Polycarboxylate superplasticizer with defoaming function and preparation method thereof

By using polycarboxylic acid water reducing agent with its own defoaming function in the gelling material, the bubble content is reduced, the appearance and mechanical properties are improved, the problem of bubble introduction in the gelling material is solved, and the compressive flexural strength is improved and durability.

CN118994508APending Publication Date: 2024-11-22TIANJIN TIANYING NEW BUILDING MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159589.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the stirring of the gelling material, anionic surfactant introduces a large number of mechanical bubbles, resulting in poor mechanical strength, durability and appearance, which is difficult for the prior art to effectively solve this problem.

Method used

Using a polycarboxylic acid water reducing agent with its own defoaming function, through the combination of methylallyl alcohol polyoxyethylene ether, organic acid, EO/PO acetic diol adduct, polyprotein, oxidant and reducing agent, through The redox system is terpolymerized to prepare a polymer that can significantly reduce the bubble content for use in hydraulic adhesive systems.

Benefits of technology

Significantly reduce the gas content of the system, improve appearance, improve compressive flexural strength, improve durability, and control the molecular weight during the polymerization process through polymerization inhibitors to reduce the risk of explosive polymerization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
Patent Text Reader

Abstract

The invention relates to a polycarboxylic acid water reducer with a defoaming function and a preparation method thereof, the polycarboxylic acid water reducer comprises 10-60 mol% of methylallyl alcohol polyoxyethylene ether, 32-75 mol% of organic acid, 0.1-2 mol% of EO / PO alkynediol addition surfactant, 0.1-0.5 mol% of polymerization inhibitor, 0.1-0.7 mol% of oxidant and 0.03-0.15 mol% of reducing agent, the preparation method comprises the following steps: synthesizing a functional polymer, dissolving the functional polymer in water to prepare a stable aqueous solution, adding the aqueous solution into the aqueous solution, and uniformly stirring to prepare the polycarboxylic acid water reducer with the defoaming function. The obtained polymer aqueous solution is subjected to ternary polymerization with methylallyl alcohol polyoxyethylene ether and organic acid through a redox system, and when the polymer for the hydraulic system is applied to a cement-based or gypsum-based system, the gas content of the system can be remarkably reduced, the appearance can be obviously improved, the compressive strength and the breaking strength can be improved, and the durability can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical construction, and in particular to a polycarboxylic acid water-reducing agent with a self-defoaming function and a preparation method thereof. Background Art

[0002] Generally, dispersants are required to be added to organic or inorganic hydraulic binder slurries, such as clay, silicate powder, chalk, carbon black, and water slurries of hydraulic binders, in order to improve the processing properties of the system, i.e., kneading, spreading, spraying, pumpability or fluidity, etc., especially for building materials such as cement, gypsum, semi-hydrated gypsum or anhydrous gypsum.

[0003] In order to convert these cementitious materials into a form suitable for construction, it is necessary to add a dispersant and water for stirring. During the stirring process, since the dispersant is generally an anionic surfactant, it will increase the surface tension of water and inevitably introduce a large number of mechanical bubbles. However, these bubbles will cause the mechanical strength, durability and appearance to deteriorate. Therefore, in order to solve the above problems, the present invention proposes a polycarboxylate water-reducing agent with a self-defoaming function and a preparation method. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a polycarboxylic acid water-reducing agent with self-defoaming function and a preparation method thereof, which can effectively reduce the bubble content.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] A polycarboxylic acid water reducer with self-defoaming function, characterized by comprising 10-60 mol% of methyl allyl alcohol polyoxyethylene ether, 32-75 mol% of organic acid, 0.1-2 mol% of EO / PO acetylene glycol adduct, 0.1-0.5 mol% of inhibitor, 0.1-0.7 mol% of oxidant, 0.03-0.15 mol% of reducing agent,

[0007] Preferably, the methyl allyl alcohol polyoxyethylene ether is one or a combination of the following: methyl allyl alcohol polyoxyethylene ether-500, methyl allyl alcohol polyoxyethylene ether-1500, methyl allyl alcohol polyoxyethylene ether-2000, methyl allyl alcohol polyoxyethylene ether-3000, methyl allyl alcohol polyoxyethylene ether-5000,

[0008] Preferably, the organic acid is one or more of the following: maleic acid, fumaric acid, acrylic acid, methacrylic acid, glacial acetic acid, polyacrylic acid, citric acid,

[0009] Preferably, the polymerization inhibitor is one or more of the following: mercaptopropionic acid, mercaptoethanol, sodium methyl methacrylate sulfonate, thioglycolic acid, sodium hypophosphite, hydroquinone, and phenothiazine.

[0010] A method for preparing a polycarboxylate water-reducing agent with a self-contained defoaming function, the specific steps are as follows:

[0011] A. Synthesizing EO / PO acetylene glycol adducts and dissolving them in water to prepare stable aqueous solutions;

[0012] B. The polymer aqueous solution obtained in step A is used for ternary copolymerization with methyl allyl alcohol polyoxyethylene ether and organic acid through a redox system.

[0013] Beneficial effects of the present invention:

[0014] The polymer for hydraulic system provided by the present invention can be applied to cement-based or gypsum-based systems to significantly reduce the gas content of the system, significantly improve the appearance, increase the compressive and flexural strengths, and enhance the durability; and the polymerization inhibitor used in the present invention can reduce the risk of explosion during the polymerization process and better control the molecular weight of the polymer. DETAILED DESCRIPTION

[0015] The technical solution of the present invention will be clearly and completely described below in combination with the embodiments and table data. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0016] Example 1

[0017] Using p-tert-butylphenol as an initiator, 15 parts of p-tert-butylphenol, 0.5 parts of 98% sodium bicarbonate and 305 parts of acetylene glycol are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. The air in the reaction vessel is replaced with an inert gas, and the temperature is raised to 145°C and maintained under the protection of an inert gas. 1650 parts of ethylene oxide are added to the reactor within 15 hours. After adding ethylene oxide, the temperature is kept for 1.5 hours. Thus, the EO / PO acetylene glycol adduct (Compound A) is prepared. After Compound A is naturally cooled, it is dissolved in water to prepare a 50% aqueous solution, and a certain amount of phenothiazine is added to inhibit polymerization.

[0018] Add 350 parts of methyl allyl alcohol polyoxyethylene ether-3000 to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Add 500 parts of water and heat to 80 degrees Celsius. Add 5 parts of sodium bicarbonate. After dissolving, turn on the refrigerator and cool to 16°C. Add 50 parts of compound A and 150 parts of glacial acetic acid. At the same time, vitamin B5 solution and hydrogen peroxide solution are added dropwise. After 240 minutes, the solution is added dropwise. The reaction is completed when no oxide residue is detected using hydrogen oxygen test paper to obtain dispersant TP-1.

[0019] Example 2

[0020] Using p-tert-butylphenol as an initiator, 10 parts of p-tert-butylphenol, 0.5 parts of 98% sodium bicarbonate and 500 parts of acetylene glycol are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. The air in the reaction vessel is replaced with an inert gas, and the temperature is raised to 120°C and maintained under the protection of an inert gas. Within 15 hours, 1050 parts of ethylene oxide and 650 parts of propylene oxide are added to the reactor. After adding ethylene oxide, the temperature is kept for 2 hours. Thus, the EO / PO acetylene glycol adduct (compound B) is prepared. After compound B is naturally cooled, it is dissolved in water to prepare a 50% aqueous solution, and a certain amount of phenothiazine is added to inhibit polymerization.

[0021] 250 parts of methyl allyl alcohol polyoxyethylene ether-3000 and 110 parts of methyl allyl alcohol polyoxyethylene ether-2000 are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Add 600 parts of water and heat to 80 degrees Celsius. Add 5 parts of sodium bicarbonate. After dissolving, turn on the refrigerator and cool to 16°C. Add 50 parts of compound B and 150 parts of glacial acetic acid. At the same time, vitamin B5 solution and hydrogen peroxide solution are added dropwise. After 180 minutes, the solution is added dropwise. The reaction is completed when no oxide residue is detected using hydrogen oxygen test paper to obtain dispersant TP-2.

[0022] Example 3

[0023] Take 30 parts of 4-hydroxybutyl vinyl ether as initiator, add 10 parts of anhydrous ethanol, 0.5 parts of 98% sodium bicarbonate and 500 parts of acetylene glycol into a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Use inert gas to replace the air in the reaction vessel, and heat up to 140°C and maintain under the protection of inert gas. Add 1000 parts of ethylene oxide and 750 parts of propylene oxide into the reactor within 15 hours. After adding ethylene oxide and propylene oxide, keep warm for 1 hour. Thus, EO / PO acetylene glycol adduct (Compound C) is prepared. After Compound C is naturally cooled, it is dissolved in water to prepare a 50% aqueous solution, and a certain amount of phenothiazine is added to inhibit polymerization.

[0024] 200 parts of methyl allyl alcohol polyoxyethylene ether-3000 and 240 parts of methyl allyl alcohol polyoxyethylene ether-5000 are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Add 400 parts of water and heat to 45 degrees Celsius. Add 15 parts of sodium bicarbonate. After dissolving, turn on the refrigerator and cool to 16°C. Add 50 parts of compound C and 150 parts of adipic acid. At the same time, vitamin B5 solution and hydrogen peroxide solution are added dropwise. After 180 minutes, the solution is added dropwise. The reaction is completed when no oxide residue is detected using hydrogen oxygen test paper to obtain dispersant TP-3.

[0025] Example 4

[0026] 200 parts of methyl allyl alcohol polyoxyethylene ether-3000 and 240 parts of methyl allyl alcohol polyoxyethylene ether-5000 are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Add 400 parts of water and heat to 45 degrees Celsius. Add 15 parts of sodium bicarbonate. After dissolving, turn on the refrigerator and cool to 16 ° C. Add 50 parts of a mixture of compound A, compound B and compound C and 59 parts of acrylic acid. Vitamin B5 solution and hydrogen peroxide solution are added dropwise at the same time. After 120 minutes, the solution is added dropwise. The reaction is completed when no oxide residue is detected using hydrogen oxygen test paper to obtain dispersant TP-4.

[0027] Example 5

[0028] 200 parts of methyl allyl alcohol polyoxyethylene ether-3000 and 240 parts of methyl allyl alcohol polyoxyethylene ether-2000 are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Add 400 parts of water and heat to 45 degrees Celsius. Add 15 parts of sodium bicarbonate. After dissolving, turn on the refrigerator and cool to 16°C. Add 50 parts of a mixture of compound B and compound C and 36 parts of acrylic acid. At the same time, vitamin B5 solution and hydrogen peroxide solution are added dropwise. After 120 minutes, the solution is added dropwise. The reaction is completed when no oxide residue is detected using hydrogen oxygen test paper to obtain dispersant TP-5.

[0029] Example 6

[0030] 200 parts of methyl allyl alcohol polyoxyethylene ether-3000 and 200 parts of methyl allyl alcohol polyoxyethylene ether-2000 are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Add 400 parts of water and heat to 45 degrees Celsius. Add 15 parts of sodium bicarbonate. After dissolving, turn on the refrigerator and cool to 16°C. Add 50 parts of a mixture of compound B and compound C and 45 parts of acrylic acid. At the same time, E51 (1% solution) and hydrogen peroxide solution (27.5%) are added dropwise. After 120 minutes, the solution is added dropwise. Potassium hydroxide solution is added to adjust the pH value to 7. The reaction is terminated when no oxide residue is detected using hydrogen peroxide test paper to obtain dispersant TP-6.

[0031] Example 7

[0032] 450 parts of methyl allyl alcohol polyoxyethylene ether-3000 are added to a pressure-resistant stainless steel reactor equipped with a thermometer, a stirrer, a pressure sensor and a nitrogen conduit. Add 400 parts of water and heat to 45 degrees Celsius. Add 15 parts of sodium bicarbonate. After dissolving, turn on the refrigerator and cool to 12°C. Add 50 parts of a mixture of compound A and compound C and 45 parts of acrylic acid. At the same time, add dropwise reducing agent FF6 (1.5% solution) and ammonium persulfate solution (3%). After 120 minutes, the solution is added dropwise. Potassium hydroxide solution is added to adjust the pH value to 7. Use hydrogen oxygen test paper to detect that there is no oxide residue, which means that the reaction is completed, and dispersant TP-7 is obtained.

[0033] Test description:

[0034] 1. Concrete testing

[0035] Concrete tests were conducted using dispersants TP-1 to TP-7 and compared with commercially available polycarboxylate water reducers using the concrete mix ratios shown in Table 1. Concrete mixing was performed using a 60L forced mixer, with crushed stone, river sand, cement, water and dispersants (TP-1 to TP-7) added in sequence and mixed within the specified time. Concrete slump and air content tests were conducted according to GB / T 50080, and the test results are shown in Table 3.

[0036]

[0037] Table 1

[0038] 2. Appearance test

[0039] Use the freshly mixed concrete used in the slump test to make a 150*150*150mm square concrete test block. After hardening, demould, and calculate the area ratio of bubbles generated on the side of the test block as an indicator for evaluating the appearance. The smaller the bubble area ratio, the better the improvement effect of the concrete appearance. The bubble area ratio <3% is excellent, 3-4% is ordinary, and >4% is poor. The appearance test results are shown in Table 3.

[0040] 3. Gypsum mortar test

[0041] Mortar tests were conducted using the mortar mix proportions shown in Table 2 using dispersants TP-1 to TP-7 and in comparison with commercially available polycarboxylate water reducers.

[0042] The fluidity test method is carried out in accordance with the provisions of "Gypsum-based Self-leveling Mortar" (JC / T1023-2021). The specific test steps are as follows: First, place the fluidity test mold in the center of the test board and ensure that its surface is clean and free of water stains. Then put the stirred gypsum-based self-leveling slurry into the fluidity test mold. After filling it up, quickly lift the test mold vertically upward. The lifting action is completed within 2 seconds. The lifting distance is approximately 5cm-10cm. Keep this action for 10s to 15s after lifting, so that the slurry flows from the test mold to the test board. After 5s, the test mold can be removed and wait for 4 minutes. During this time, the slurry will flow into a circle on the test board. Then you can use a steel ruler to measure the diameter of the circle formed by the slurry on the test board. When measuring, measure the two diameter values ​​in the vertical direction and then take the average value. The value is accurate to 1mm. Then place the slurry in a stirring pot and let it stand for (30±0.5)min, then stir it slowly for 1min, and repeat the above method to retest the fluidity, that is, 30min fluidity.

[0043] In the 40mm×40mm×160mm strength test mold, the slurry is filled and leveled with a scraper. The specimen is demoulded within 1 hour after final setting. Two groups of specimens are prepared at the same time. The specimens are left to stand for (24±0.5)h under standard experimental conditions. One group is directly tested for 24h flexural strength according to the provisions of "Determination of Mechanical Properties of Building Gypsum" (GB / T17669.3-1999); the other group is moved to the oven and dried in an electric blast drying oven at (40±2)℃ to a constant weight (the weight of the specimen is constant if the weight reduction is not more than 1g in 24h). The dried specimens should be cooled to room temperature under standard experimental conditions, and then the absolute dry flexural strength is tested according to the provisions of "Determination of Mechanical Properties of Building Gypsum" (GB / T17669.3-1999). The compressive strength was measured using a compression testing machine in accordance with the requirements of "Determination of Mechanical Properties of Building Gypsum" (GB / T17669.3-1999), where the pressure-bearing area is 40.0mm×40.0mm.

[0044] The compressive strength is calculated according to formula 2-1, and the calculation result is accurate to 0.1MPa.

[0045]

[0046] Where: R C — compressive strength,

[0047] P—failure load, N;

[0048] — equal to 1600, pressure bearing area, The appearance test in the gypsum mortar test is to use the mortar after the fluidity test to make a 160*40*40mm rectangular square test block. After hardening, demoulding is performed, and the area ratio of bubbles generated on the side of the test block is calculated as an indicator for evaluating the appearance. The smaller the bubble area ratio, the better the mortar appearance improvement effect. The bubble area ratio <3% is excellent, 3-4% is ordinary, and >4% is poor. The data of the test structure are shown in Table 4.

[0049]

[0050] Table 2

[0051]

[0052] Table 3

[0053]

[0054] Table 4

[0055] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A polycarboxylate water reducer with self-defoaming function, characterized in that The invention comprises 10-60 mol% of methyl allyl alcohol polyoxyethylene ether, 32-75 mol% of organic acid, 0.1-2 mol% of EO / PO acetylene glycol adduct, 0.1-0.5 mol% of polymerization inhibitor, 0.1-0.7 mol% of oxidant and 0.03-0.15 mol% of reducing agent.

2. The polycarboxylate water-reducing agent with self-defoaming function according to claim 1, characterized in that The methyl allyl alcohol polyoxyethylene ether is one or a combination of the following: methyl allyl alcohol polyoxyethylene ether-500, methyl allyl alcohol polyoxyethylene ether-1500, methyl allyl alcohol polyoxyethylene ether-2000, methyl allyl alcohol polyoxyethylene ether-3000, and methyl allyl alcohol polyoxyethylene ether-5000.

3. The polycarboxylate water-reducing agent with self-defoaming function according to claim 1, characterized in that The organic acid is one or more of the following: maleic acid, fumaric acid, acrylic acid, methacrylic acid, glacial acetic acid, polyacrylic acid, and citric acid.

4. The polycarboxylate water-reducing agent with self-defoaming function according to claim 1, characterized in that The polymerization inhibitor is one or more of the following compositions: mercaptopropionic acid, mercaptoethanol, sodium methyl propylene sulfonate, thioglycolic acid, sodium hypophosphite, hydroquinone, and phenothiazine.

5. The method for preparing a polycarboxylate water-reducing agent with self-defoaming function according to any one of claims 1 to 4, wherein the specific steps are as follows: A. Synthesizing EO / PO acetylene glycol adducts and dissolving them in water to prepare stable aqueous solutions; B. The polymer aqueous solution obtained in step A is used for ternary copolymerization with methyl allyl alcohol polyoxyethylene ether and organic acid through a redox system.