Composite sodium vanadium phosphate material and preparation method thereof, positive pole piece and secondary battery
Through high-temperature sintering and post-treatment technology, a high-pressure density composite vanadium phosphate material was prepared, and a mutual doping structure was formed using manganese fluorine-manganese doping and anions, which solved the problems of high cost and low cost-effectiveness of vanadium phosphate material, and achieved the Significant improvements in capacity and voltage platforms.
Patent Information
- Application Number
- CN202411188965.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
The high cost and low cost performance of sodium vanadium phosphate materials make it difficult to effectively increase their capacity while controlling costs.
Using vanadium salt, organic acid sodium salt, manganese fluorogenic compounds, phosphate and inorganic carbon sources, high-pressure density composite vanadium phosphate materials are prepared through high-pressure density, and oxygen, phosphate and pyrophosphate are introduced. Roots and fluorine ions form mutual doping structures to increase voltage platform and capacity.
The compaction density and capacity of composite vanadium phosphate material have been significantly improved, the cost performance has been greatly improved, the voltage platform and ionic conductivity have also been improved, and the cost increment is smaller than the capacity increment.
Smart Images

Figure CN118993018A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy materials, specifically to a composite sodium vanadium phosphate material and a preparation method thereof, a positive electrode sheet and a secondary battery. Background Art
[0002] The widespread use of ion batteries around the world has intensified the consumption of lithium resources, and its cost and raw materials will limit its future development. Sodium and lithium have similar physical and chemical properties and are abundant in reserves. According to the principle of lithium-ion "rocking chair" batteries (the charging and discharging process of lithium-ion batteries is the process of lithium ions intercalating and deintercalating between the positive and negative electrodes, which is vividly called "rocking chair batteries"), sodium-rich ion compounds can be similar to lithium-rich positive electrode materials, providing sodium ions and structures that can be intercalated and deintercalated. Sodium ions are larger than lithium ions, and their reversible intercalation reactions require that the material structure has a large sodium-accommodating site and ion migration channels. The polyanion sodium vanadium phosphate Na3V2(PO4)3 belongs to the sodium-ion superconductor (NASICON) material. Its NASICON structural skeleton forms a stable sodium-accommodating site, and the open three-dimensional ion migration channel is conducive to improving the diffusion of sodium ions. It has a high charging and discharging voltage platform, large energy storage capacity, and good cycle stability. It is a very promising sodium-ion battery positive electrode material.
[0003] The common synthesis methods of sodium vanadium phosphate are solid phase method and sol-gel method, and also include spray drying method, hydrothermal method, electrospinning method, etc. However, the biggest problem is that the cost is high, and the capacity is relatively low compared with the cost. In order to improve its cost performance, there are two methods. The first is to reduce its cost, such as using other base metals to replace vanadium; the second is to increase its capacity to improve its cost performance. Summary of the invention
[0004] In view of the technical problems existing in the background technology, the present application provides a composite sodium vanadium phosphate material and its preparation method, a positive electrode plate and a secondary battery, aiming to solve the technical problem that the capacity cannot be effectively increased while controlling the cost during the synthesis process of sodium vanadium phosphate.
[0005] In a first aspect, the present invention provides a method for preparing a composite sodium vanadium phosphate material, comprising the following steps: The vanadium salt, the organic acid sodium salt and water are mixed to obtain a mixed solution, and then the mixed solution is dried and calcined to obtain a carbon-doped sodium vanadium oxide composite; The carbon-doped sodium vanadium oxide composite is mixed with sodium salt, fluorine manganese compound, phosphate, pyrophosphate and inorganic carbon source, and slurried with water, and then ground and dried to obtain a dried material; The dried material is calcined and post-treated to obtain a composite sodium vanadium phosphate material.
[0006] In the technical solution of the embodiment of the present application, vanadium salt, organic acid sodium salt and water are mixed to form a solution, and then a carbon-doped sodium vanadium oxide complex is prepared at high temperature, wherein the organic acid sodium salt provides a sodium source and a carbon source at the same time, and is mixed with the vanadium salt during the calcination process and then calcined. Under high temperature and carbon thermal reduction, vanadium is reduced to a trivalent state, and at the same time, the residual carbon will be compounded on the sodium vanadium oxide complex under high temperature carbonization of the organic acid radical, thereby obtaining a carbon-doped sodium vanadium oxide complex with a high compaction density; further, by introducing sodium salts, phosphates, pyrophosphates, etc., at high temperature, part of the oxides in the carbon-doped sodium vanadium oxide complex are converted into phosphates and pyrophosphates by phosphates and pyrophosphates to obtain composite sodium vanadate and fluorine-manganese-doped sodium vanadium phosphate materials, and at the same time, the carbon obtained by carbonization and decomposition of the organic acid radicals and the newly introduced inorganic carbon source form an organic / inorganic carbon composite as a conductive agent, thereby effectively improving the electronic conductivity of the material.
[0007] The present application introduces four anions, namely oxygen, phosphate, pyrophosphate, and fluoride ions, which can not only improve the voltage platform and capacity, but also form mutual doping, thereby improving its ionic conductivity; at the same time, although the traditional sodium vanadium phosphate has three sodium ions, because one sodium is in the skeleton structure, only two sodiums can be released, making its capacity relatively low, and the mutual doping structure formed by the four anions of the present application can make the third sodium in the sodium vanadium phosphate partially released without affecting its structure. At the same time, due to the doping of manganese and fluoride ions, the voltage platform can also be further improved, among which manganese doping can improve ionic conductivity and voltage platform, fluorine doping can improve voltage platform and ionic conductivity, and compared with other elements, the present application adopts fluorine-manganese doping, which can play a double superposition effect and have a better effect.
[0008] In the present application, a two-step sintering is performed, i.e., a carbon-doped sodium vanadium oxide composite with a high compaction density is first prepared, and then a composite sodium vanadium phosphate material is obtained by conversion of anions. The compaction density of the composite sodium vanadium phosphate material prepared in the present application is 20-50% higher than that of the sodium vanadium phosphate prepared by the traditional preparation process.
[0009] In some embodiments, the vanadium salt comprises one or more of ammonium metavanadate or sodium metavanadate; and / or Sodium salts of organic acids include sodium citrate; and / or The molar ratio of vanadium salt to organic acid sodium salt is (2.9-3.2):1; and / or The concentration of sodium ions in the mixed solution is 3-5 mol / L.
[0010] In this embodiment, vanadium salts are common salts with wide sources and low cost; sodium citrate can introduce sodium, and at the same time, citrate can leave a small amount of carbon, acting as a carbon source. If the molar ratio of vanadium salt to organic acid sodium salt is too large, the sodium content is high, resulting in a high pH of the prepared product, a high carbon content, a high BET, and poor processing performance; if it is too small, sodium is lacking, resulting in a low product capacity. The molar ratio of vanadium salt to organic acid sodium salt is (2.9-3.2):1, which is conducive to obtaining a material with good processing performance, high compaction density and high capacity.
[0011] In some embodiments, in the step of obtaining the carbon-doped sodium vanadium oxide composite by drying and calcining, the calcining process includes: heating the temperature to 800-900° C. at a heating rate of 1-3° C. / min under a nitrogen atmosphere, and keeping the temperature for 4-6 hours.
[0012] In this embodiment, the calcination temperature cannot be too high or too low. If it is too high, the particles of the sodium vanadium oxide complex are too large and the BET is too small, which is not conducive to the subsequent reaction and also affects the electrical properties of the final product. If it is too low, the crystallinity of the sodium vanadium oxide complex is very poor, and even the sodium vanadium oxide complex cannot be obtained by reaction. The time cannot be too long or too short. If the reaction time is too long, the reaction efficiency is low, and it may also cause the crystal particles to be too large, affecting the capacity. If the reaction time is too short, it will cause incomplete crystal growth and low crystallinity, thereby causing low cycle performance of the final product. It can be seen that in this application, the reaction temperature cannot be reduced indefinitely by simply extending the reaction time, and better results can only be achieved within the said range.
[0013] In some embodiments, the sodium salt comprises sodium acetate or sodium bicarbonate; and / or The fluorine manganese compound comprises one or more of manganese difluoride, manganese trifluoride or manganese tetrafluoride; and / or The phosphate includes one or more of monoammonium hydrogen phosphate, diammonium hydrogen phosphate or ammonium phosphate; and / or The pyrophosphate includes one or more of monoammonium pyrophosphate, diammonium pyrophosphate, triammonium pyrophosphate or ammonium pyrophosphate; and / or The inorganic carbon source comprises graphene; and / or The molar ratio of sodium to sodium salt, fluorine manganese compound, phosphate and pyrophosphate in the carbon-doped sodium vanadium oxide composite is 1: (1.5-1.7): (0.08-0.12): (1.05-1.25): (0.425-0.625); and / or The mass of the inorganic carbon source is 30-60% of the total mass of the sodium carbon in the carbon-doped sodium vanadium oxide composite.
[0014] In this embodiment, fluorine-manganese compound doping is adopted to complete fluorine-manganese doping without introducing other impurities; sodium salts, phosphates and pyrophosphates are introduced, and at high temperature, the amount of phosphates and pyrophosphates added is controlled, so that part of the oxides are converted into phosphates and pyrophosphates, and composite sodium vanadate and fluorine-manganese doped sodium vanadium phosphate materials are obtained. At the same time, because the organic acid radicals are carbonized and decomposed to obtain carbon and the graphene introduced later, an organic / inorganic carbon composite is formed, thereby effectively improving the electronic conductivity of the material. And the amount of fluorine-manganese cannot be too high or too low. If the manganese doping is too high, the structure will be unstable due to the Jan-Taylor effect of manganese. If the fluorine doping amount is too high, the cyclic performance of the material will be reduced; if the doping is too low, the effect will not be obvious. In some embodiments, the steps of mixing the carbon-doped sodium vanadium oxide composite with a sodium salt, a fluorine manganese compound, a phosphate, a pyrophosphate and an inorganic carbon source, adding water to slurry, grinding and drying to obtain a dried material include: The carbon-doped sodium vanadium oxide composite is mixed with sodium salt, fluorine manganese compound, phosphate, pyrophosphate and inorganic carbon source and slurried with water to obtain a slurry with a solid content of 30% to 40%; The slurry is ground to a particle size of 300-500 nm, and then the slurry is dried to a moisture content of less than or equal to 0.3% to obtain a dried material.
[0015] In this embodiment, the solid content will affect the subsequent grinding and drying, and may result in failure to obtain a slurry with a target particle size, so the preferred solid content is 30-40%.
[0016] In some embodiments, the calcination process of the dried material includes: heating up to a temperature of 550-650°C at a heating rate of 0.5-1°C / min, and keeping warm for 6-10 hours, and then cooling down to a temperature of the dried material less than 80°C for discharge; wherein, nitrogen is introduced during the calcination process to ensure that the humidity in the insulation section is ≤3% and the oxygen content is less than 2ppm.
[0017] In this embodiment, if the calcination temperature is too high, the primary particle size of the final composite sodium vanadium phosphate will be too large, and it may also cause decomposition and structural collapse of the sodium vanadium phosphate material, causing the sodium to migrate too far or unable to migrate, affecting the electrical properties; if the calcination temperature is too low, the sodium vanadium oxide complex cannot be fully converted into composite sodium vanadium phosphate, thereby causing the attenuation of the cycle performance; at the same time, the present application takes into account the problem of the carbon coating layer and the change in the valence state of vanadium, and therefore requires a stricter protective atmosphere during the calcination process.
[0018] In some embodiments, post-processing includes crushing, screening and iron removal.
[0019] In this embodiment, post-treatments such as crushing, screening and iron removal are used to obtain a template product with high purity and performance.
[0020] More preferably, the material is crushed to a particle size of 1 to 3 μm; an electromagnetic iron remover is used for iron removal, and the magnetic material in the material is removed to less than 0.5 ppm.
[0021] In a second aspect, an embodiment of the present application provides a composite sodium vanadium phosphate material, which is prepared by the above preparation method, wherein the compaction density of the composite sodium vanadium phosphate material is 2.35-2.46 g / mL, and the powder internal resistance is 20.1-23.5 Ω·cm.
[0022] In the technical scheme of the embodiment of the present application, the composite sodium vanadium phosphate material is a composite sodium vanadate material in fluorine-manganese-doped sodium vanadium phosphate. Through this structure, the capacity of the material can be greatly improved, and the compaction density of the material can also be improved. The present application introduces four anions, namely oxygen, phosphate, pyrophosphate, and fluoride ions, which can not only improve the voltage platform and capacity, but also form mutual doping, thereby improving its ionic conductivity; at the same time, although the traditional sodium vanadium phosphate has 3 sodium ions, because one sodium is in the skeleton structure, only 2 sodiums can be removed, making its capacity low, and the mutual doping structure formed by the four anions of the present application can make the third sodium in the sodium vanadium phosphate partially removed without affecting its structure, and at the same time, because of the doping of manganese and fluoride ions, the voltage platform can also be further improved, wherein, manganese doping can improve ionic conductivity and voltage platform, fluorine doping can improve voltage platform and ionic conductivity, and relative to other elements, the present application adopts fluorine-manganese doping, which can play a double superposition effect, and the effect is better.
[0023] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising: the above-mentioned composite sodium vanadium phosphate material.
[0024] In this embodiment, the positive electrode plate contains the above-mentioned composite sodium vanadium phosphate material, and thus has the advantages of high compaction density, good electronic conductivity and high capacity.
[0025] In a fourth aspect, an embodiment of the present application provides a secondary battery comprising the above-mentioned positive electrode plate.
[0026] In this embodiment, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantages of high compaction density, good electronic conductivity and high capacity.
[0027] In a fifth aspect, an embodiment of the present application provides an electrical device comprising the above-mentioned secondary battery.
[0028] In this embodiment, the electrical device includes the secondary battery, which has the advantages of good electronic conductivity and high capacity.
[0029] Compared with the prior art, the beneficial effects of this application are: The composite sodium vanadate and fluorine-manganese-doped sodium vanadium phosphate materials of the present application, compared with the traditional sodium vanadium phosphate, introduce four anions of oxygen, phosphate, pyrophosphate, and fluoride ions, which can not only improve the voltage platform and capacity, but also form mutual doping, thereby improving its ionic conductivity, and can make the third sodium part in the sodium vanadium phosphate escape without affecting its structure. At the same time, because of the doping of manganese and fluoride ions, the capacity and voltage platform are effectively improved while controlling the cost, and the capacity increment is significantly greater than the cost increment, and the compaction density is significantly improved. The present application is sintered in two steps, that is, the composite oxide with high density is first prepared, and then the composite sodium vanadium phosphate material is obtained by the conversion of anions, so that its compaction density is 20-50% higher than that of the traditional sodium vanadium phosphate, and the overall process is simple.
[0030] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 This is a schematic diagram of the process for preparing the composite sodium vanadium phosphate material of the present application; Figure 2 This is a SEM image of the carbon-doped sodium vanadium oxide composite in Example 1 of the present application; Figure 3 This is a SEM image of the second spray-dried material in Example 1 of the present application; Figure 4 This is a SEM image of the composite sodium vanadium phosphate material in Example 1 of the present application, wherein the magnification is 50000×; Figure 5 This is a SEM image of the composite sodium vanadium phosphate material in Example 1 of the present application, wherein the magnification is 100000×; Figure 6 The charge and discharge curves of the composite sodium vanadium phosphate material under different current rate conditions in Example 1 of the present application. DETAILED DESCRIPTION
[0033] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0035] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0036] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0037] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0038] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0039] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0040] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0041] At present, the commonly used synthesis methods of sodium vanadium phosphate are solid phase method and sol-gel method, and also include spray drying method, hydrothermal method, electrospinning method, etc. However, the biggest problem is that the cost is high, and the capacity is low compared with the cost. In order to improve its cost performance, there are two methods. The first is to reduce its cost, such as using other base metals to replace vanadium; the second is to increase its capacity to improve its cost performance, but it is usually difficult to take both cost and capacity into account at the same time.
[0042] In order to solve the technical problem that the capacity cannot be effectively increased while controlling the cost during the synthesis of sodium vanadium phosphate, the present application provides a composite sodium vanadium phosphate material and a preparation method thereof, a positive electrode sheet, a secondary battery and an electrical device.
[0043] In the first aspect, the present application provides a method for preparing a composite sodium vanadium phosphate material, such as Figure 1 As shown, the following steps are included: S1, mixing vanadium salt, organic acid sodium salt and water to obtain a mixed solution, and then drying and calcining to obtain a carbon-doped sodium vanadium oxide composite; S2, mixing the carbon-doped sodium vanadium oxide composite with sodium salt, fluorine manganese compound, phosphate, pyrophosphate and inorganic carbon source, adding water to slurry, grinding and drying to obtain a dried material; S3, calcining and post-treating the dried material to obtain a composite sodium vanadium phosphate material.
[0044] In the technical scheme of the embodiment of the present application, vanadium salt, organic acid sodium salt and water are mixed to form a solution, and then a carbon-doped sodium vanadium oxide complex is prepared at high temperature, wherein the organic acid sodium salt provides a sodium source and a carbon source at the same time, and is mixed with the vanadium salt during the calcination process and calcined, and vanadium is reduced to a trivalent state under high temperature and carbon thermal reduction, and the residual carbon is compounded on the sodium vanadium oxide complex under high temperature carbonization of the organic acid radical, and in this step, a material with a very high compaction density can be obtained; and then sodium salt, phosphate, pyrophosphate and inorganic carbon source are introduced to provide its electronic conductivity. The present application is sintered in two steps, that is, a composite oxide with a high degree of density is first prepared, and then a composite sodium vanadium phosphate is obtained by the conversion of anions, and its compaction density is 20-50% higher than that of traditional sodium vanadium phosphate.
[0045] In some embodiments, in step S1, the vanadium salt includes ammonium metavanadate or sodium metavanadate; the organic acid sodium salt includes sodium citrate. In the present application, the vanadium salts are all common salts with wide sources and low costs, and the amine in ammonium metavanadate is more volatile during the calcination process; sodium citrate can introduce sodium, and at the same time, the citrate radical can leave a small amount of carbon, acting as a carbon source.
[0046] In the technical solution of the embodiment of the present application, vanadium is first reduced under carbon reduction conditions at high temperature to prepare a carbon-doped sodium vanadium oxide complex, that is, sodium citrate is used as a carbon source, mixed with ammonium metavanadate under an inert atmosphere and then calcined, and vanadium is reduced to a trivalent state under high temperature and carbon thermal reduction. At the same time, the residual carbon will be compounded on the sodium vanadium oxide complex under high temperature carbonization of the citrate. In this step, a material with a very high compaction density can be obtained.
[0047] Further preferably, the molar ratio of the vanadium salt to the organic acid sodium salt is (2.9-3.2):1, such as 2.9:1, 3:1, 3.1:1 or 3.2:1; pure water is added in step S1 to form a mixed solution, and the concentration of sodium ions in the mixed solution is 3-5 mol / L, such as 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L or 5 mol / L.
[0048] In the technical solution of the embodiment of the present application, if the molar ratio of ammonium metavanadate and sodium citrate is too large, the sodium content will be high, which will cause the pH of the product to be high, and the carbon content will be high, the BET will be high, and the processing performance will be poor. If it is too small, there will be a lack of sodium, resulting in a low product capacity; the present application preferably has a molar ratio of ammonium metavanadate and sodium citrate of (2.9-3.2):1, which is conducive to obtaining a material with good processing performance, high compaction density and high capacity.
[0049] In some embodiments, the drying in step S1 is spray drying carried out in a drying tower. During the spray drying process, the speed of the atomizing wheel is controlled so that the particle size of the final spray is 3-10 μm; the air inlet temperature of the drying tower is 200-300°C, such as 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C, etc.; in the drying tower, the feed rate is controlled so that the temperature in the drying tower is 110-120°C, such as 110°C, 112°C, 114°C, 115°C, 116°C, 118°C or 200°C, etc.; the air outlet temperature is 80-100°C, such as 80°C, 82°C, 85°C, 88°C, 90°C, 93°C, 95°C, 97°C, 98°C or 100°C, etc.
[0050] In the technical solution of the embodiment of the present application, the mixed solution of the vanadium salt and the organic acid sodium salt is first dried to facilitate the subsequent calcination.
[0051] In some embodiments, the calcination process in step S1 is: in a nitrogen atmosphere (nitrogen is introduced so that the oxygen content in the atmosphere is less than 100 ppm), the temperature is increased to 800-900°C at a heating rate of 1-3°C / min, and the reaction is kept at 800-900°C for 4-6 hours; such as the heating rate is 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min or 3°C / min, the temperature is increased to 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C or 900°C, etc.; the reaction time is 4h, 4.5h, 5h, 5.5h or 6h, etc.
[0052] In the technical solution of the embodiment of the present application, step S1 obtains a carbon-doped sodium vanadium oxide complex by calcination, wherein the temperature cannot be too high or too low. If it is too high, the particles of the sodium vanadium oxide complex are too large and the BET is too small, which is not conducive to the subsequent reaction and also affects the electrical properties of the final product. If it is too low, the crystallinity of the sodium vanadium oxide complex is very poor, and even the sodium vanadium oxide complex cannot be obtained by reaction; the time cannot be too long or too short. If the reaction time is too long, the reaction efficiency is low, and it may also cause the crystal particles to be too large, affecting the capacity; if the reaction time is too short, the crystal growth is incomplete and the crystallinity is low, resulting in low cycle performance of the final product; it can be seen that in the present application, the reaction temperature cannot be reduced indefinitely by simply extending the reaction time, and better results can only be achieved within the said range.
[0053] In some embodiments, in step S2, the sodium salt includes sodium acetate or sodium bicarbonate; the fluorine manganese compound includes one or more of manganese difluoride, manganese trifluoride or manganese tetrafluoride; the phosphate includes one or more of ammonium monohydrogen phosphate, ammonium dihydrogen phosphate or ammonium phosphate; the pyrophosphate includes one or more of ammonium monohydrogen pyrophosphate, ammonium dihydrogen pyrophosphate, ammonium trihydrogen pyrophosphate or ammonium pyrophosphate; and the inorganic carbon source includes graphene.
[0054] In the technical solution of the embodiment of the present application, by adopting fluorine manganese compound doping, other impurities are not introduced while fluorine manganese doping is completed. Unless otherwise specified, manganese fluoride in the following text refers to manganese difluoride.
[0055] In some embodiments, in step S2, the molar ratio of sodium in the carbon-doped sodium vanadium oxide composite to sodium salt, fluorine manganese compound, phosphate, and pyrophosphate is 1: (1.5-1.7): (0.08-0.12): (1.05-1.25): (0.425-0.625), and the molar amount of sodium acetate can be 1.5, 1.55, 1.6, 1.65 or 1.7, etc., and the molar amount of fluorine manganese compound can be 0.08, 0.0 The molar amount multiple of phosphate can be 1.05, 1.1, 1.15, 1.2 or 1.25, and the molar amount multiple of pyrophosphate can be 0.425, 0.45, 0.475, 0.5, 0.525, 0.55, 0.575, 0.6 or 0.625, etc.; the mass of the added inorganic carbon source is 30-60% of the total mass of sodium carbon in the carbon-doped sodium vanadium oxide composite, such as 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc.
[0056] In the technical solution of the embodiment of the present application, sodium salts, phosphates and pyrophosphates are introduced. At high temperature, by controlling the amount of phosphates and pyrophosphates added, part of the oxides are converted into phosphates and pyrophosphates to obtain composite sodium vanadate and fluorine-manganese-doped sodium vanadium phosphate materials. At the same time, due to the carbonization and decomposition of organic acid radicals, carbon and graphene introduced later are formed to form an organic / inorganic carbon composite, thereby effectively improving the electronic conductivity of the material.
[0057] In some embodiments, step S2 specifically includes: mixing the carbon-doped sodium vanadium oxide complex with sodium salt, fluorine manganese compound, phosphate, pyrophosphate and inorganic carbon source and adding water to slurry to obtain a slurry with a solid content of 30% to 40%; the solid content can be, for example, 30%, 35% or 40%; then grinding the slurry to a particle size of 300 to 500 nm, and then spray drying the slurry to a moisture content of less than or equal to 0.3% to obtain a dried material; the grinding conditions can be selected according to conventional techniques in the art to ensure that the slurry particle size meets the target requirements; preferably, the slurry particle size is 300 to 500 nm, such as any one or more mixtures of 300 nm, 325 nm, 350 nm, 370 nm, 380 nm, 400 nm, 415 nm, 430 nm, 450 nm, 480 nm and 500 nm. The spray drying conditions in step S2 can refer to the spray drying conditions in step S1.
[0058] In the technical solution of the embodiment of the present application, the solid content refers to the total mass of solids in the slurry divided by the mass of all components constituting the slurry. The solid content will affect the subsequent grinding and drying, and may result in the inability to obtain a slurry with a target particle size, so the preferred solid content is 30-40%.
[0059] In some embodiments, the calcination process of the dried material in step S3 includes: heating to a temperature of 550-650°C at a heating rate of 0.5-1°C / min, keeping the temperature at this temperature for 6-10 hours, and then cooling the material to a temperature below 80°C before discharging; wherein, nitrogen is introduced during the calcination process so that the humidity of the insulation section is ≤3% and the oxygen content is less than 2ppm. wherein, the insulation temperature can be selected from 550°C, 555°C, 560°C, 575°C, 580°C, 590°C, 600°C, 605°C, 615°C, 630°C, 640°C or 650°C, etc.; the insulation time can be selected from 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h or 10h, etc.
[0060] In the technical solution of the embodiment of the present application, if the calcination temperature of step S3 is too high, the primary particle size of the final composite sodium vanadium phosphate will be too large, and it may also cause the decomposition and structural collapse of the sodium vanadium phosphate material, causing the migration distance of sodium to be too far or the sodium to be unable to migrate, affecting the electrical performance; if it is too low, the sodium vanadium oxide complex cannot be fully converted into composite sodium vanadium phosphate, thereby causing the attenuation of the cycle performance; at the same time, the present application takes into account the problem of the carbon coating layer and the change of the valence state of vanadium, so a more stringent protective atmosphere is required during the calcination process in step S3.
[0061] In some embodiments, the post-processing of step S3 includes crushing, screening and iron removal; packaging may also be performed depending on the situation.
[0062] Further preferably, in the pulverizing process, a jet mill is used, and the pulverizing is stopped after the material particle size is 1 to 3 μm; an electromagnetic iron remover is used for iron removal, and the magnetic material of the material is removed to less than 0.5 ppm; the packaging process is carried out in a constant temperature and humidity room, maintaining the temperature at 25±5°C and the humidity ≤10%.
[0063] As a preferred embodiment, the preparation method of the composite sodium vanadium phosphate material of the present application comprises the following steps: S1, adding ammonium metavanadate to sodium citrate, adding pure water, stirring to dissolve, then spray drying, and then calcining under an inert atmosphere to obtain a carbon-doped sodium vanadium oxide composite; S2, adding the carbon-doped sodium vanadium oxide composite to sodium acetate, manganese fluoride, phosphate, pyrophosphate and graphene, then mixing, adding pure water to slurry, and then continuing to grind until the slurry particle size is 300-500nm; then spray drying to obtain a spray-dried material; S3, calcining the spray-dried material under an inert atmosphere to obtain a calcined material, crushing the calcined material, screening to remove iron and packaging to obtain a composite sodium vanadium phosphate material.
[0064] In this embodiment, the cost of the obtained composite sodium vanadium phosphate material is increased by about 10-15% compared with traditional sodium vanadium phosphate, but the capacity is increased by about 20%, the compaction density is increased by 20-50%, the voltage platform is increased by 10%, and the cost performance is greatly improved.
[0065] In a second aspect, an embodiment of the present application provides a composite sodium vanadium phosphate material, which is prepared using the above preparation method.
[0066] In the technical solution of the embodiment of the present application, the composite sodium vanadium phosphate material is a sodium vanadate material composited in sodium vanadium phosphate doped with fluorine and manganese. Through this structure, the capacity of the material can be greatly improved, and the compaction density of the material is also improved. The present application introduces four anions, namely oxygen, phosphate, pyrophosphate, and fluoride, which can not only improve the voltage platform and capacity, but also form mutual doping, thereby improving its ionic conductivity; at the same time, although the traditional sodium vanadium phosphate has three sodium ions, because one sodium is in the skeleton structure, only two sodiums can be released, making its capacity relatively low, and the mutual doping structure formed by the four anions of the present application can make the third sodium in the sodium vanadium phosphate partially released without affecting its structure, and at the same time, due to the doping of manganese and fluoride ions, the voltage platform can be further improved, among which manganese doping can improve ionic conductivity and voltage platform, fluorine doping can improve voltage platform and ionic conductivity, and relative to other elements, the present application adopts fluorine-manganese doping, which can play a double superposition effect and has a better effect, and the dosage of the two cannot be too high or too low. If the manganese doping is too high, the structure will be unstable due to the Jan-Taylor effect of manganese, and if the fluorine doping amount is too high, the cycle performance of the material will be reduced; if the doping is too low, the effect is not obvious.
[0067] In the technical solution of the embodiment of the present application, the composite sodium vanadium phosphate has excellent performance, a compaction density of 2.35-2.46 g / mL, a powder internal resistance of 20.1-23.5 Ω·cm, a 0.1C charge capacity of 131.7-132.9 mAh / g, a 0.1C discharge capacity of 117.5-118.9 mAh / g, and a 0.1C discharge median voltage of 3.35-3.44 V.
[0068] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising: the above-mentioned composite sodium vanadium phosphate material, or the composite sodium vanadium phosphate material prepared by any of the above-mentioned methods.
[0069] In this embodiment, the positive electrode plate contains the above-mentioned composite sodium vanadium phosphate material, and thus has the advantages of high compaction density, good electronic conductivity and high capacity.
[0070] In a fourth aspect, an embodiment of the present application provides a secondary battery comprising the above-mentioned positive electrode plate.
[0071] In this embodiment, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantages of high compaction density, good electronic conductivity and high capacity.
[0072] In a fifth aspect, an embodiment of the present application provides an electrical device comprising the above-mentioned secondary battery.
[0073] In this embodiment, the electrical device includes the secondary battery, which has the advantages of good electronic conductivity and high capacity.
[0074] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0075] 1. Preparation method Example 1 S1, adding ammonium metavanadate to sodium citrate, adding pure water, stirring and dissolving, the molar ratio of ammonium metavanadate to sodium citrate is 3:1, the concentration of sodium in the solution is 4 mol / L, and the obtained solution is spray dried. During the spray drying process, the atomizing wheel speed is controlled so that the final spray particle size is 8.4 μm, the inlet air temperature is 245±5°C, and the outlet air temperature is 85-89°C. In the drying tower, the temperature in the drying tower is 115±2°C by controlling the feed rate, and the first spray dried material is obtained; the first spray dried material is calcined in an inert atmosphere, and during the calcination process, the temperature rise curve is 2°C / min, and the temperature is raised to 860°C, and the reaction is carried out at this temperature for 5 hours, and nitrogen is introduced so that the oxygen content in the atmosphere is less than 100 ppm, to obtain a carbon-doped sodium vanadium oxide complex; S2, adding sodium acetate, manganese fluoride, ammonium dihydrogen phosphate, ammonium dihydrogen pyrophosphate and graphene to the carbon-doped sodium vanadium oxide complex obtained above, the molar ratio of sodium in the carbon-doped sodium vanadium oxide complex to sodium acetate, manganese fluoride, phosphate and pyrophosphate is 1:1.6:0.1:1.15:0.525, the mass of graphene added is 40% of the mass of sodium carbon in the carbon-doped sodium vanadium oxide complex, pure water is added to the mixture to make a slurry, so that the solid content in the slurry is 34.7%, and then continue to grind until the slurry particle size is 415nm; then spray drying to obtain a second spray-dried material, the moisture content in the second spray-dried material is 0.21%; S3, calcining the second spray-dried material under nitrogen atmosphere at a heating rate of 0.8°C / min to a temperature of 600°C, keeping the temperature at this temperature for 8h, then cooling the temperature to a temperature below 80°C before discharging the material, introducing nitrogen during the calcination process to make the humidity in the insulation section 2.1-2.5%, and the oxygen content below 2ppm, to obtain a calcined material, pulverizing the calcined material, using a jet mill to pulverize the material until the particle size is 1.63μm and then stopping, sieving through a 100-mesh ultrasonic vibrating sieve, and then removing iron by an electromagnetic iron remover, and removing iron until the magnetic substance of the material is less than 0.5ppm before packaging, the packaging process is carried out in a constant temperature and humidity room, maintaining the temperature at 25±5°C and the humidity ≤10%, to obtain a composite sodium vanadium phosphate material, which can be recorded as Na according to its raw material ratio. 2.6 VO0.6 Mn 0.1 F 0.1 (PO4) 1.15 (P2O7) 0.525 / C.
[0076] Example 2 The difference between Example 2 and Example 1 is that the calcination and holding temperature in step S1 is 800° C. The remaining preparation steps are the same as those in Example 1 to obtain a composite sodium vanadium phosphate material.
[0077] Example 3 The difference between Example 3 and Example 1 is that the calcination and holding temperature in step S1 is 900° C. The remaining preparation steps are the same as those in Example 1 to obtain a composite sodium vanadium phosphate material.
[0078] Example 4 The difference between Example 4 and Example 1 is that: in step S2, the molar ratio of sodium to manganese fluoride in the carbon-doped sodium vanadium oxide composite is 1:0.08. The remaining preparation steps are the same as those in Example 1 to obtain a composite sodium vanadium phosphate material.
[0079] Example 5 The difference between Example 5 and Example 1 is that: in step S2, the molar ratio of sodium to manganese fluoride in the carbon-doped sodium vanadium oxide composite is 1:0.12. The remaining preparation steps are the same as those in Example 1 to obtain a composite sodium vanadium phosphate material.
[0080] Example 6 The difference between Example 5 and Example 1 is that: in step S3, the sintering temperature is 550° C. The remaining preparation steps are the same as those in Example 1, and a composite sodium vanadium phosphate material is obtained.
[0081] Example 7 The difference between Example 5 and Example 1 is that: in step S3, the sintering temperature is 650° C. The remaining preparation steps are the same as those in Example 1, and a composite sodium vanadium phosphate material is obtained.
[0082] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that manganese fluoride is removed in step S2. The remaining preparation steps are the same as those in Example 1 to obtain a composite sodium vanadium phosphate material.
[0083] The results showed that after removing manganese fluoride, the voltage platform and ionic conductivity of the obtained composite sodium vanadium phosphate material decreased due to the lack of fluorine manganese doping.
[0084] Performance Testing 1. The products obtained in the three steps of Example 1 were respectively subjected to electron microscope scanning, and the obtained SEM images are as follows: Figure 2-5 shown.
[0085] See also Figure 2 The SEM image of the carbon-doped sodium vanadium oxide composite obtained in step S1 of Example 1 shows that it is a block particle.
[0086] See also Figure 3 The second spray-dried material obtained in step S2 of Example 1 is densely packed spherical particles.
[0087] See also Figure 4 and Figure 5 The final product of Example 1, the composite sodium vanadium phosphate material, is granular, and the primary particle size is about 400 nm.
[0088] 2. The products obtained in the three steps of Example 1 were sampled and tested respectively, and the results are shown in Tables 1 to 3 below; wherein: During the test, the carbon content was tested using a carbon-sulfur analyzer. The compacted density was tested using a 3T pressure test. The pH test method was to take 10g of material, add 100mL of pure water, stir and mix for 10 minutes, filter, and test the filtrate at 25°C. The powder resistivity was tested using a four-probe method with a pressure of 3T.
[0089] Table 1 Sampling and testing results of carbon-doped sodium vanadium oxide composites
[0090] It can be seen from Table 1 that the compacted density of the carbon-doped sodium vanadium oxide composite obtained in Example 1 can reach 3.52 g / mL.
[0091] Table 2 Test results of the second spray-dried material
[0092] As shown in Table 2, the specific surface area (BET) of the second spray-dried material obtained in Example 1 after grinding and other treatments is significantly increased relative to the carbon-doped sodium vanadium oxide composite, reaching 17.6 m 2 / g.
[0093] Table 3 Test results of composite sodium vanadium phosphate materials
[0094] It can be seen from Table 3 that after calcination, Example 1 has completed the doping of fluorine, manganese and carbon. At the same time, after secondary sintering, the graphitization degree of carbon is also improved, the carbon content is increased, and the powder resistivity of the obtained composite sodium vanadium phosphate material is reduced.
[0095] 3. The composite sodium vanadium phosphate material obtained in Example 1 was mixed with PVDF and SP in a mass ratio of 85:8:7, and NMP was added to homogenize it. Then, it was coated on a carbon-coated aluminum foil as a positive electrode. 1 mol / L sodium hexafluorophosphate was used in the electrolyte, to which 1,3,6-hexane trinitrile and fluorocarbonate were added in a molar ratio of 1:1. A sodium sheet was used as the negative electrode. The battery was assembled into a button, and the test voltage range was 2-4.5V. The current of different rates was used for testing. The results are shown in Table 4 and Figure 6 shown.
[0096] Table 4 Test results of the composite sodium vanadium phosphate material assembled with buckle battery obtained in Example 1
[0097] As shown in Table 4, the composite sodium vanadium phosphate material obtained in Example 1 is used to assemble a button battery, and the discharge efficiency is high, which is above 88%; the capacity retention rate at low temperature is above 86%; at room temperature, the capacity retention rate is high (up to 97.4%) after 500 cycles at 1C.
[0098] like Figure 6 As shown, it is the charging and discharging curve of the buckle assembly of the material obtained in Example 1. Figure 6 From the above, we can see that the capacity has been significantly improved, and the voltage has also been improved to a certain extent. The median voltage of 0.1C discharge is about 3.4V, which is about 0.2V higher than the median voltage of pure sodium vanadium phosphate of about 3.2V (measured under the same test conditions in this application), an increase of 6.25%.
[0099] 4. Tests were conducted on Examples 1-7 and Comparative Example 1, mainly including tests on the compaction density and powder internal resistance of the composite sodium vanadium phosphate material; the composite sodium vanadium phosphate material was assembled and charged under the same conditions as in Article 3 above, and the battery capacity and median discharge voltage at a rate of 0.1C were tested; the results are shown in Table 5 below.
[0100] Table 5 Data comparison results of the embodiments and comparative examples
[0101] It can be seen from Examples 1-3 that as the calcination and insulation temperature in step S1 increases, the powder internal resistance of the final product composite sodium vanadium phosphate material shows a downward trend, the charging capacity and the discharge capacity both increase first and then decrease, the discharge median voltage remains basically unchanged, and the overall performance does not change much. Therefore, the preferred calcination and insulation temperature in step S1 of the present invention is 800-900°C.
[0102] It can be seen from Example 1 and Examples 4-5 that with the increase of the amount of manganese fluoride doping in step S2, the internal resistance of the powder shows a downward trend, and the charging capacity, discharge capacity and discharge median voltage all show a trend of first increasing and then stabilizing. In Comparative Example 1, manganese fluoride is not doped, and the material properties are significantly reduced, especially the discharge capacity and discharge median voltage. Therefore, the molar ratio of sodium to manganese fluoride in the carbon-doped sodium vanadium oxide composite in step S2 of the present invention is preferably 1: (0.08-0.12).
[0103] It can be seen from Example 1 and Examples 6-7 that with the increase of the calcination and insulation temperature in step S3, the powder internal resistance of the final product composite sodium vanadium phosphate material shows a downward trend. Within a certain range, a relatively low calcination and insulation temperature is more conducive to improving the charge and discharge capacity. Therefore, the preferred calcination and insulation temperature in step S3 of the present invention is 550-650°C.
[0104] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a composite sodium vanadium phosphate material, characterized in that: The following steps are involved: The vanadium salt, the organic acid sodium salt and water are mixed to obtain a mixed solution, and then the mixed solution is dried and calcined to obtain a carbon-doped sodium vanadium oxide composite; The carbon-doped sodium vanadium oxide composite is mixed with sodium salt, fluorine manganese compound, phosphate, pyrophosphate and inorganic carbon source, and slurried with water, and then ground and dried to obtain a dried material; The dried material is calcined and post-treated to obtain a composite sodium vanadium phosphate material.
2. The method for preparing the composite sodium vanadium phosphate material according to claim 1, characterized in that: The vanadium salt comprises one or more of ammonium metavanadate or sodium metavanadate; and / or The organic acid sodium salt comprises sodium citrate; and / or The molar ratio of the vanadium salt to the organic acid sodium salt is (2.9-3.2):1; and / or The concentration of sodium ions in the mixed solution is 3-5 mol / L.
3. The method for preparing the composite sodium vanadium phosphate material according to claim 1, characterized in that: In the step of obtaining the carbon-doped sodium vanadium oxide composite by drying and calcining, the calcining process comprises: heating the temperature to 800-900° C. at a heating rate of 1-3° C. / min under a nitrogen atmosphere, and keeping the temperature for a reaction of 4-6 hours.
4. The method for preparing the composite sodium vanadium phosphate material according to claim 1, characterized in that: The sodium salt includes sodium acetate or sodium bicarbonate; and / or The fluorine manganese compound includes one or more of manganese difluoride, manganese trifluoride or manganese tetrafluoride; and / or The phosphate includes one or more of monoammonium hydrogen phosphate, diammonium hydrogen phosphate or ammonium phosphate; and / or The pyrophosphate includes one or more of monoammonium pyrophosphate, diammonium pyrophosphate, triammonium pyrophosphate or ammonium pyrophosphate; and / or The inorganic carbon source comprises graphene; and / or The molar ratio of sodium to sodium salt, fluorine manganese compound, phosphate and pyrophosphate in the carbon-doped sodium vanadium oxide composite is 1: (1.5-1.7): (0.08-0.12): (1.05-1.25): (0.425-0.625); and / or The mass of the inorganic carbon source is 30-60% of the total mass of the sodium carbon in the carbon-doped sodium vanadium oxide composite.
5. The method for preparing the composite sodium vanadium phosphate material according to claim 1, characterized in that: The step of mixing the carbon-doped sodium vanadium oxide composite with sodium salt, fluorine manganese compound, phosphate, pyrophosphate and inorganic carbon source, adding water to slurry, grinding and drying to obtain a dried material comprises: The carbon-doped sodium vanadium oxide composite is mixed with sodium salt, fluorine manganese compound, phosphate, pyrophosphate and inorganic carbon source and slurried with water to obtain a slurry with a solid content of 30% to 40%; The slurry is ground to a particle size of slurry particles of 300-500 nm, and then the slurry is dried to a moisture content of less than or equal to 0.3% to obtain the dried material.
6. The method for preparing the composite sodium vanadium phosphate material according to claim 1, characterized in that: The calcination process of the dried material includes: heating the temperature to 550-650°C at a heating rate of 0.5-1°C / min, and keeping the temperature for 6-10 hours, and then cooling the temperature to less than 80°C before discharging the dried material; Wherein, nitrogen is introduced during the calcination process to ensure that the humidity in the insulation section is ≤3% and the oxygen content is lower than 2ppm.
7. The method for preparing the composite sodium vanadium phosphate material according to claim 1, characterized in that: The post-processing includes crushing, screening and iron removal.
8. A composite sodium vanadium phosphate material, characterized in that: The composite sodium vanadium phosphate material is prepared by the preparation method according to any one of claims 1 to 7, wherein the compaction density of the composite sodium vanadium phosphate material is 2.35 to 2.46 g / mL, and the powder internal resistance is 20.1 to 23.5 Ω·cm.
9. A positive electrode sheet, characterized in that: The positive electrode plate comprises the composite sodium vanadium phosphate material according to claim 8.
10. A secondary battery, characterized in that: The invention comprises the positive electrode sheet as claimed in claim 9.
Citation Information
Cited By
Modified sodium vanadium phosphate positive electrode material as well as preparation method and application thereof