Explosive welding structure of super-large-area titanium-steel composite plate and welding process of explosive welding structure

By using low-explosion speed explosives and combined explosive layers in the explosion welding of super-large area titanium-steel composite panels, combined with V-shaped gaps and insulation, the problems of poor exhaust and excessive corrugation in traditional processes are solved, and high quality is achieved welding effect and efficient production.

CN118989549APending Publication Date: 2024-11-22NANJING BAOTAI SPECIAL MATERIALS CO LTD +1
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411424229.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the explosive welding of ultra-large area titanium-steel composite panels, the traditional high-explosion speed process leads to poor exhaust gas, excessive corrugation on the bonding surface, and unevenness, affecting welding quality and production efficiency.

Method used

Low-explosion speed explosives are used and combined with explosive layers and detonation columns through design, combining V-shaped gaps and insulation parts, and optimized welding processes to reduce explosive burst speed, improve exhaust time and bonding surface flatness.

Benefits of technology

It significantly improves the welding quality and flatness of the bonding surface of the titanium-steel composite panel, reduces welding defects, meets industry standards, and improves production efficiency and finished product qualification rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989549A_ABST
    Figure CN118989549A_ABST
Patent Text Reader

Abstract

The invention is suitable for the technical field of production of metal composite plates, and particularly relates to an explosive welding structure of an ultra-large-area titanium-steel composite plate and a welding process of the explosive welding structure, the explosive welding structure comprises a steel base plate, a plurality of supporting blocks are arranged on the surface of the steel base plate, and one ends of the supporting blocks are jointly connected with a titanium composite plate. According to the method, the explosive with the low detonation velocity is creatively used as an energy source, the detonation velocity of the explosive is further reduced to about 1600 m / s at the welding end, and the exhaust time between metal plates in the explosion process is effectively prolonged, so that the amplitude of corrugations on the bonding surface is reduced, and a smoother interface waveform with small corrugations is obtained. According to the optimized design, when the titanium-steel composite plate is produced, the quality of a product and the flatness of a joint surface can be remarkably improved, the welding defect caused by unsmooth exhaust or overlarge corrugation in a traditional process is avoided, and especially in the welding process of the titanium-steel composite plate with an ultra-large area specification, the welding quality of the titanium-steel composite plate is greatly improved. And challenges caused by a large-area joint surface can be effectively handled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal composite plate production, in particular to an explosion welding structure of an ultra-large area titanium-steel composite plate and a welding process thereof. Background Art

[0002] The titanium-steel composite plate explosion welding technology is a processing method that combines different metal materials together through the high-energy impact force generated by the explosion. It is widely used in the fields of chemical industry, metallurgy, and electricity. This technology uses the huge energy generated by the explosion to cause a high-energy collision between the titanium plate and the steel substrate in a very short time, and forms a tight metallurgical bond with the help of the jet effect and interatomic force between the metal surfaces. Titanium-steel composite plates have the excellent corrosion resistance of titanium materials and the strength and cost advantages of steel, so they are widely used in the manufacture of large equipment such as high-pressure vessels and reactors. However, due to the large differences in the physical and chemical properties of titanium and steel, during the explosion welding process, problems such as poor exhaust, large ripples on the bonding surface, and poor fit of the composite plates are often encountered, resulting in unstable welding quality.

[0003] At present, the traditional explosion welding process of ultra-large-area titanium-steel composite plates usually uses explosives with higher detonation speed to ensure sufficient impact energy to achieve metallurgical bonding of the two metal materials. However, this high detonation speed process will cause a series of problems in the welding process of ultra-large-area titanium-steel composite plates. First, the exhaust time is short during welding, and the amplitude of the bonding surface corrugation is too large, resulting in uneven interface waveforms, especially on large-area joint surfaces. The unevenness of the waveform will be more obvious, affecting the overall bonding quality. In addition, high detonation speed may bring excessive impact force, causing deformation or even material damage to the titanium composite plate or steel substrate, thereby affecting the bonding strength and durability of the composite plate.

[0004] For ultra-large titanium-steel composite plates, the problem of poor exhaust is more prominent due to their large area, which easily leads to defects such as pores and cracks on the joint surface. These defects will directly affect the product's fit rate and welding quality, resulting in low production efficiency and high rework rate. Therefore, in the process of explosive welding of ultra-large titanium-steel composite plates, how to optimize the welding process, reduce the explosion speed, and improve the exhaust effect has become the key to improving welding quality and efficiency. Summary of the invention

[0005] The purpose of the embodiments of the present invention is to provide an explosion welding structure of an ultra-large area titanium-steel composite plate and a welding process thereof, aiming to solve the technical problems mentioned in the background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] An explosive welding structure of an ultra-large area titanium-steel composite plate, comprising a steel base plate, a plurality of support blocks are arranged on the surface of the steel base plate, and one end of the plurality of support blocks is commonly connected to a titanium composite plate, a protective layer is arranged on the surface of the titanium composite plate, a combined explosive layer is laid on the surface of the protective layer, an explosive column is arranged in the central area of ​​the combined explosive layer, and a detonator is arranged inside the explosive column;

[0008] The combined explosive layer includes a first explosive layer and a second explosive layer, and the first explosive layer and the second explosive layer are both laid on the surface of the protective layer, the first explosive layer is cylindrical, and the axis of the first explosive layer is in the same straight line with the center of the titanium composite plate, the second explosive layer surrounds the first explosive layer, and the second explosive layer completely covers the surface of the protective layer.

[0009] Furthermore, the first explosive layer has a detonation velocity of 1810-1830 M / s, a strength of 7 mm, and a density of 0.94 g / cm 3 , milk powder accounts for 46.5%, the second explosive layer has a detonation velocity of 1600-1630M / s, a strength of 6mm, and a density of 1.40g / cm 3 , milk powder accounts for 36%;

[0010] The explosive dosage of the first explosive layer and the second explosive layer is 17.5 kg / m 2 and 15kg / m 2 .

[0011] Furthermore, the gap between the titanium composite plate and the steel base plate is V-shaped.

[0012] Furthermore, the surfaces of the titanium composite plate and the steel base plate are both provided with heat insulation components.

[0013] An explosive welding process for ultra-large area titanium-steel composite plates comprises the following steps:

[0014] S1: Select an area with solid and flat soil, evenly spread a layer of fine sand with a preset thickness, and level it as the ground foundation 7;

[0015] S2: Prepare the titanium composite plate and the steel substrate, fully remove the weld on the surface of the titanium composite plate, trim the edges of the steel substrate using an oxyacetylene flame, and grind the surfaces to be bonded of the titanium composite plate and the steel substrate;

[0016] S3: Preheat the titanium composite plate and the steel base plate, and attach thermal insulation components to the surfaces of the titanium composite plate and the steel base plate;

[0017] S4: Place the steel base plate on the ground foundation, clean up the excess yellow sand around the ground foundation, and then place several support blocks on the surface of the steel base plate in order, and place the titanium composite plate stably on the several support blocks;

[0018] S5: laying a protective layer on the surface of the titanium composite plate, laying a first preset explosive in a designated area with a radius of a preset distance and a center point of the protective layer as the center point of a circle, and laying a second preset explosive in other areas of the surface of the protective layer except the designated area, so as to form a combined explosive layer;

[0019] S6: setting a detonation point in the central area of ​​the combined explosive layer, arranging a detonating charge column inside the detonation point, and setting a detonator inside the detonating charge column;

[0020] S7: Clean the heat-insulating parts from the surface of the titanium composite plate and the steel base plate, detonate the detonator and detonate the combined explosive layer.

[0021] Furthermore, the preset thickness is 50 mm.

[0022] Furthermore, in step S2, a 40-mesh flap wheel is used to grind and polish the surface to be bonded of the titanium composite plate, and a 40-mesh sand belt is used to grind and polish the surface to be bonded of the steel substrate.

[0023] Furthermore, in step S3, when the titanium composite plate and the steel substrate are preheated, the preheating temperature is not less than 350°C, the preheating time is not less than 30 minutes, and step S7 should be performed within 1.5 hours after the preheating treatment.

[0024] Furthermore, the first preset explosive has a detonation velocity of 1810-1830 M / s, a strength of 7 mm, and a density of 0.94 g / cm 3 , milk powder accounts for 46.5%, the height of the medicine is 40mm, and the dosage is 17.5kg / m 2 ;

[0025] The second preset explosive has a detonation velocity of 1600-1630 M / s, a strength of 6 mm, and a density of 1.40 g / cm 3 , milk powder accounts for 36%, the height of the medicine is 40mm, and the dosage is 15kg / m 2 .

[0026] Furthermore, the density of the explosive column is 0.72 g / cm 3 , it is made of powdered emulsion explosive with a detonation velocity of 3750m / s, and the diameter of the explosive column is 25mm and the height is 40mm.

[0027] The explosive welding structure of a super-large area titanium-steel composite plate and the welding process thereof provided by the present invention have the following beneficial effects:

[0028] The present invention innovatively uses low-detonation-velocity explosives as energy, and further reduces the explosive detonation velocity to about 1600m / s at the welding end, effectively increasing the exhaust time between the metal plates during the explosion process, thereby reducing the amplitude of the ripples on the joint surface, and obtaining a smoother interface waveform with smaller ripples. This optimized design can significantly improve the quality of the product and the flatness of the joint surface when producing titanium-steel composite plates, avoiding welding defects caused by poor exhaust or excessive ripples in traditional processes, especially in the welding process of ultra-large-area titanium-steel composite plates, and can effectively cope with the challenges brought by large-area joint surfaces.

[0029] Compared with the traditional metal composite plate production process, this process uses theoretical analysis and a large number of experimental verifications to finally determine a series of key parameters, especially by using low-detonation-velocity explosives to reduce the non-fitting defects in the production of composite plates. This method not only makes the titanium-steel composite plates produced meet the requirements of the third part of the industry standard NB / T47002-2009 "Explosion-welded Composite Plates for Pressure Vessels", but also achieves a 100% fit rate and a minimum shear strength τb ≥ 195Mpa (the minimum shear strength τb of titanium-steel composite tube sheets is ≥ 140Mpa), ensuring the excellent performance of the composite plates in high-pressure vessels. In addition, the detonator shadow area can be flexibly avoided according to the finished product processing, further improving the finished product qualification rate and processing flexibility.

[0030] The explosive welding process of the present invention greatly reduces the non-fitting phenomenon in the production of composite plates in practical applications, reduces the defective rate and the repair rate, thereby saving a lot of time, manpower and material costs. The process simplifies the operation steps and improves the production efficiency. It is particularly suitable for the production of large-area composite plates and has great industrial application value. It can meet the urgent needs of the domestic composite plate production industry for efficient and stable processes, especially in the explosive welding process of ultra-large-area titanium-steel composite plates. It shows more significant advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a front schematic diagram of an explosively welded structure of an ultra-large area titanium-steel composite plate.

[0032] In the figure: 1. detonator; 2. combined explosive layer; 3. protective layer; 4. titanium composite plate; 5. support block; 6. steel base plate; 7. ground foundation. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0034] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0035] like Figure 1 As shown, an embodiment of the present invention provides an explosive welding structure of an ultra-large area titanium-steel composite plate, including a steel base plate 6, a surface of the steel base plate 6 is provided with a plurality of support blocks 5, and one end of the plurality of support blocks 5 is commonly connected to a titanium composite plate 4, a surface of the titanium composite plate 4 is provided with a protective layer 3, a surface of the protective layer 3 is paved with a combined explosive layer 2, and a detonating column is provided in the central area of ​​the combined explosive layer 2.

[0036] A detonator 1 is arranged inside the explosive column, and the detonator 1 adopts a double electronic detonator series detonation method to ensure the reliability and synchronization of detonation. The series design of the double electronic detonator can effectively improve the accuracy and stability of detonation, reduce the phenomenon of false explosion or delay, and thus ensure the uniform release of energy and the stability of welding quality during the explosion welding of titanium-steel composite plates.

[0037] The combined explosive layer 2 includes a first explosive layer and a second explosive layer, and the first explosive layer and the second explosive layer are both laid on the surface of the protective layer 3. The first explosive layer is cylindrical, and the axis of the first explosive layer is in the same straight line with the center of the titanium composite plate 4. The second explosive layer surrounds the first explosive layer, and the second explosive layer completely covers the surface of the protective layer 3.

[0038] The detonation velocity of the first explosive layer is 1810-1830M / s, the intensity is 7mm, and the density is 0.94g / cm 3 , milk powder accounts for 46.5%, the second explosive layer has a detonation velocity of 1600-1630M / s, a strength of 6mm, and a density of 1.40g / cm 3 , milk powder accounts for 36%;

[0039] The explosive dosage of the first explosive layer and the second explosive layer is 17.5kg / m 2 and 15kg / m 2 .

[0040] In one embodiment of the present invention, the steel substrate 6 used in the present application is a Q235-B steel plate with a size of 42mm×3960mm×12700mm, and the titanium composite plate 4 is a SB265 Gr1 plate with a size of 4mm×4000mm×12750mm. The steel substrate and titanium composite plate of the above specifications are both of the ultra-large area type.

[0041] When performing explosive welding, the worker first detonates the detonator 1 through remote control, and the detonator 1 detonates the explosive column, which then detonates the combined explosive layer. In the process of detonating the combined explosive layer, the first explosive layer in the inner circle is detonated first, and with the explosion of the first explosive layer, the second explosive layer on the periphery is also detonated. In this process, the titanium composite plate 4 is rapidly accelerated by the energy of the explosive explosion. When the movement speed of the titanium composite plate 4 reaches stability, it begins to collide violently with the steel substrate 6.

[0042] During the collision, a high-temperature and high-pressure re-entry flow (jet) is generated at the contact point. This re-entry flow can effectively remove impurities such as oxides, nitrides, gas films, and moisture on the surfaces to be bonded between the titanium composite plate 4 and the steel substrate 6, exposing fresh active metal on the metal surface. While the metal surface is cleaned, due to the huge pressure generated during the collision, the active surfaces of the two metals are forced to come into close contact, and a reliable connection between the titanium composite plate 4 and the steel substrate 6 is achieved through the force between atoms, thereby achieving a high-quality welding effect.

[0043] When the titanium composite plate 4 approaches and collides with the steel base plate 6, the strong airflow caused by the explosion will blow away the support block 5 between the titanium composite plate and the steel base plate, so that the support block 5 will not remain between the two plates, ensuring that the welding surface is clean and free of impurities, thereby ensuring the welding quality.

[0044] In addition, since the detonation velocity, density, intensity and other parameters of the first and second explosive layers have been precisely designed and matched, their graded detonation method ensures that the titanium composite plate is subjected to uniform and appropriate impact force throughout the process, thereby avoiding excessive deformation or damage of the titanium composite plate and further improving the quality and reliability of titanium-steel composite plate welding.

[0045] In this embodiment, the gap between the titanium composite plate 4 and the steel substrate 6 is designed as a V-shaped structure, and its tip is facing the detonation point. This design not only helps to guide the gas generated during the explosion to be discharged quickly, but also significantly reduces the resistance during gas discharge, avoiding welding defects caused by gas retention or poor discharge. At the same time, the V-shaped gap design can ensure that the titanium composite plate moves closer to the steel substrate more smoothly during the explosion acceleration process, reducing unnecessary energy loss, thereby ensuring that the titanium composite plate achieves the best impact force and speed matching when colliding with the steel substrate.

[0046] This structure optimizes the energy transfer between metal plates during explosive welding, improves the uniformity and tightness of the surface bonding between the titanium composite plate and the steel substrate, and effectively avoids unevenness on the welding surface, such as pores or loose welds. In addition, the existence of the V-shaped gap can also provide an additional channel for removing surface impurities and gases, further ensuring the cleanliness of the bonding surface and enhancing the firmness and durability of metal welding.

[0047] In this embodiment, the surfaces of the titanium composite plate 4 and the steel substrate 6 are both provided with insulation. The insulation can be a flexible insulation blanket or a high temperature resistant ceramic fiber cloth made of high temperature insulation material. The insulation is provided to keep the plate in a high temperature state after preheating and reduce temperature fluctuations during welding, thereby ensuring that the metal surface remains active during explosive welding and avoiding a decrease in bonding performance due to a rapid drop in temperature. In addition, the insulation can also effectively reduce the interference of the external environment temperature on the plate, ensuring that the welding process of the titanium composite plate and the steel substrate is more stable and reliable, thereby improving the welding quality and welding strength.

[0048] like Figure 1 As shown, an explosion welding process for a super large area titanium-steel composite plate provided by an embodiment of the present invention comprises the following steps:

[0049] S1: Select an area with solid and flat soil, evenly spread a layer of fine sand of a preset thickness, and level it as the ground foundation7.

[0050] The preset thickness is 50mm. The 50mm fine sand layer can not only provide stable support to ensure the stability of the steel base plate in subsequent operations, but also absorb part of the explosion impact energy to prevent the ground reaction force from affecting the flatness and welding quality of the welding process. This fine sand foundation design optimizes the construction conditions on site and ensures the stability and safety of the composite plate during welding.

[0051] S2: Prepare the titanium composite plate 4 and the steel substrate 6, fully remove the weld on the surface of the titanium composite plate 4, trim the edges of the steel substrate 6 using an oxyacetylene flame, and grind the surfaces to be bonded of the titanium composite plate 4 and the steel substrate 6 to ensure surface finish and bonding effect.

[0052] Titanium composite plate 4 (SB265 Gr1) is welded using the GTAW (gas tungsten arc welding) process. After welding, the weld excess height needs to be removed from both sides to ensure the surface flatness of the weld area. After performance testing, the mechanical properties of the weld should be similar to those of the parent material to ensure that the weld will not become a weak point and affect the overall strength of the composite plate during the subsequent explosion welding process. In order to further ensure the edge quality of the steel base plate 6 (Q235-B steel plate), an oxyacetylene flame is used to trim the edges around it to avoid edge defects such as fracture burrs and misalignment. These defects can easily develop into cracks during the explosion welding process, thereby affecting the welding quality. Therefore, edge trimming can effectively prevent the occurrence of such problems.

[0053] Before the explosion welding, the flatness of the titanium composite plate 4 and the steel substrate 6 is also required to be strictly controlled, and the flatness is required to be within the range of ≤3mm / m and ≤10mm / whole plate, and no sharp bends or obvious local bending are allowed. This flatness requirement ensures that the titanium composite plate can be evenly accelerated during the explosion process, and can achieve a smooth collision with the steel substrate, avoiding local stress concentration or poor welding due to uneven surfaces.

[0054] Through the above settings and strict preliminary treatment, the titanium composite plate and the steel base plate can achieve the best bonding state, ensuring that during the explosion welding process, the bonding surface of the two is clean, flat, and free of stress concentration areas, thereby greatly improving the quality and welding strength of the final composite plate and ensuring the controllability and stability of the process.

[0055] S3: Preheating the titanium composite plate 4 and the steel base plate 6.

[0056] The preheating temperature is not less than 350°C and the duration is not less than 30 minutes to ensure that the metal surface is fully activated. After the preheating treatment is completed, the surface of the titanium composite plate 4 and the steel base plate 6 is immediately attached with a heat-insulating member, which can be a flexible heat-insulating blanket, a high-temperature ceramic fiber cloth or a composite heat-insulating board made of a high-temperature heat-insulating material. Such heat-insulating members can effectively isolate the influence of the external temperature and prevent the metal plate from cooling due to heat dissipation before the explosion welding.

[0057] The function of the heat preservation part is not only to maintain the temperature of the preheated plate, but also to ensure that the metal surface is at the optimal bonding temperature during the explosion welding process, to prevent the metal surface from being passivated or inactive due to temperature drop, thereby affecting the welding quality of the titanium composite plate 4 and the steel base plate 6. By using the heat preservation part, the thermal equilibrium state of the titanium composite plate and the steel base plate before the explosion welding can be effectively guaranteed, providing a more stable temperature environment for the subsequent welding process, reducing welding defects caused by temperature difference stress, and further improving the bonding strength and uniformity between metals.

[0058] S4: Place the steel base plate 6 on the ground foundation 7, clean up the excess yellow sand around the ground foundation 7, and then place a number of support blocks 5 on the surface of the steel base plate 6 in an orderly manner, and stably place the titanium composite plates 4 on the support blocks 5.

[0059] The position and number of support blocks are precisely designed to ensure the stability and uniformity of the support. The gap between the titanium composite plate 4 and the steel substrate 6 is maintained at about 8 mm, and the gap is designed as a V-shaped structure with the tip facing the detonation point. This V-shaped gap design helps to guide the flow of gas generated by the explosion during the explosion process, significantly reducing the resistance during gas discharge and avoiding welding defects caused by gas retention or uneven discharge. In addition, this structural design can also ensure that the titanium composite plate accelerates more smoothly under the action of the explosion energy, achieves uniform and flat contact with the steel substrate 6, and effectively reduces stress concentration and deformation of the metal plate.

[0060] Through reasonable arrangement of support blocks 5 and V-shaped gap design, it is possible to ensure that the titanium composite plate 4 is combined with the steel substrate 6 at an optimal speed and angle when colliding, thereby maximizing the cleanliness and activity of the metal surface, thereby improving the welding strength and welding quality of the titanium-steel composite plate.

[0061] S5: Laying a protective layer 3 on the surface of the titanium composite plate 4, and laying a first preset explosive in a designated area with a radius of a preset distance and a center point of the protective layer 3 as the center point of a circle, and laying a second preset explosive in other areas of the surface of the protective layer 3 except the designated area, so as to form a combined explosive layer.

[0062] On the premise that the steel base plate 6 is a Q235-B steel plate with a specification of 42 mm×3960 mm×12700 mm and the titanium composite plate 4 is a SB265 Gr1 plate with a specification of 4 mm×4000 mm×12750 mm, the preset distance is 3100 mm.

[0063] S6: a detonation point is set in the central area of ​​the combined explosive layer, and an explosive column is arranged inside the detonation point, and a detonator 1 is set inside the explosive column.

[0064] S7: Clean the heat-insulating parts from the surfaces of the titanium composite plate 4 and the steel base plate 6, detonate the detonator 1 and detonate the combined explosive layer.

[0065] The first preset explosive has a detonation velocity of 1810-1830M / s, a strength of 7mm, and a density of 0.94g / cm 3 , milk powder accounts for 46.5%, the height of the medicine is 40mm, and the dosage is 17.5kg / m 2 ;

[0066] The second preset explosive has a detonation velocity of 1600-1630M / s, a strength of 6mm, and a density of 1.40g / cm 3 , milk powder accounts for 36%, the height of the medicine is 40mm, and the dosage is 15kg / m 2 .

[0067] The amount of the first preset explosive and the second preset explosive is significantly lower than that of the conventional stainless steel plate, because the density of the titanium plate is much lower than that of the stainless steel plate. Therefore, using less explosives can provide sufficient impact force for the titanium composite plate to achieve effective welding. In addition, appropriately reducing the amount of explosives can also avoid the generation of excessive shock waves during the explosion process and prevent the formation of adiabatic shear lines. The generation of adiabatic shear lines will cause unevenness in the welding interface, thereby affecting the welding quality, so reducing the amount of explosives helps to achieve a more stable and uniform metal bonding effect.

[0068] In one embodiment of the present invention, an explosion welding process for titanium-steel composite plates is proposed, which combines precise explosion parameter control and plate processing methods to ensure high-quality composite welding effects according to the different characteristics of the titanium composite plate and the steel base plate.

[0069] In this process, first of all, the titanium composite plate (SB265 Gr1) and the steel base plate (Q235-B steel plate) are fully prepared. The titanium composite plate is welded using the GTAW (gas tungsten arc welding) process. After welding, the weld excess height must be removed and the mechanical properties of the weld must be equivalent to those of the parent material to avoid weak points in the subsequent welding process. The steel base plate is trimmed with an oxyacetylene flame to eliminate defects such as burrs or misalignments on the edges to prevent these defects from developing into cracks during explosions.

[0070] The flatness of the joint surface of the titanium composite plate and the steel base plate needs to be strictly controlled, and the flatness is required to be ≤3mm / m and ≤10mm / whole plate to ensure that the plates can be accelerated and collided smoothly and evenly during the explosive welding process to avoid welding defects caused by local stress concentration. The two metal plates are preheated at more than 350℃ for a duration of not less than 30 minutes. The surface of the preheated plates is covered with insulation to ensure that the metal maintains the best activity and temperature before welding to avoid the decline of welding quality due to cooling.

[0071] A V-shaped gap of about 8mm is designed between the titanium composite plate and the steel substrate, with the tip facing the detonation point. The V-shaped structure can not only effectively reduce the resistance during gas discharge, but also guide the airflow discharge during explosion, prevent gas stagnation or uneven discharge, thereby ensuring a tighter bond between the titanium composite plate and the steel substrate.

[0072] The most critical part of this process is the design of explosives. The combined explosive layer consists of a first preset explosive and a second preset explosive. The first preset explosive has a detonation velocity of 1810-1830M / s, a strength of 7mm, and a density of 0.94g / cm 3 Milk powder accounts for 46.5%, the medicine spreading height is 40mm, and the dosage per unit area is 17.5kg / m 2The main function of the explosive layer is to provide the initial impact force, so that the titanium composite plate can be quickly accelerated to a speed suitable for welding, and provide sufficient kinetic energy for welding, while controlling the deformation of the titanium composite plate. Its high detonation speed and high intensity ensure that the titanium composite plate can quickly reach the required collision speed.

[0073] The second preset explosive has a detonation velocity of 1600-1630 M / s, a strength of 6 mm, and a density of 1.40 g / cm 3 Milk powder accounts for 36%, the height of the medicine is 40mm, and the dosage per unit area is 15kg / m 2 Compared with the first explosive layer, the second explosive layer has a lower detonation speed and softer force. It is mainly responsible for balancing and replenishing energy in the process of accelerating the titanium composite plate to approach the steel substrate, ensuring that the titanium composite plate contacts the steel substrate at the optimal speed and pressure during the collision, avoiding damage to the plate caused by excessive impact.

[0074] Through the precise design and control of the two layers of explosives, the first layer of explosives provides sufficient impact force to accelerate the titanium composite plate, while the second layer of explosives is responsible for controlling the release of energy, so that the collision between the titanium composite plate and the steel substrate can produce sufficient bonding force without causing material damage. This staged detonation method can effectively improve the welding quality of titanium-steel composite plates, ensure that the bonding surface is uniform, crack-free, and delaminated, and maximize the welding strength and stability.

[0075] In general, the present invention achieves the best welding effect of titanium-steel composite plates through meticulous preliminary plate processing, efficient preheating and heat preservation measures, and precise explosion energy control, thereby ensuring the performance stability and durability of the composite materials in various complex application environments.

[0076] In this embodiment, a fine grinding and polishing process is used when the surfaces of the titanium composite plate 4 and the steel substrate 6 to be bonded are treated in step S2. Specifically, a 40-mesh flap wheel is used to grind and polish the surfaces of the titanium composite plate 4 to ensure that the surfaces are smooth and free of oxides and other impurities; for the steel substrate 6, a 40-mesh sanding belt is used to grind and polish to ensure that the surfaces of the surfaces to be bonded are also flat and smooth. Through this fine grinding process, the activity and cleanliness of the bonding surfaces are further improved, providing a good foundation for the subsequent explosive welding and ensuring the close bonding and welding quality between the metals.

[0077] In this embodiment, the explosive column uses a density of 0.72g / cm 3 The explosive column is made of powdered emulsion explosive with a detonation velocity of 3750m / s, and has excellent explosion stability and reliability. The diameter of the explosive column is designed to be 25mm and the height is 40mm. These dimensions and material parameters have been precisely calculated to ensure that the explosive column can generate sufficient impact force when detonated, and quickly and evenly detonate the combined explosive layer.

[0078] The design of the explosive column not only provides sufficient explosion energy, but also effectively controls the propagation speed and range of the explosion, ensuring the synchronization and stability of the entire detonation process. This design can avoid excessive or uneven distribution of local energy, thereby ensuring that the titanium composite plate and the steel base plate achieve the best combination effect when they collide, and maximizing the welding strength and quality of the composite plate.

[0079] After the explosive welding operation is completed, the turret should be trimmed to ensure that the overall flatness of the turret is controlled within the range of ≤6mm / whole plate, and no holes or protrusions should appear locally to avoid poor exhaust due to poor foundation flatness, which affects the welding quality. At the same time, a 50mm thick fine sand layer is evenly laid on the ground to provide buffer protection to prevent the welded area from being delaminated due to the tensile wave caused by the hard foundation during the explosive composite process.

[0080] After the explosive composite is completed, after heat treatment and leveling processes, the final composite plate produced meets the relevant requirements of the third part of the industry standard NB / T47002-2009 "Explosion-welded Composite Plates for Pressure Vessels". Except for the detonator shadow area, the composite plate has a 100% fit rate and its minimum shear strength τb is not less than 195MPa (the minimum shear strength τb of titanium-steel composite tube sheet is not less than 140MPa). The detonator shadow area (detonation point) can be avoided according to the processing requirements of the finished product to ensure that the finished product maintains integrity and high strength in key areas.

[0081] In summary, by innovatively applying low-detonation-velocity explosives as energy and further reducing the explosive detonation velocity to about 1600m / s at the welding end, the exhaust time between the metal plates during the explosion process is effectively increased, thereby reducing the amplitude of the ripples on the bonding surface and obtaining a smoother interface waveform with smaller ripples. This optimized design can significantly improve the quality of the product and the flatness of the bonding surface when producing titanium-steel composite plates, and avoid welding defects caused by poor exhaust or excessive ripples in traditional processes.

[0082] Compared with the traditional metal composite plate production process, this process uses theoretical analysis and a large number of experimental verifications to finally determine a series of key parameters, especially by using low-detonation-velocity explosives to reduce the non-fitting defects in the production of composite plates. This method not only makes the titanium-steel composite plates produced meet the requirements of the third part of the industry standard NB / T47002-2009 "Explosion-welded Composite Plates for Pressure Vessels", but also achieves a 100% fit rate and a minimum shear strength τb ≥ 195Mpa (the minimum shear strength τb of titanium-steel composite tube sheets is ≥ 140Mpa), ensuring the excellent performance of the composite plates in high-pressure vessels. In addition, the detonator shadow area can be flexibly avoided according to the finished product processing, further improving the finished product qualification rate and processing flexibility.

[0083] The explosive welding process of the present invention greatly reduces the non-fitting phenomenon in the production of composite panels in practical applications, reduces the defective rate and the repair rate, thereby saving a lot of time, manpower and material costs. The process simplifies the operation steps and improves the production efficiency. It is particularly suitable for the production of large-area composite panels, has great industrial application value, and can meet the urgent needs of the domestic composite panel production industry for efficient and stable processes.

[0084] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An explosion-welded structure of an ultra-large area titanium-steel composite plate, comprising a steel substrate, characterized in that: A plurality of support blocks are arranged on the surface of the steel substrate, and one end of the plurality of support blocks is commonly connected to a titanium composite plate, a protective layer is arranged on the surface of the titanium composite plate, a combined explosive layer is laid on the surface of the protective layer, an explosive column is arranged in the central area of ​​the combined explosive layer, and a detonator is arranged inside the explosive column; The combined explosive layer includes a first explosive layer and a second explosive layer, and the first explosive layer and the second explosive layer are both laid on the surface of the protective layer, the first explosive layer is cylindrical, and the axis of the first explosive layer is in the same straight line with the center of the titanium composite plate, the second explosive layer surrounds the first explosive layer, and the second explosive layer completely covers the surface of the protective layer.

2. The explosion welding structure of an ultra-large area titanium-steel composite plate according to claim 1 is characterized in that: The first explosive layer has a detonation velocity of 1810-1830 M / s, a strength of 7 mm, and a density of 0.94 g / cm 3 , milk powder accounts for 46.5%, the second explosive layer has a detonation velocity of 1600-1630M / s, a strength of 6mm, and a density of 1.40g / cm 3 , milk powder accounts for 36%; The explosive dosage of the first explosive layer and the second explosive layer is 17.5 kg / m 2 and 15kg / m 2 .

3. The explosion welding structure of a super large area titanium-steel composite plate according to claim 1 is characterized in that: The gap between the titanium composite plate and the steel base plate is V-shaped.

4. The explosion welding structure of a super large area titanium-steel composite plate according to claim 1 is characterized in that: The surfaces of the titanium composite plate and the steel base plate are both provided with heat insulation components.

5. An explosive welding process for ultra-large area titanium-steel composite plates, characterized in that: The following steps are involved: S1: Select an area with solid and flat soil, evenly spread a layer of fine sand of preset thickness, and level it as the ground foundation; S2: Prepare the titanium composite plate and the steel substrate, fully remove the weld on the surface of the titanium composite plate, trim the edges of the steel substrate using an oxyacetylene flame, and grind the surfaces to be bonded of the titanium composite plate and the steel substrate; S3: Preheat the titanium composite plate and the steel base plate, and attach thermal insulation components to the surfaces of the titanium composite plate and the steel base plate; S4: Place the steel base plate on the ground foundation, clean up the excess yellow sand around the ground foundation, and then place several support blocks on the surface of the steel base plate in order, and place the titanium composite plate stably on the several support blocks; S5: laying a protective layer on the surface of the titanium composite plate, laying a first preset explosive in a designated area with a radius of a preset distance and a center point of the protective layer as the center point of a circle, and laying a second preset explosive in other areas of the surface of the protective layer except the designated area, so as to form a combined explosive layer; S6: setting a detonation point in the central area of ​​the combined explosive layer, arranging a detonating charge column inside the detonation point, and setting a detonator inside the detonating charge column; S7: Clean the heat-insulating parts from the surface of the titanium composite plate and the steel base plate, detonate the detonator and detonate the combined explosive layer.

6. The explosion welding process of a super large area titanium-steel composite plate according to claim 5 is characterized in that: The preset thickness is 50 mm.

7. The explosion welding process of a super large area titanium-steel composite plate according to claim 5 is characterized in that: In step S2, a 40-mesh flap wheel is used to grind and polish the surface to be bonded of the titanium composite plate, and a 40-mesh sand belt is used to grind and polish the surface to be bonded of the steel substrate.

8. The explosion welding process of a super large area titanium-steel composite plate according to claim 5 is characterized in that: In step S3, when the titanium composite plate and the steel substrate are preheated, the preheating temperature is not less than 350°C, the preheating time is not less than 30 minutes, and step S7 should be performed within 1.5 hours after the preheating treatment.

9. The explosion welding process of a super large area titanium-steel composite plate according to claim 5 is characterized in that: The first preset explosive has a detonation velocity of 1810-1830 M / s, a strength of 7 mm, and a density of 0.94 g / cm 3 , milk powder accounts for 46.5%, the height of the medicine is 40mm, and the dosage is 17.5kg / m 2 ; The second preset explosive has a detonation velocity of 1600-1630 M / s, a strength of 6 mm, and a density of 1.40 g / cm 3 , milk powder accounts for 36%, the height of the medicine is 40mm, and the dosage is 15kg / m 2 .

10. The explosion welding process of ultra-large area titanium-steel composite plate according to claim 5, characterized in that: The density of the explosive column is 0.72 g / cm 3 , it is made of powdered emulsion explosive with a detonation velocity of 3750m / s, and the diameter of the explosive column is 25mm and the height is 40mm.

Citation Information

Cited By

  • Dust-removing and environment-friendly explosive welding method

    CN119489254A

  • Preparation method of medium-entropy alloy and stainless steel explosive welding composite board

    CN119501268A

  • Preparation method of CoCrNi medium-entropy alloy and Q235B steel explosive welding composite board

    CN119501270A

  • Explosive welding method for composite spherical crown lining plate

    CN119681405A

  • Metal composite plate explosive welding device and method for reducing interface defects

    CN119703314A