic polypropylene is greater than or equal to 95%; the modified nano oxide is one or more of silane coupling agent modified silicon dioxide, silane coupling agent modified titanium dioxide and silane coupling agent modified aluminum oxide; the silane coupling agent includes at least one unsaturated hydrocarbon group. According to the polypropylene-based insulating material provided by the invention, space charge accumulation can be inhibited, and the breakdown field strength is improved; meanwhile, the high mechanical property and the good temperature resistance are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electric power engineering materials, and in particular to a polypropylene-based insulating material and a preparation method thereof, and a high-voltage cable. Background Art

[0002] Wires and cables are called the "arteries" and "nerves" of the national economy, and their products are widely used in the fields of construction, transportation, power plants, automobiles, petrochemicals, etc. Among them, high-voltage DC cable lines have the advantages of low loss, large transmission capacity, unlimited transmission distance, high operating stability, and the ability to connect to asynchronous power grids. Therefore, they have been widely used in new power systems based on new energy, such as urbanization and large-scale urban agglomeration construction, clean energy grid access, marine economic development and island power supply, and asynchronous power grid interconnection.

[0003] As an important component of high-voltage direct current transmission, the usage and demand of high-voltage direct current cables are increasing year by year. The insulation level of power cables is a key factor in determining the voltage level and operating reliability of cables. At present, cross-linked polyethylene (XLPE) is used as the main insulation of high-voltage direct current cables, and XLPE cables account for more than 95%. However, with the increasing operation time and power demand, the shortcomings of XLPE as the main insulation of cables are gradually becoming apparent. For example, the cross-linking agent used in the production process of XLPE and the by-products produced in the cross-linking process will ionize impurities under high DC voltage, which will aggravate the accumulation of space charge in the cable insulation layer, thereby causing electric field distortion and insulation aging, and even partial discharge and insulation breakdown in severe cases; at the same time, its low softening temperature makes it unsuitable for working at high temperatures, and there is a problem of low mechanical strength. Summary of the invention

[0004] Based on this, the present application provides a polypropylene-based insulating material and a preparation method thereof, and a high-voltage direct current polypropylene insulated cable. The polypropylene-based insulating material provided in the present application can not only inhibit the accumulation of space charges and improve the breakdown field strength, but also has high mechanical properties and good temperature resistance.

[0005] In a first aspect of the present application, a polypropylene-based insulating material is provided, which comprises the following raw materials, measured by weight: 65 to 85 parts of polypropylene resin, 25 to 50 parts of thermoplastic elastomer, 3 to 6 parts of modified nano-oxide, 1 to 2 parts of compatibilizer, and 0.5 to 5 parts of nucleating agent;

[0006] Wherein, the polypropylene resin is isotactic polypropylene, and the isotacticity of the isotactic polypropylene is ≥95%;

[0007] The modified nano oxide is one or more of silane coupling agent modified nano silicon dioxide, silane coupling agent modified nano titanium dioxide and silane coupling agent modified nano aluminum oxide; the silane coupling agent includes at least one unsaturated hydrocarbon group.

[0008] In one embodiment, the silane coupling agent includes one or more of vinyl triethoxysilane, vinyl trimethoxysilane and γ-(methacryloyloxy)propyl trimethoxysilane.

[0009] In one embodiment, the modified nano-oxide comprises the following raw materials, measured in parts by weight: 2.5 to 4.5 parts of oxide and 0.5 to 1.5 parts of silane coupling agent; wherein the oxide comprises nano-silicon dioxide, nano-titanium dioxide and nano-aluminum oxide.

[0010] In one embodiment, the preparation steps of the modified nano oxide include:

[0011] Mixing the oxide with a first solvent to prepare a first solution;

[0012] Mixing the silane coupling agent with a second solvent to prepare a second solution;

[0013] The first solution and the second solution are mixed and heated under an inert atmosphere to prepare the modified nano-oxide;

[0014] Wherein, the first solvent is a benzene solvent; the second solvent is an aliphatic alcohol solvent; and the heating temperature is the boiling point of the first solvent ±10°C.

[0015] In one embodiment, the thermoplastic elastomer includes ethylene-α-olefin copolymer.

[0016] In one embodiment, the compatibilizer includes one or more of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride, and acrylonitrile-butadiene-styrene grafted maleic anhydride.

[0017] In one embodiment, the density of the polypropylene resin is 0.9 g / cm 3 ~0.95g / cm 3 .

[0018] In one embodiment, the particle size of the modified nano-oxide is 40nm~90nm.

[0019] In one embodiment, the nucleating agent includes one or more of an amine nucleating agent and a rare earth nucleating agent.

[0020] In one of the embodiments, the polypropylene-based insulating material further includes 0.5 to 3 parts of an antioxidant by weight.

[0021] In one embodiment, the antioxidant includes one or more of a phosphate antioxidant and a hindered phenol antioxidant.

[0022] In a second aspect of the present application, there is provided a polypropylene-based insulating material according to any one of the embodiments of the first aspect of the present application, comprising the following steps:

[0023] A raw material for preparing the polypropylene-based insulating material according to any one of the embodiments of the first aspect of the present application;

[0024] The polypropylene-based insulating material is prepared by melt-blending the raw materials.

[0025] A third aspect of the present application provides a high-voltage direct current polypropylene insulated cable, comprising the polypropylene-based insulating material described in any one of the embodiments of the first aspect of the present application.

[0026] The present application uses isotactic polypropylene as the polypropylene resin matrix, and adds modified nano oxides and nucleating agents; wherein, the functional groups introduced by the silane coupling agent modified nano oxides can effectively regulate the charge distribution and energy level structure on the surface of titanium dioxide, improve the surface electron transport characteristics, and reduce surface defects; thereby effectively inhibiting the accumulation of space charges and improving the breakdown field strength of polypropylene-based insulating materials. At the same time, the nucleating agent can provide crystallization points for isotactic polypropylene to promote the crystallization process of isotactic polypropylene, make the arrangement of crystals more orderly, increase the temperature resistance of the insulating material, and the breakdown field strength and insulation performance at high temperatures. In addition, the thermoplastic elastomer included in the polypropylene-based insulating material provided by the present application can cooperate with isotactic polypropylene, which can effectively improve the tensile strength and other mechanical properties of the insulating material. Further, the compatibilizer can weaken the secondary bonds such as hydrogen bonds between isotactic polypropylene molecules to increase the mobility between resin molecules, reduce the crystallinity of resin molecules, increase the plasticity of resin molecules, enhance its flexibility, and make it easy to process.

[0027] In summary, the polypropylene-based insulating material provided in the present application not only has high mechanical properties, good heat resistance and insulation properties, but can also effectively inhibit the accumulation of space charges and improve the breakdown field strength of the material. That is, the polypropylene-based insulating material provided in the present application has improved high temperature resistance, mechanical properties and insulation properties. DETAILED DESCRIPTION

[0028] The following is a further complete and clear description of the polypropylene-based insulating material and its preparation method, and the high-voltage direct current polypropylene insulated cable of the present application in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0029] Generally speaking, the distribution of energy bases such as wind power and hydropower is uneven with the distribution of load centers, so it is necessary to develop long-distance, low-loss power transmission channels. Among them, high-voltage DC cable lines have the advantages of low loss, large transmission capacity, unlimited transmission distance, high operating stability, and the ability to connect to asynchronous power grids, and their application is increasingly valued.

[0030] At present, cross-linked polyethylene is used as the main cable insulation in high-voltage DC cables. The cross-linking reaction of polyethylene changes polyethylene from thermoplastic to thermosetting. After the polyethylene insulation expires, it can only be disposed of by incineration, burial, etc., which puts tremendous pressure on environmental protection and makes it difficult to meet the demand for green and low-carbon power equipment in the new era. In addition, the cross-linking agent used in the production process of cross-linked polyethylene and the by-products produced in the cross-linking process are ionized under high DC voltage, which aggravates the accumulation of space charge in the cable insulation layer, thereby causing electric field distortion and insulation aging, and even partial discharge and insulation breakdown in severe cases. At the same time, long submarine cables are required for new energy power generation methods such as offshore wind power generation, but the melting temperature of cross-linked polyethylene is low. Therefore, in the production process of cross-linked polyethylene cables, in order to avoid the "scorch" phenomenon, long cables cannot be produced.

[0031] Compared with cross-linked polyethylene, the cross-linking and degassing steps are omitted in the extrusion process of polypropylene (PP) cables, which greatly shortens the cable production cycle and significantly reduces production energy consumption. After retirement, it can still be thermoformed again, which is more in line with environmental protection concepts and has potential engineering application value. At the same time, the melting temperature of polypropylene can reach above 150°C, which is more than 40% higher than that of polyethylene materials. It can work continuously in an environment of 90°C. It has excellent high temperature resistance and can effectively increase the operating temperature of polypropylene insulation materials. Therefore, how to carry out reasonable material design to provide environmentally friendly, high temperature resistant, and excellent mechanical and temperature resistant polypropylene-based insulation materials has become an important issue that needs to be solved.

[0032] Based on this, the first aspect of the present application provides a polypropylene-based insulating material, which includes the following raw materials, measured by weight: 65 to 85 parts of polypropylene resin, 25 to 50 parts of thermoplastic elastomer, 3 to 6 parts of modified nano oxide, 1 to 2 parts of compatibilizer, and 0.5 to 5 parts of nucleating agent;

[0033] Wherein, the polypropylene resin is isotactic polypropylene, and the isotacticity of the isotactic polypropylene is ≥95%;

[0034] The modified nano oxide is one or more of silane coupling agent modified silicon dioxide, silane coupling agent modified titanium dioxide and silane coupling agent modified aluminum oxide; the silane coupling agent includes at least one unsaturated hydrocarbon group.

[0035] The present application uses isotactic polypropylene as the polypropylene resin matrix, and adds modified nano oxides and nucleating agents; wherein, the functional groups introduced by the silane coupling agent modified nano oxides can effectively regulate the charge distribution and energy level structure on the surface of titanium dioxide, improve the surface electron transport characteristics, and reduce surface defects; thereby effectively inhibiting the accumulation of space charges and improving the breakdown field strength of polypropylene-based insulating materials. At the same time, the nucleating agent can provide crystallization points for isotactic polypropylene to promote the crystallization process of isotactic polypropylene, make the arrangement of crystals more orderly, increase the temperature resistance of the insulating material, and the breakdown field strength and insulation performance at high temperatures. In addition, the thermoplastic elastomer included in the polypropylene-based insulating material provided by the present application can cooperate with isotactic polypropylene, which can effectively improve the tensile strength and other mechanical properties of the insulating material. Further, the compatibilizer can weaken the secondary bonds such as hydrogen bonds between isotactic polypropylene molecules to increase the mobility between resin molecules, reduce the crystallinity of resin molecules, increase the plasticity of resin molecules, enhance its flexibility, and make it easy to process.

[0036] In summary, the polypropylene-based insulating material provided in the present application not only has high mechanical properties, good heat resistance and insulation properties, but can also effectively inhibit the accumulation of space charges and improve the breakdown field strength of the material. That is, the polypropylene-based insulating material provided in the present application has improved high temperature resistance, mechanical properties and insulation properties.

[0037] It can be understood that in the present application, the weight parts of the polypropylene resin can be selected from any value between 65 parts and 85 parts. Specifically, the weight parts of the polypropylene resin include but are not limited to 65 parts, 66 parts, 68 parts, 70 parts, 73 parts, 74 parts, 75 parts, 76 parts, 78 parts, 79 parts, 80 parts, 81 parts, 83 parts or 85 parts.

[0038] In the present application, the weight percentage of the thermoplastic elastomer can be selected from any value between 25 and 50. Specifically, the weight percentage of the thermoplastic elastomer includes but is not limited to 25, 26, 28, 30, 32, 33, 34, 35, 36, 38, 39, 40, 42, 45, 48 or 50 parts.

[0039] In the present application, the weight percentage of the modified nano oxide can be selected from any value between 3 and 6. Specifically, the weight percentage of the modified nano oxide includes but is not limited to 3, 3.1, 3.3, 3.5, 3.8, 3.9, 4, 4.1, 4.2, 4.5, 4.8, 5, 5.1, 5.2, 5.5, 5.8, 5.9 or 6.

[0040] In the present application, the weight percentage of the compatibilizer can be selected from any value between 1 and 2. Specifically, the weight percentage of the compatibilizer includes but is not limited to 1, 1.1, 1.2, 1.3, 1.5, 1.8, 1.9 or 2 parts.

[0041] In the present application, the weight percentage of the nucleating agent can be selected from any value between 0.5 and 5. Specifically, the weight percentage of the nucleating agent includes but is not limited to 0.5, 0.6, 0.8, 0.9, 1, 1.1, 1.2, 1.5, 1.8, 2, 2.1, 2.2, 2.5, 3, 3.5, 4, 4.5 or 5 parts.

[0042] In one example, the silane coupling agent includes vinyl triethoxysilane , Vinyltrimethoxysilane and γ-(methacryloyloxy)propyltrimethoxysilane One or more of .

[0043] The above-mentioned silane coupling agent contains an unsaturated hydrocarbon group, and the breaking of the carbon-carbon double bond enables the silane coupling agent to be grafted onto oxides such as silicon dioxide, titanium dioxide and aluminum oxide; in addition, the above-mentioned silane coupling agent has an organic group and an inorganic silicon group, which enables them to establish good interface compatibility between the organic resin matrix and the inorganic oxide, thereby improving the performance of the polypropylene-based insulating material.

[0044] In one example, the modified nano oxide includes the following raw materials, measured in parts by weight: 2.5 to 4.5 parts of oxide and 0.5 to 1.5 parts of silane coupling agent; wherein the oxide includes silicon dioxide, titanium dioxide and aluminum oxide.

[0045] It is understandable that in the present application, the weight parts of the oxide can be selected from any value between 2.5 parts and 4.5 parts. Specifically, the weight parts of the oxide include but are not limited to 2.5 parts, 2.7 parts, 2.9 parts, 3 parts, 3.1 parts, 3.3 parts, 3.5 parts, 3.8 parts, 4 parts, 4.2 parts, 4.3 parts, 4.4 parts or 4.5 parts.

[0046] It is understandable that in the present application, the weight percentage of the silane coupling agent can be selected from any value between 0.5 and 1.5. Specifically, the weight percentage of the silane coupling agent includes but is not limited to 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.2, 1.4 or 1.5 parts.

[0047] In one example, the particle size of the modified nano oxide is 40nm~90nm. It is understandable that the particle size of the modified nano oxide can be selected from any value between 40nm~90nm. Specifically, the particle size of the modified nano oxide includes but is not limited to 40nm, 45nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75nm, 80 nm, 85 nm or 90nm. The modified nano oxide of the above particle size can be uniformly dispersed in the polypropylene resin matrix to enhance the mechanical properties of the polypropylene-based insulating material.

[0048] In one example, the steps of preparing the modified nano oxide include:

[0049] Mixing the oxide with a first solvent to prepare a first solution;

[0050] Mixing the silane coupling agent with a second solvent to prepare a second solution;

[0051] The first solution and the second solution are mixed and heated under an inert atmosphere to prepare the modified nano-oxide;

[0052] Wherein, the first solvent is a benzene solvent; and the heating temperature is the boiling point of the first solvent ±10°C.

[0053] In one example, the first solvent is toluene. Toluene can help the functional groups in the silane coupling agent bind to the oxide nanoparticles. The first solvent is anhydrous ethanol. Alcohols can help the silane coupling agent to be better dispersed and contact the nanoparticles.

[0054] In one example, the second solvent is anhydrous ethanol.

[0055] In one example, the heating temperature is 100°C~120°C.

[0056] In one specific example, the preparation steps of the modified nano oxide include:

[0057] Mixing the oxide with toluene to prepare a first solution;

[0058] Mixing the silane coupling agent with anhydrous ethanol to prepare a second solution;

[0059] The first solution and the second solution are mixed and heated under an inert atmosphere to prepare the modified nano-oxide.

[0060] In one example, in the first solution, the mass concentration of the oxide is 0.25 g / mL to 0.4 g / mL. Specifically, in the first solution, the mass concentration of the oxide includes but is not limited to 0.25 g / mL, 0.28 g / mL, 0.3 g / mL, 0.32 g / mL, 0.33 g / mL, 0.34 g / mL, 0.35 g / mL, 0.38 g / mL or 0.4 g / mL.

[0061] In one example, in the second solution, the mass concentration of the silane coupling agent is 0.05 g / mL to 0.15 g / mL. Specifically, in the second solution, the mass concentration of the silane coupling agent includes but is not limited to 0.05 g / mL, 0.08 g / mL, 0.09 g / mL, 0.1 g / mL, 0.11 g / mL, 0.13 g / mL, 0.14 g / mL or 0.15 g / mL.

[0062] In one example, the thermoplastic elastomer includes ethylene-α-olefin copolymer. The thermoplastic elastomer has excellent elasticity and flexibility, and when combined with the isotactic polypropylene resin matrix, it can increase the tensile properties and impact resistance of the polypropylene-based insulation material, thereby improving the durability and reliability of the material.

[0063] The addition of a compatibilizer plays an important role in improving the compatibility between raw materials such as polypropylene resin and thermoplastic elastomer. In one example, the compatibilizer includes one or more of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride and acrylonitrile-butadiene-styrene grafted maleic anhydride.

[0064] In one example, the density of the polypropylene resin is 0.9 g / cm 3 ~0.95g / cm 3 Specifically, the density of polypropylene resin includes but is not limited to 0.9 g / cm 3 , 0.92 g / cm 3 , 0.93 g / cm 3 , 0.94 g / cm 3 or 0.95 g / cm 3 The polypropylene resin selected within this density range has a low density, which is beneficial to reducing the weight of the polypropylene insulation material. At the same time, it has good insulation properties, can effectively block current conduction, and provide excellent electrical insulation properties.

[0065] Nucleating agents play an important role in promoting the specific crystallization process of polypropylene resin, guiding the molecular arrangement to form a more uniform and stable crystal structure, and improving the mechanical properties and heat resistance of polypropylene-based insulation materials. In one example, the nucleating agent includes one or more of an amine nucleating agent and a rare earth nucleating agent. For example, the nucleating agent includes but is not limited to dicyclohexyl p-phenylenediamine DCTH, TMB-5 or a rare earth nucleating agent WBG.

[0066] In one example, the polypropylene-based insulating material further includes 0.5 to 3 parts of an antioxidant by weight. The antioxidant can effectively inhibit the oxidative degradation reaction of the polypropylene-based insulating material under high temperature, oxygen, ultraviolet light and other environments, extend the service life of the insulating material, and improve the stability and durability of the product. Specifically, the weight percentage of the antioxidant includes but is not limited to 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, 2.1 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts or 3 parts.

[0067] In one example, the antioxidant includes one or more of a phosphate antioxidant and a hindered phenol antioxidant. For example, the antioxidant includes but is not limited to antioxidant DLTP, antioxidant TPP or antioxidant 164.

[0068] In a second aspect of the present application, there is provided a polypropylene-based insulating material as described in any example of the first aspect of the present application, comprising the following steps:

[0069] A raw material for preparing a polypropylene-based insulating material according to any example of the first aspect of the present application;

[0070] The polypropylene-based insulating material is prepared by melt-blending the raw materials.

[0071] In one example, the process parameters of the melt blending process include: a mixing temperature of 170°C to 220°C. It can be understood that the mixing temperature includes but is not limited to: 170°C, 174°C, 175°C, 180°C, 184°C, 185°C, 188°C, 189°C, 190°C, 191°C, 194°C, 195°C, 196°C, 197°C, 198°C, 200°C, 205°C, 208°C, 210°C, 211°C, 212, 215°C, 218°C or 220°C.

[0072] In one example, the process parameters of the melt blending process include: mixing time is 10min~30n.

[0073] In one example, the process parameters of the melt blending process include: a mixing speed of 1200 r / min to 1400 r / min. The mixing speed includes but is not limited to: 1200 r / min, 1250 r / min, 1300 r / min, 1350 r / min, 1380 r / min or 1400 r / min.

[0074] In one example, the process parameters of the melt blending process include: the mixing method is internal mixing or extrusion.

[0075] In one specific example, the polypropylene-based insulating material comprises the following steps:

[0076] a1. Weigh all raw materials according to their weight; mix polypropylene resin, thermoplastic elastomer, antioxidant and compatibilizer at 170°C-220°C, extrude and pelletize; then add modified nano oxide and nucleating agent, mix at 170°C-220°C for 10min-30min to obtain a mixed material;

[0077] (2) Extruding the mixture into granules at an extrusion temperature of 170° C. to 220° C. and an extrusion speed of 1200 r / min to 1400 r / min to obtain a polypropylene-based composite material.

[0078] A third aspect of the present application provides a high-voltage direct current polypropylene insulated cable, comprising the polypropylene-based insulating material described in any example of the first aspect of the present application.

[0079] The following further specific examples are provided to explain the present application in detail. It should also be understood that the following examples are only used to further explain the present application and cannot be understood as limiting the scope of protection of the present application. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present application belong to the scope of protection of the present application. The specific process parameters of the following embodiments are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not necessarily limited to the specific values ​​of the embodiments below.

[0080] [Silane coupling agent]

[0081] Vinyl triethoxysilane: purchased from Guangzhou Zhongjie Chemical Technology Co., Ltd.

[0082] Vinyltrimethoxysilane: purchased from Guangzhou Zhongjie Chemical Technology Co., Ltd.

[0083] γ-(Methacryloyloxy)propyltrimethoxysilane: purchased from Guangzhou Zhongjie Chemical Technology Co., Ltd.;

[0084] [Thermoplastic elastomer]

[0085] POE: purchased from Dow;

[0086] [Antioxidant]

[0087] DLTP: purchased from Panhua Chemical Co., Ltd.

[0088] TPP: purchased from: Panhua Chemical Co., Ltd.;

[0089] Antioxidant 164: purchased from Panhua Chemical Co., Ltd.

[0090] [Compatibilizer]

[0091] Polypropylene grafted with maleic anhydride: purchased from: Dongguan Dinghai Plastic Chemical Co., Ltd.;

[0092] Polyethylene grafted maleic anhydride: purchased from: Dongguan Dinghai Plastic Chemical Co., Ltd.;

[0093] Acrylonitrile-butadiene-styrene grafted maleic anhydride: purchased from: Dongguan Dinghai Plastic Chemical Co., Ltd.;

[0094] [Nucleating agent]

[0095] Dicyclohexyl-p-phenylenediamine DCTH: purchased from Guangdong Weilinna New Materials Technology Co., Ltd.;

[0096] TMB-52: purchased from Guangdong Weilinna New Materials Technology Co., Ltd.;

[0097] Rare earth nucleating agent WBG: purchased from Guangdong Weilinna New Materials Technology Co., Ltd.

[0098] Preparation Example 1

[0099] (1) Dispersing 5 g of nano-silicon dioxide in 150 ml of toluene and stirring for 30 min using ultrasonic mechanical stirring to prepare a first solution;

[0100] (2) dissolving 2 g of a silane coupling agent (vinyl triethoxysilane) in 20 ml of anhydrous ethanol to prepare a second solution;

[0101] (3) Add the second solution into the flask and mix with the first solution, pass nitrogen and cooling water, heat to the reflux temperature of toluene, 140°C, and maintain for 2 hours;

[0102] (4) Cooling to room temperature, centrifuging, drying, extracting for 12 hours, and drying to obtain modified nano-silica.

[0103] Preparation Example 2

[0104] (1) Dispersing 5 g of nano-titanium dioxide in 150 ml of toluene and stirring for 30 min using ultrasonic mechanical stirring to prepare a first solution;

[0105] (2) dissolving 1.8 g of a silane coupling agent (vinyl trimethoxy silane) in 20 ml of anhydrous ethanol to prepare a second solution;

[0106] (3) Add the second solution into the flask and mix with the first solution, pass nitrogen and cooling water, heat to the toluene reflux temperature of 140°C, and maintain for 2 hours;

[0107] (4) Cooling to room temperature, centrifuging, drying, extracting for 12 hours, and drying to obtain modified nano-titanium dioxide.

[0108] Preparation Example 3

[0109] (1) Dispersing 5 g of nano-alumina in 150 ml of toluene and stirring for 30 min using ultrasonic mechanical stirring to prepare a first solution;

[0110] (2) dissolving 2 g of a silane coupling agent (γ-(methacryloyloxy)propyltrimethoxysilane) in 20 ml of anhydrous ethanol to prepare a second solution;

[0111] (3) Add the second solution into the flask and mix with the first solution, pass nitrogen and cooling water, heat to the toluene reflux temperature of 145°C, and maintain for 2 hours;

[0112] (4) Cooling to room temperature, centrifuging, drying, extracting for 12 hours, and drying to obtain modified nano-alumina.

[0113] Example 1

[0114] (1) Weigh each raw material according to its weight; 65 parts of density 0.93-0.95g / cm 3 40 parts of polypropylene resin (isotacticity ≥ 95%), 40 parts of thermoplastic elastomer POE, 1 part of antioxidant DLTP, and 1 part of compatibilizer polypropylene grafted maleic anhydride are put into a twin-screw, mixed evenly at 175°C, and then extruded and pelletized; then 5 parts of modified nano-silicon dioxide with a particle size range of 40 nm (prepared in Preparation Example 1) and 2 parts of nucleating agent dicyclohexyl-p-phenylenediamine (DCTH) are added, and mixed in an internal mixer at 195°C for 15 minutes to obtain a mixed material;

[0115] (2) The obtained mixture is extruded and granulated by a twin-screw extruder at an extrusion temperature of 220° C. and an extrusion speed of 1200 r / min to obtain a polypropylene-based high-voltage direct current polypropylene insulated cable material.

[0116] Example 2

[0117] (1) Weigh each raw material according to the weight; 75 parts of density 0.93-0.95g / cm 325 parts of thermoplastic elastomer POE, 0.5 parts of antioxidant TPP, and 2 parts of compatibilizer polyethylene grafted maleic anhydride are put into a twin-screw, mixed evenly at 210°C, and then extruded and pelletized; 4 parts of modified nano titanium dioxide with a particle size range of 75nm (prepared in Preparation Example 2) and 0.5 parts of nucleating agent TMB-52 are added, and mixed in an internal mixer at 185°C for 15 minutes to obtain a mixed material;

[0118] (2) The obtained mixture is extruded and granulated by a twin-screw extruder at an extrusion temperature of 210° C. and an extrusion speed of 1350 r / min to obtain a polypropylene-based high-voltage direct current polypropylene insulated cable material.

[0119] Example 3

[0120] (1) Weigh each raw material according to its weight; 80 parts of density 0.9-0.94g / cm 3 30 parts of thermoplastic elastomer POE, 3 parts of antioxidant 164, and 1 part of compatibilizer acrylonitrile-butadiene-styrene grafted maleic anhydride are put into a twin-screw, mixed evenly at 185°C, and then extruded and pelletized; 6 parts of modified nano-alumina with a particle size range of 80nm (prepared in Preparation Example 3) and 1 part of rare earth nucleating agent WBG are added, and mixed in an internal mixer at 195°C for 15 minutes to obtain a mixed material;

[0121] (2) The obtained mixture is extruded and granulated by a twin-screw extruder at an extrusion temperature of 195° C. and an extrusion speed of 1400 r / min to obtain a polypropylene-based high-voltage direct current polypropylene insulated cable material.

[0122] The tensile properties, electrical properties, and heat resistance of the polypropylene-based high-voltage direct current prepared in the examples and comparative examples were tested. The corresponding test methods or test standards are specifically as follows:

[0123] (1) Tensile properties: The elongation at break is tested based on GB / T1040.1-2018;

[0124] (2) Electrical performance: The breakdown field strength is tested based on GB / T19264.2-2013;

[0125] (3) Heat resistance: To evaluate whether the insulating material can maintain the necessary mechanical strength under the expected overload temperature, prepare the sample according to the tensile performance test method. Use the standard test method of thermal elongation test. Hang one end of the sample in an oven, set the oven temperature to 150°C, and add a weight at the other end that converts the mass of the sample to a tensile force of 0.2MPa according to the cross section of the sample. After a set time of 15 minutes, measure the elongation at break of the sample.

[0126] (4) Conductivity: Based on ASTM D257, a conductivity current test was performed on a sample with a thickness of 0.2 mm. The test time was 1800 s. The steady-state value of the current was obtained and the conductivity was calculated. The test results are shown in Table 1.

[0127] Table 1

[0128]

[0129] As can be seen from Table 1, the polypropylene-based high-voltage DC polypropylene insulated cable material prepared in this application has a tensile strength of not less than 36 MPa, an elongation at break of not less than 590%, a breakdown field strength of not less than 354 kV / mm, and an electrical conductivity of 7.13×10 -16 That is, the polypropylene high-voltage direct current polypropylene insulated cable material prepared in the present application not only has high mechanical properties and good temperature resistance, but also can effectively inhibit the accumulation of space charges and improve the breakdown field strength of the material.

[0130] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0131] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A polypropylene-based insulating material, It is characterized in that The raw materials include, by weight: 65 to 85 parts of polypropylene resin, 25 to 50 parts of thermoplastic elastomer, 3 to 6 parts of modified nano oxide, 1 to 2 parts of compatibilizer, and 0.5 to 5 parts of nucleating agent; Wherein, the polypropylene resin is isotactic polypropylene, and the isotacticity of the isotactic polypropylene is ≥95%; The modified nano oxide is one or more of silane coupling agent modified nano silicon dioxide, silane coupling agent modified nano titanium dioxide and silane coupling agent modified nano aluminum oxide; the silane coupling agent includes at least one unsaturated hydrocarbon group.

2. The polypropylene-based insulating material according to claim 1, It is characterized in that The silane coupling agent includes one or more of vinyl triethoxysilane, vinyl trimethoxysilane and γ-(methacryloyloxy)propyl trimethoxysilane.

3. The polypropylene-based insulating material according to claim 1, It is characterized in that In parts by weight, the modified nano oxide comprises the following raw materials: 2.5 to 4.5 parts of oxide and 0.5 to 1.5 parts of the silane coupling agent; wherein the oxide comprises nano silicon dioxide, nano titanium dioxide and nano aluminum oxide.

4. The polypropylene-based insulating material according to claim 3, It is characterized in that The preparation steps of the modified nano oxide include: Mixing the oxide with a first solvent to prepare a first solution; Mixing the silane coupling agent with a second solvent to prepare a second solution; The first solution and the second solution are mixed and heated under an inert atmosphere to prepare the modified nano-oxide; Wherein, the first solvent is a benzene solvent; the second solvent is an aliphatic alcohol solvent; and the heating temperature is the boiling point of the first solvent ±10°C.

5. The polypropylene-based insulating material according to any one of claims 1 to 4, It is characterized in that The thermoplastic elastomer includes an ethylene-α-olefin copolymer.

6. The polypropylene-based insulating material according to any one of claims 1 to 4, It is characterized in that The compatibilizer includes one or more of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride and acrylonitrile-butadiene-styrene grafted maleic anhydride.

7. The polypropylene-based insulating material according to any one of claims 1 to 4, It is characterized in that The polypropylene-based insulation material has one or more of the following characteristics: (1) The density of the polypropylene resin is 0.9 g / cm 3 ~0.95g / cm 3 ; (2) The particle size of the modified nano-oxide is 40nm~90nm; (3) The nucleating agent includes one or more of an amine nucleating agent and a rare earth nucleating agent.

8. The polypropylene-based insulating material according to any one of claims 1 to 4, It is characterized in that The polypropylene-based insulating material further comprises 0.5 to 3 parts of an antioxidant in parts by weight; Optionally, the antioxidant includes one or more of a phosphate antioxidant and a hindered phenol antioxidant.

9. A polypropylene-based insulating material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: The raw material for preparing the polypropylene-based insulating material according to any one of claims 1 to 8; The polypropylene-based insulating material is prepared by melt-blending the raw materials.

10. A high voltage direct current polypropylene insulated cable, It is characterized in that The invention comprises the polypropylene-based insulating material as described in any one of claims 1 to 8.

Citation Information

Cited By

  • High-voltage direct-current cable insulating material as well as preparation method and application thereof

    CN119529422A

  • Heavy-current copper core conductor polypropylene insulation medium-voltage power cable

    CN120932967A