Cold-resistant EPDM (Ethylene-Propylene-Diene Monomer) rubber material for sealing power battery and preparation method thereof
The modification of white carbon black, black carbon black, nano silica and adjust the component ratio by macromolecular silane coupling agent, combined with the co-vulcanization of ethylene-butad rubber and ethylene-propylene rubber, the EPDM rubber material is solved in cold resistance and The physical and mechanical properties of the material have improved the stability and flame retardancy of the material at low temperatures.
Patent Information
- Application Number
- CN202411246697.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
During the preparation of EPDM rubber materials, carbon black is prone to aggregation, resulting in a decline in material performance, making it difficult to maintain both cold resistance and physical and mechanical properties.
The macromolecular silane coupling agent is used to chemically modify white carbon black, black carbon black and nano silica, and the modified filler is formed by adjusting the component ratio and process parameters to improve the cold resistance and flame retardancy of the material, combined with three Co-vulcanization of ethylene-butadiene rubber and ethylene-propylene rubber to enhance physical and mechanical properties.
It significantly improves the cold resistance, physical and mechanical properties and flame retardancy of EPDM rubber materials, ensuring the improvement of structural stability and comprehensive performance in low temperature environments.
Smart Images

Figure BDA0005030981300000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber preparation, in particular to a cold-resistant EPDM rubber material for power battery sealing and a preparation method thereof. Background Art
[0002] EPDM is a synthetic rubber with excellent heat and cold resistance. This material is composed of a terpolymer of ethylene, propylene and non-conjugated dienes. Since its commercial production began in 1963, it has been widely used in various fields due to its superior resistance to oxidation, ozone and corrosion. The cold resistance of EPDM is mainly measured by its glass transition temperature (Tg). The lower the Tg, the better the cold resistance. By adjusting parameters such as the type and content of the third monomer, the ethylene-propylene ratio, and the molecular weight, the cold resistance and other physical properties of EPDM can be optimized. New EPDM materials such as VNB-EPT and EBT not only maintain excellent temperature resistance, but also improve durability, which is conducive to resource conservation and environmental protection, showing an important role and development potential in modern industry.
[0003] At present, in the process of preparing EPDM rubber materials, carbon black and other related materials are often added. Since carbon black is easy to aggregate, the performance of the rubber material is greatly reduced. Therefore, in order to solve the above problems, the present invention prepares a cold-resistant EPDM rubber material for power battery sealing and a preparation method thereof. Summary of the invention
[0004] The object of the present invention is to provide a cold-resistant EPDM rubber material for power battery sealing and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for preparing a cold-resistant EPDM rubber material for power battery sealing, comprising the following steps:
[0007] Step 1: Add EPDM rubber, chlorinated polyethylene and EPDM rubber into an internal mixer, mix at 100-120°C for 2-5 minutes, add modified filler, continue mixing for 5-8 minutes, finally add 2-mercaptobenzimidazole and paraffin, heat to 150-170°C, mix for 4-6 minutes, and obtain a mixed rubber;
[0008] Step 2: After the mixed rubber is allowed to stand for 2-3 hours, triallyl isocyanurate and di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 90-120° C. for 6-8 minutes, and the mixture is allowed to stand for 20-24 hours, and then a vulcanization reaction is carried out to obtain an EPDM rubber material.
[0009] More optimally, the modified filler comprises the following components: by weight, 10-12 parts of macromolecular silane coupling agent and 4-5 parts of multi-component filler.
[0010] More optimally, the multi-component filler includes white carbon black, black carbon black, and nano-silicon dioxide in a mass ratio of 1:1:(2-3).
[0011] More optimally: the preparation process of the macromolecular silane coupling agent is:
[0012] S1: (1) dissolving N-benzyl-N-(3-butene)amine in dimethyl sulfoxide to obtain an N-benzyl-N-(3-butene)amine solution; (2) adding the N-benzyl-N-(3-butene)amine solution dropwise to ethyl dichlorophosphate at 80-90° C., and adding triethylamine, reacting for 4-5 hours, filtering, washing, and drying to obtain intermediate A;
[0013] S2: Dissolve intermediate A in ethylene glycol, heat to 80-90°C, slowly add amino EPDM rubber, stir ultrasonically, and react for 4-5h to obtain intermediate B;
[0014] S3: Mix the intermediate B, 3-mercaptopropyltrimethoxysilane and ethanol, stir ultrasonically for 30-40 minutes, add azobisisobutyronitrile under protective atmosphere, heat to 70-80°C, react for 5-8 hours, and obtain a macromolecular silane coupling agent.
[0015] More optimally: the raw materials of the intermediate A include the following components: by weight, 8-10 parts of ethyl dichlorophosphate, 6-7 parts of N-benzyl-N-(3-butene)amine, and 1-2 parts of triethylamine;
[0016] The raw materials of the intermediate B include the following components: by weight, 6-8 parts of intermediate A, 5-6 parts of amino ethylene propylene diene monomer rubber, and 40-50 parts of ethylene glycol;
[0017] The raw materials of the macromolecular silane coupling agent include the following components: by weight, 4-5 parts of intermediate B, 3-4 parts of 3-mercaptopropyltrimethoxysilane, 20-25 parts of ethanol, and 0.1-0.2 parts of azobisisobutyronitrile.
[0018] More optimally: the preparation process of the modified filler is: mix the macromolecular silane coupling agent and ethanol, use glacial acetic acid to adjust the pH to 5±0.2, add the multi-element filler, ultrasonically stir for 30-40 minutes, heat to 50-60°C, stir for 3-4 hours, wash and dry to obtain the modified filler.
[0019] More optimally, the EPDM rubber material includes the following components: by weight, 30-40 parts of ethylene propylene diene monomer rubber, 20-25 parts of ethylene butylene monomer rubber, 8-10 parts of chlorinated polyethylene, 3-4 parts of modified filler, 0.5-0.8 parts of 2-mercaptobenzimidazole, 0.8-1 parts of paraffin, 2-3 parts of triallyl isocyanurate, and 3-4 parts of di-tert-butyl peroxyisopropylbenzene.
[0020] More optimally, the process parameters of the vulcanization reaction are: temperature 150-160°C, time 40-50min, pressure 12-15Mpa.
[0021] The present invention chemically modifies white carbon black, black carbon black and nano silicon dioxide by using a macromolecular silane coupling agent, and controls the dosage of various components at the same time, so that the obtained EPDM rubber material has improved physical and mechanical properties and flame retardancy on the basis of good cold resistance. The details are as follows:
[0022] First, after hydrolysis, the macromolecular silane coupling agent can combine with the groups on the surface of white carbon black, black carbon black, and nano-silicon dioxide to form silicon-oxygen bonds, thereby improving the cold resistance of the overall material. At the same time, nano-silicon dioxide has a three-dimensional network structure, which can ensure the structural stability of the material in a low-temperature environment. Compared with a single filler, a multi-filler has better synergy, thereby effectively improving the comprehensive performance of the rubber material.
[0023] Second: The macromolecular silane coupling agent has a PN junction, which improves the flame retardant effect of the modified filler. The EPDM rubber segment it contains allows the multi-component filler to be well cross-linked with the base rubber, improving the compatibility of white carbon black, black carbon black, and nano-silicon dioxide in the matrix and avoiding the interaction between the three. At the same time, the three as reinforcing materials can effectively enhance the physical properties of rubber materials.
[0024] Third: The use of EPDM and EPDM together makes the main chain more active and more suitable for functioning at low temperatures. In addition, the co-vulcanization of chlorinated polyethylene with EPDM and EPDM can effectively enhance the overall physical and mechanical properties of the rubber, reduce the vulcanization time and enhance the vulcanization efficiency. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that the following parts are parts by weight. The purchase manufacturers of all raw materials involved in the present invention are exemplified without any special restrictions: in the following embodiments, N-benzyl-N-(3-butene)amine CAS is 17150-62-8, and the purchase manufacturer is Hongchuang Pharmaceutical Technology; ethyl dichlorophosphate CAS is 1498-51-7, and the purchase manufacturer is Beijing Bailingwei Technology Co., Ltd.; 3-mercaptopropyltrimethoxysilane CAS is 4420-74-0, and the purchase manufacturer is Beijing Bailingwei Technology Co., Ltd.; white carbon black CAS is 10279-57-9, and the purchase manufacturer is Shandong Binli New Materials Co., Ltd.; black carbon black CAS is 1333-86-4, and the purchase manufacturer is Shijiazhuang Yuexiu Technology Co., Ltd.; nano-silica is Brofos-SiO2, purchased from Bohuas Nanotechnology.
[0027] Preparation of amino ethylene propylene rubber: (1) At 60°C, add 10 parts of ethylene propylene rubber to a flask filled with xylene and stir until it is completely dissolved. At 65°C, under a nitrogen atmosphere, add 0.5 parts of acrylonitrile and 0.05 parts of azobisisobutyronitrile in sequence and stir to react for 5 hours. Use acetone for precipitation, extract with N,N-dimethylformamide, and vacuum dry to obtain cyanated ethylene propylene rubber. (2) At 60°C, add 10 parts of cyanated ethylene propylene rubber and 1 part of activated RaneyNi catalyst in sequence to a flask filled with xylene. Control the reaction pressure to 5 MPa and stir to react for 60 minutes to obtain amino ethylene propylene rubber.
[0028] Embodiment 1: A method for preparing a cold-resistant EPDM rubber material for power battery sealing, comprising the following steps:
[0029] Preparation of macromolecular silane coupling agent:
[0030] S1: (1) dissolving 6 parts of N-benzyl-N-(3-butene)amine in 50 parts of dimethyl sulfoxide to obtain an N-benzyl-N-(3-butene)amine solution; (2) adding the N-benzyl-N-(3-butene)amine solution dropwise to 8 parts of ethyl dichlorophosphate at 80°C, and adding 1 part of triethylamine, reacting for 4 hours, filtering, washing, and drying to obtain an intermediate A;
[0031] S2: Dissolve 6 parts of intermediate A in 40 parts of ethylene glycol, heat to 80°C, slowly add 5 parts of amino ethylene propylene rubber, stir ultrasonically, and react for 4 hours to obtain intermediate B;
[0032] S3: 4 parts of intermediate B, 3 parts of 3-mercaptopropyltrimethoxysilane and 20 parts of ethanol were mixed, ultrasonically stirred for 30 minutes, 0.1 parts of azobisisobutyronitrile were added under nitrogen, the temperature was raised to 70°C, and the reaction was carried out for 5 hours to obtain a macromolecular silane coupling agent;
[0033] Preparation of modified filler: 10 parts of macromolecular silane coupling agent and 30 parts of ethanol were mixed, pH was adjusted to 5 with glacial acetic acid, 4 parts of multi-component filler (1 part of white carbon black, 1 part of black carbon black, 2 parts of nano-silica) were added, ultrasonic stirring was performed for 30 minutes, the temperature was raised to 50°C, stirring was performed for 3 hours, washing and drying were performed to obtain modified filler;
[0034] Step 1: Add 30 parts of EPDM rubber, 8 parts of chlorinated polyethylene, and 20 parts of EPDM rubber into an internal mixer, mix at 100°C for 2 minutes, add 3 parts of modified filler, continue mixing for 5 minutes, and finally add 0.5 parts of 2-mercaptobenzimidazole and 0.8 parts of paraffin, heat to 150°C, mix for 4 minutes, and obtain a mixed rubber;
[0035] Step 2: After the mixed rubber is allowed to stand for 2 hours, 2 parts of triallyl isocyanurate and 3 parts of di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 90°C for 6 minutes, and the mixture is allowed to stand for 20 hours. After that, the mixture is vulcanized at 150°C and a pressure of 12 MPa for 40 minutes to obtain an EPDM rubber material.
[0036] Embodiment 2: A method for preparing a cold-resistant EPDM rubber material for power battery sealing, comprising the following steps:
[0037] Preparation of macromolecular silane coupling agent:
[0038] S1: (1) dissolving 7 parts of N-benzyl-N-(3-butene)amine in 50 parts of dimethyl sulfoxide to obtain an N-benzyl-N-(3-butene)amine solution; (2) adding the N-benzyl-N-(3-butene)amine solution dropwise to 10 parts of ethyl dichlorophosphate at 90°C, and adding 2 parts of triethylamine, reacting for 5 hours, filtering, washing, and drying to obtain an intermediate A;
[0039] S2: 8 parts of intermediate A are dissolved in 50 parts of ethylene glycol, the temperature is raised to 90°C, 6 parts of amino ethylene propylene rubber are slowly added, ultrasonic stirring is performed, and the reaction is performed for 5 hours to obtain intermediate B;
[0040] S3: 5 parts of intermediate B, 4 parts of 3-mercaptopropyltrimethoxysilane and 25 parts of ethanol were mixed, ultrasonically stirred for 30 minutes, 0.2 parts of azobisisobutyronitrile were added under nitrogen, the temperature was raised to 80°C, and the reaction was carried out for 8 hours to obtain a macromolecular silane coupling agent;
[0041] Preparation of modified filler: 12 parts of macromolecular silane coupling agent and 35 parts of ethanol were mixed, pH was adjusted to 5 with glacial acetic acid, 5 parts of multi-component filler (1 part of white carbon black, 1 part of black carbon black, 3 parts of nano-silica) were added, ultrasonic stirring was performed for 40 minutes, the temperature was raised to 60°C, stirring was performed for 4 hours, washing and drying were performed to obtain modified filler;
[0042] Step 1: Add 40 parts of EPDM rubber, 10 parts of chlorinated polyethylene, and 25 parts of EPDM rubber into an internal mixer, mix at 120°C for 5 minutes, add 4 parts of modified filler, continue mixing for 8 minutes, and finally add 0.8 parts of 2-mercaptobenzimidazole and 1 part of paraffin, heat to 170°C, mix for 6 minutes, and obtain a mixed rubber;
[0043] Step 2: After the mixed rubber is allowed to stand for 3 hours, 3 parts of triallyl isocyanurate and 4 parts of di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 120°C for 8 minutes, and the mixture is allowed to stand for 24 hours. After that, the mixture is vulcanized at 160°C and a pressure of 15 MPa for 50 minutes to obtain an EPDM rubber material.
[0044] Embodiment 3: A method for preparing a cold-resistant EPDM rubber material for power battery sealing, comprising the following steps:
[0045] Preparation of macromolecular silane coupling agent:
[0046] S1: (1) dissolving 6.5 parts of N-benzyl-N-(3-butene)amine in 50 parts of dimethyl sulfoxide to obtain an N-benzyl-N-(3-butene)amine solution; (2) adding the N-benzyl-N-(3-butene)amine solution dropwise to 9 parts of ethyl dichlorophosphate at 85° C., and adding 1.5 parts of triethylamine, reacting for 4.5 hours, filtering, washing, and drying to obtain an intermediate A;
[0047] S2: Dissolve 7 parts of intermediate A in 45 parts of ethylene glycol, heat to 85°C, slowly add 5.5 parts of amino ethylene propylene rubber, stir ultrasonically, and react for 4.5 hours to obtain intermediate B;
[0048] S3: 4.5 parts of intermediate B, 3.5 parts of 3-mercaptopropyltrimethoxysilane and 22 parts of ethanol were mixed, ultrasonically stirred for 30 minutes, 0.15 parts of azobisisobutyronitrile were added under nitrogen, the temperature was raised to 75°C, and the reaction was carried out for 8 hours to obtain a macromolecular silane coupling agent;
[0049] Preparation of modified filler: 11 parts of macromolecular silane coupling agent and 32 parts of ethanol were mixed, pH was adjusted to 5 with glacial acetic acid, 5.5 parts of multi-component filler (1 part of white carbon black, 1 part of black carbon black, 3.5 parts of nano-silicon dioxide) were added, ultrasonic stirring was performed for 40 minutes, the temperature was raised to 60°C, stirring was performed for 4 hours, washing and drying were performed to obtain modified filler;
[0050] Step 1: Add 35 parts of EPDM rubber, 9 parts of chlorinated polyethylene, and 22 parts of EPDM rubber into an internal mixer, mix at 120°C for 5 minutes, add 3.5 parts of modified filler, continue mixing for 8 minutes, and finally add 0.6 parts of 2-mercaptobenzimidazole and 0.9 parts of paraffin, heat to 170°C, mix for 6 minutes, and obtain a mixed rubber;
[0051] Step 2: After the mixed rubber is allowed to stand for 3 hours, 2.5 parts of triallyl isocyanurate and 3.5 parts of di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 120°C for 8 minutes, and the mixture is allowed to stand for 24 hours. After that, the mixture is vulcanized at 155°C and a pressure of 13 MPa for 45 minutes to obtain an EPDM rubber material.
[0052] Embodiment 4: A method for preparing a cold-resistant EPDM rubber material for power battery sealing, comprising the following steps:
[0053] Preparation of macromolecular silane coupling agent:
[0054] S1: (1) dissolving 7 parts of N-benzyl-N-(3-butene)amine in 50 parts of dimethyl sulfoxide to obtain an N-benzyl-N-(3-butene)amine solution; (2) adding the N-benzyl-N-(3-butene)amine solution dropwise to 10 parts of ethyl dichlorophosphate at 90°C, and adding 2 parts of triethylamine, reacting for 5 hours, filtering, washing, and drying to obtain an intermediate A;
[0055] S2: 8 parts of intermediate A are dissolved in 50 parts of ethylene glycol, the temperature is raised to 90°C, 6 parts of amino ethylene propylene rubber are slowly added, ultrasonic stirring is performed, and the reaction is performed for 5 hours to obtain intermediate B;
[0056] S3: 4.5 parts of intermediate B, 3.5 parts of 3-mercaptopropyltrimethoxysilane and 22 parts of ethanol were mixed, ultrasonically stirred for 30 minutes, 0.15 parts of azobisisobutyronitrile were added under nitrogen, the temperature was raised to 75°C, and the reaction was carried out for 8 hours to obtain a macromolecular silane coupling agent;
[0057] Preparation of modified filler: 10 parts of macromolecular silane coupling agent and 30 parts of ethanol were mixed, pH was adjusted to 5 with glacial acetic acid, 4 parts of multi-component filler (1 part of white carbon black, 1 part of black carbon black, 2 parts of nano-silica) were added, ultrasonic stirring was performed for 30 minutes, the temperature was raised to 50°C, stirring was performed for 3 hours, washing and drying were performed to obtain modified filler;
[0058] Step 1: Add 40 parts of EPDM rubber, 10 parts of chlorinated polyethylene, and 25 parts of EPDM rubber into an internal mixer, mix at 120°C for 5 minutes, add 4 parts of modified filler, continue mixing for 8 minutes, and finally add 0.8 parts of 2-mercaptobenzimidazole and 1 part of paraffin, heat to 170°C, mix for 6 minutes, and obtain a mixed rubber;
[0059] Step 2: After the mixed rubber is allowed to stand for 3 hours, 2.5 parts of triallyl isocyanurate and 3.5 parts of di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 120°C for 8 minutes, and the mixture is allowed to stand for 24 hours. After that, the mixture is vulcanized at 155°C and a pressure of 13 MPa for 45 minutes to obtain an EPDM rubber material.
[0060] Comparative Example 1: No nano-silicon dioxide was added, and the rest was the same as Example 4, specifically as follows:
[0061] Preparation of macromolecular silane coupling agent:
[0062] S1: (1) dissolving 7 parts of N-benzyl-N-(3-butene)amine in 50 parts of dimethyl sulfoxide to obtain an N-benzyl-N-(3-butene)amine solution; (2) adding the N-benzyl-N-(3-butene)amine solution dropwise to 10 parts of ethyl dichlorophosphate at 90°C, and adding 2 parts of triethylamine, reacting for 5 hours, filtering, washing, and drying to obtain an intermediate A;
[0063] S2: 8 parts of intermediate A are dissolved in 50 parts of ethylene glycol, the temperature is raised to 90°C, 6 parts of amino ethylene propylene rubber are slowly added, ultrasonic stirring is performed, and the reaction is performed for 5 hours to obtain intermediate B;
[0064] S3: 4.5 parts of intermediate B, 3.5 parts of 3-mercaptopropyltrimethoxysilane and 22 parts of ethanol were mixed, ultrasonically stirred for 30 minutes, 0.15 parts of azobisisobutyronitrile were added under nitrogen, the temperature was raised to 75°C, and the reaction was carried out for 8 hours to obtain a macromolecular silane coupling agent;
[0065] Preparation of modified filler: 10 parts of macromolecular silane coupling agent and 30 parts of ethanol were mixed, pH was adjusted to 5 with glacial acetic acid, 4 parts of multi-component filler (2 parts of white carbon black and 2 parts of black carbon black) were added, ultrasonic stirring was performed for 30 minutes, the temperature was raised to 50°C, stirring was performed for 3 hours, washing and drying were performed to obtain modified filler;
[0066] Step 1: Add 40 parts of EPDM rubber, 10 parts of chlorinated polyethylene, and 25 parts of EPDM rubber into an internal mixer, mix at 120°C for 5 minutes, add 4 parts of modified filler, continue mixing for 8 minutes, and finally add 0.8 parts of 2-mercaptobenzimidazole and 1 part of paraffin, heat to 170°C, mix for 6 minutes, and obtain a mixed rubber;
[0067] Step 2: After the mixed rubber is allowed to stand for 3 hours, 2.5 parts of triallyl isocyanurate and 3.5 parts of di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 120°C for 8 minutes, and the mixture is allowed to stand for 24 hours. After that, the mixture is vulcanized at 155°C and a pressure of 13 MPa for 45 minutes to obtain an EPDM rubber material.
[0068] Comparative Example 2: No macromolecular silane coupling agent is used to modify white carbon black, black carbon black, and nano-silicon dioxide, and the modified filler is replaced by a mixed filler; the rest is the same as Example 4, specifically as follows:
[0069] Step 1: Add 40 parts of EPDM rubber, 10 parts of chlorinated polyethylene, and 25 parts of EPDM rubber into an internal mixer, mix at 120°C for 5 minutes, add 4 parts of mixed filler (1 part of white carbon black, 1 part of black carbon black, and 2 parts of nano-silica), continue mixing for 8 minutes, and finally add 0.8 parts of 2-mercaptobenzimidazole and 1 part of paraffin, heat to 170°C, and mix for 6 minutes to obtain a mixed rubber;
[0070] Step 2: After the mixed rubber is allowed to stand for 3 hours, 2.5 parts of triallyl isocyanurate and 3.5 parts of di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 120°C for 8 minutes, and the mixture is allowed to stand for 24 hours. After that, the mixture is vulcanized at 155°C and a pressure of 13 MPa for 45 minutes to obtain an EPDM rubber material.
[0071] Comparative Example 3: The macromolecular silane coupling agent is replaced with vinyl triethoxysilane to modify white carbon black, black carbon black and nano silicon dioxide, as follows:
[0072] Preparation of modified filler: 10 parts of vinyl triethoxysilane and 30 parts of ethanol were mixed, pH was adjusted to 5 with glacial acetic acid, 4 parts of multi-component filler (1 part of white carbon black, 1 part of black carbon black, 2 parts of nano-silica) were added, ultrasonic stirring was performed for 30 minutes, the temperature was raised to 50°C, stirring was performed for 3 hours, washing and drying were performed to obtain modified filler;
[0073] Step 1: Add 40 parts of EPDM rubber, 10 parts of chlorinated polyethylene, and 25 parts of EPDM rubber into an internal mixer, mix at 120°C for 5 minutes, add 4 parts of modified filler, continue mixing for 8 minutes, and finally add 0.8 parts of 2-mercaptobenzimidazole and 1 part of paraffin, heat to 170°C, mix for 6 minutes, and obtain a mixed rubber;
[0074] Step 2: After the mixed rubber is allowed to stand for 3 hours, 2.5 parts of triallyl isocyanurate and 3.5 parts of di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 120°C for 8 minutes, and the mixture is allowed to stand for 24 hours. After that, the mixture is vulcanized at 155°C and a pressure of 13 MPa for 45 minutes to obtain an EPDM rubber material.
[0075] Detection experiment:
[0076] (1) At room temperature, the oxygen index of the EPDM rubber materials obtained in Example 4 and Comparative Examples 1-3 was measured according to the national standard GB / T10707 "Determination of Rubber Combustion Properties"; the tensile strength and elongation at break were measured according to the national standard GB / T 528 "Determination of Tensile Properties of Vulcanized Rubber and Thermoplastic Rubber";
[0077] (2) At 25° C., according to standard Q / CR563-2017, the EPDM rubber materials of Example 4 and Comparative Examples 1-3 were vertically loaded to 25 kN, and the stiffness between 1 and 25 kN was calculated;
[0078] (3) The EPDM rubber materials of Example 4 and Comparative Examples 1-3 were placed in an environment of -40°C for 24 hours, kept at a constant temperature for 24 hours, and the stiffness was measured and compared with that at 25°C to calculate the static stiffness change rate;
[0079] (4) The EPDM rubber materials of Example 4 and Comparative Examples 1-3 were measured for glass transition temperature using ASTM D3418;
[0080] The measured data are shown in the following table:
[0081]
[0082] Table 1
[0083] Conclusion: Example 4 chemically modifies white carbon black, black carbon black and nano-silicon dioxide by using a modifier, and controls the dosage of various components at the same time, so that the physical mechanical properties and flame retardancy are improved. And its glass transition temperature is -75.7℃, indicating that it can be transformed from a hard and brittle state to a soft and elastic state in a low temperature environment, so the obtained EPDM rubber material can be used at a lower temperature and has excellent cold resistance.
[0084] In Comparative Example 1, nano-silica is not added, which reduces the overall performance of the material; in Comparative Example 2, no macromolecular silane coupling agent is used to modify white carbon black, black carbon black, and nano-silica, which reduces the compatibility of white carbon black, black carbon black, and nano-silica with the group, affecting the overall physical properties of the material, and due to the lack of flame retardant groups, the flame retardant effect of the material is also reduced; in Comparative Example 3, the macromolecular silane coupling agent is replaced with vinyl triethoxy silane to modify white carbon black, black carbon black, and nano-silica, resulting in reduced performance.
[0085] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0086] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a cold-resistant EPDM rubber material for power battery sealing, characterized in that: The following steps are involved: Step 1: Add EPDM rubber, chlorinated polyethylene and EPDM rubber into an internal mixer, mix at 100-120°C for 2-5 minutes, add modified filler, continue mixing for 5-8 minutes, finally add 2-mercaptobenzimidazole and paraffin, heat to 150-170°C, mix for 4-6 minutes, and obtain a mixed rubber; Step 2: After the mixed rubber is allowed to stand for 2-3 hours, triallyl isocyanurate and di-tert-butyl peroxyisopropylbenzene are added, and the mixture is mixed at 90-120° C. for 6-8 minutes, and the mixture is allowed to stand for 20-24 hours, and then a vulcanization reaction is carried out to obtain an EPDM rubber material.
2. The method for preparing a cold-resistant EPDM rubber material for power battery sealing according to claim 1, characterized in that: The modified filler comprises the following components: by weight, 10-12 parts of a macromolecular silane coupling agent and 4-5 parts of a multi-component filler.
3. The method for preparing a cold-resistant EPDM rubber material for power battery sealing according to claim 2, characterized in that: The multi-component filler comprises white carbon black, black carbon black and nano silicon dioxide in a mass ratio of 1:1:(2-3).
4. The method for preparing a cold-resistant EPDM rubber material for power battery sealing according to claim 2, characterized in that: The preparation process of the macromolecular silane coupling agent is: S1: (1) dissolving N-benzyl-N-(3-butene)amine in dimethyl sulfoxide to obtain an N-benzyl-N-(3-butene)amine solution; (2) adding the N-benzyl-N-(3-butene)amine solution dropwise to ethyl dichlorophosphate at 80-90° C., and adding triethylamine, reacting for 4-5 hours, filtering, washing, and drying to obtain intermediate A; S2: Dissolve intermediate A in ethylene glycol, heat to 80-90°C, slowly add amino EPDM rubber, stir ultrasonically, and react for 4-5h to obtain intermediate B; S3: Mix the intermediate B, 3-mercaptopropyltrimethoxysilane and ethanol, stir ultrasonically for 30-40 minutes, add azobisisobutyronitrile under protective atmosphere, heat to 70-80°C, react for 5-8 hours, and obtain a macromolecular silane coupling agent.
5. The method for preparing a cold-resistant EPDM rubber material for power battery sealing according to claim 4, characterized in that: The raw materials of the intermediate A include the following components: by weight, 8-10 parts of ethyl dichlorophosphate, 6-7 parts of N-benzyl-N-(3-butene)amine, and 1-2 parts of triethylamine; The raw materials of the intermediate B include the following components: by weight, 6-8 parts of intermediate A, 5-6 parts of amino ethylene propylene diene rubber, and 40-50 parts of ethylene glycol; The raw materials of the macromolecular silane coupling agent include the following components: by weight, 4-5 parts of intermediate B, 3-4 parts of 3-mercaptopropyltrimethoxysilane, 20-25 parts of ethanol, and 0.1-0.2 parts of azobisisobutyronitrile.
6. The method for preparing a cold-resistant EPDM rubber material for power battery sealing according to claim 2, characterized in that: The preparation process of the modified filler is as follows: mixing a macromolecular silane coupling agent and ethanol, adjusting the pH to 5±0.2 with glacial acetic acid, adding a multi-element filler, ultrasonically stirring for 30-40 minutes, heating to 50-60° C., stirring for 3-4 hours, washing, and drying to obtain the modified filler.
7. The method for preparing a cold-resistant EPDM rubber material for power battery sealing according to claim 1, characterized in that: The EPDM rubber material comprises the following components: by weight, 30-40 parts of ethylene propylene diene monomer rubber, 20-25 parts of ethylene butylene monomer rubber, 8-10 parts of chlorinated polyethylene, 3-4 parts of modified filler, 0.5-0.8 parts of 2-mercaptobenzimidazole, 0.8-1 parts of paraffin, 2-3 parts of triallyl isocyanurate, and 3-4 parts of di-tert-butyl peroxyisopropylbenzene.
8. The method for preparing a cold-resistant EPDM rubber material for power battery sealing according to claim 1, characterized in that: The process parameters of the vulcanization reaction are: temperature 150-160° C., time 40-50 min, and pressure 12-15 MPa.
9. The EPDM rubber material obtained according to the method for preparing a cold-resistant EPDM rubber material for power battery sealing according to any one of claims 1 to 8.
Citation Information
Cited By
EPDM-based crosslinked rubber material and preparation method thereof
CN122302436A