High-damping solid buoyancy material and preparation method thereof

Through the combination of polyurethane/polymethyl methacrylate blended polymer and hollow glass microbeads, a high-damping solid buoyancy material with an interpenetrating network structure is solved, and the problem of insufficient deformation and damping characteristics of existing materials in deep-sea environments is solved. It realizes lightweight, pressure-resistant and high damping characteristics, suitable for high-pressure environments of submersibles and submarines.

CN118994890APending Publication Date: 2024-11-22TAIZHOU CBM FUTURE NEW MATERIALS S & T CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411261113.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing solid buoyancy materials are difficult to maintain small deformation in deep-sea environments, and cannot have damping characteristics and rigidity at the same time, so as to meet the high-pressure environment needs of submersibles and submarines.

Method used

Polyurethane/polymethyl methacrylate blended polymer is used as the matrix, combined with hollow glass beads as filler, forming an interpenetrating network structure, achieving high damping characteristics and good stiffness, and preparing through specific ratios and process steps High damping solid buoyancy material.

Benefits of technology

It realizes the lightweight, pressure-resistant and high damping characteristics of the material, and can maintain small deformation in deep-sea environments. It is suitable for the use of submersibles and submarines, and has sound insulation, vibration damping and impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005036161120000081
    Figure BDA0005036161120000081
Patent Text Reader

Abstract

The invention provides a high-damping solid buoyancy material. The high-damping solid buoyancy material comprises the following raw materials in parts by weight: 100 parts of polyether polyol; 1 to 5 parts of trimethylolpropane; 70 to 130 parts of diphenylmethane diisocyanate; 20 to 90 parts of methyl methacrylate; 0.1 to 5 parts of azodiisobutyronitrile; and 20-150 parts of hollow glass beads. According to the invention, a technical route in which a polyurethane / polymethyl methacrylate blend polymer is used as a matrix and hollow glass beads are used as a light pressure-resistant filler is adopted. The polyurethane / polymethyl methacrylate blended polymer has an interpenetrating network structure, and also has high damping characteristic and better rigidity; the hollow glass beads reduce the density of the material on the basis of ensuring the pressure-resistant characteristic, so that the material has the buoyancy characteristic. The finally formed solid buoyancy material product simultaneously has the characteristics of light weight, pressure resistance and high damping, and meets the use requirements of submersibles and submarines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a high-damping solid buoyancy material and a preparation method thereof. Background Art

[0002] Traditional solid buoyancy materials are generally composed of epoxy resin matrix and hollow glass microsphere filler, with low density and high pressure resistance, and are widely used in submersibles to provide buoyancy support. With the improvement of technical requirements for submersibles, a high-damping buoyancy material is needed that can provide sound insulation, vibration reduction and impact resistance while ensuring the buoyancy support function.

[0003] The prior art discloses buoyancy materials with polyurethane as the matrix and hollow glass microspheres as the filler, but the problem solved is to reduce the water absorption rate. At the same time, polyurethane can form an elastomeric matrix with excellent damping properties. However, due to its low rigidity, it is difficult to maintain a small deformation under high pressure environment (such as deep sea environment), so it is not suitable to be used as a matrix alone for buoyancy materials. Traditional buoyancy materials with epoxy resin as the matrix cannot achieve satisfactory results due to the brittleness and high cross-linking degree of its matrix material.

[0004] Therefore, it is very important to develop a buoyancy material that combines the effects of damping properties and rigidity. Summary of the invention

[0005] In view of this, the technical problem to be solved by the high damping solid buoyancy material of the present invention is to provide a high damping solid buoyancy material, which has both damping characteristics and rigidity effects.

[0006] The present invention provides a high-damping solid buoyancy material, comprising the following raw materials in parts by weight:

[0007] 100 parts of polyether polyol;

[0008] 1 to 5 parts of trimethylolpropane;

[0009] 70-130 parts of diphenylmethane diisocyanate;

[0010] 20-90 parts of methyl methacrylate;

[0011] 0.1 to 5 parts of azobisisobutyronitrile;

[0012] 20 to 150 parts of hollow glass microspheres.

[0013] Preferably, the high damping solid buoyancy material comprises the following raw materials in parts by weight:

[0014] 100 parts of polyether polyol;

[0015] 2-4 parts of trimethylolpropane;

[0016] 80-120 parts of diphenylmethane diisocyanate;

[0017] 30-80 parts of methyl methacrylate;

[0018] 0.2-4.0 parts of azobisisobutyronitrile;

[0019] 30-120 parts of hollow glass microspheres.

[0020] Preferably, the high damping solid buoyancy material comprises the following raw materials in parts by weight:

[0021] 100 parts of polyether polyol;

[0022] 3 parts of trimethylolpropane;

[0023] 110 parts of diphenylmethane diisocyanate;

[0024] 40 parts of methyl methacrylate;

[0025] 0.5 parts of azobisisobutyronitrile;

[0026] 80 parts of hollow glass microspheres.

[0027] Preferably, the density of the hollow glass microspheres is in the range of 0.1 to 0.6 g / cm 3

[0028] Preferably, the average functionality of the polyether polyol is 3-4.

[0029] The present invention provides a method for preparing a high-damping solid buoyancy material according to any one of the above technical solutions, comprising the following steps:

[0030] A) mixing polyether polyol, trimethylolpropane and methyl methacrylate, adding into a stirring device, heating and stirring under vacuum;

[0031] B) adding diphenylmethane diisocyanate and hollow glass microspheres into a stirring device, and heating and stirring under vacuum;

[0032] C) adding azobisisobutyronitrile to a stirring device, heating and stirring under vacuum to obtain a mixed material;

[0033] D) The mixed material is placed in a mold, heated and solidified, and cooled to obtain the product.

[0034] Preferably, in step A), the vacuum degree is -0.08 to -0.1 MPa; the heating temperature is 30 to 50° C., and the stirring time is 10 to 20 min.

[0035] Preferably, the vacuum degree of step B) is -0.08 to -0.1 MPa; the heating temperature is 30 to 50° C., and the stirring time is 10 to 20 min;

[0036] Step C) the vacuum degree is -0.08 to -0.1 MPa; the heating temperature is 30 to 50°C, and the stirring time is 5 to 10 minutes;

[0037] Preferably, in step D), the mold needs to be preheated at a temperature of 80 to 120° C., the temperature of the heating curing is 80 to 120° C., and the time is 0.5 to 24 hours; and the cooling is cooling to below 70° C.

[0038] The present invention provides a diving device, the raw materials of which include the material described in any one of the above technical solutions.

[0039] Compared with the prior art, the present invention provides a high-damping solid buoyancy material, comprising the following raw materials in parts by weight: 100 parts of polyether polyol; 1 to 5 parts of trimethylolpropane; 70 to 130 parts of diphenylmethane diisocyanate; 20 to 90 parts of methyl methacrylate; 0.1 to 5 parts of azobisisobutyronitrile; 20 to 150 parts of hollow glass microspheres. The present invention adopts a technical route of using polyurethane / polymethyl methacrylate blended polymer as a matrix and hollow glass microspheres as lightweight pressure-resistant fillers. The polyurethane / polymethyl methacrylate blended polymer has an interpenetrating network structure, and has high damping properties and good stiffness; the hollow glass microspheres reduce the density of the material on the basis of ensuring the pressure-resistant properties, so that it has buoyancy properties. The solid buoyancy material product finally formed has the characteristics of light weight, pressure resistance and high damping, meeting the use requirements of submersibles and submarines. DETAILED DESCRIPTION

[0040] The present invention provides a high damping solid buoyancy material and a preparation method thereof. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0041] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0042] The present invention provides a high-damping solid buoyancy material, comprising the following raw materials in parts by weight:

[0043] 100 parts of polyether polyol;

[0044] 1 to 5 parts of trimethylolpropane;

[0045] 70-130 parts of diphenylmethane diisocyanate;

[0046] 20-90 parts of methyl methacrylate;

[0047] 0.1 to 5 parts of azobisisobutyronitrile;

[0048] 20 to 150 parts of hollow glass microspheres.

[0049] The high damping solid buoyancy material provided by the present invention comprises 100 parts by weight of polyether polyol; the average functionality of the polyether polyol is 3 to 4

[0050] The high damping solid buoyancy material provided by the present invention comprises 1 to 5 parts by weight of trimethylolpropane; specifically, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight or 5 parts by weight; or a range value between any two of the above.

[0051] The high damping solid buoyancy material provided by the present invention comprises 70 to 130 parts by weight of diphenylmethane diisocyanate; specifically, it can be 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, 120 parts by weight or 130 parts by weight; or a range value between any two of the above.

[0052] The high damping solid buoyancy material provided by the present invention comprises 20 to 90 parts by weight of methyl methacrylate; specifically, it can be 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight or 90 parts by weight; or a range value between any two of the above.

[0053] The high damping solid buoyancy material provided by the present invention comprises 0.1 to 5 parts by weight of azobisisobutyronitrile; specifically, it can be 0.1 parts by weight, 0.3 parts by weight, 0.5 parts by weight, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight or 5 parts by weight; or a range value between any two of the above.

[0054] The high damping solid buoyancy material provided by the present invention comprises 20 to 150 parts by weight of hollow glass microspheres, which may be 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight or 150 parts by weight, or a range between any two of the above.

[0055] The density of the hollow glass microspheres is in the range of 0.1 to 0.6 g / cm 3

[0056] The present invention synthesizes polyurethane from isocyanate and polyether polyol; and synthesizes polymethyl methacrylate from methyl methacrylate and azobisisobutyronitrile. The buoyancy material comprises PU / PMMA, which is a mixed copolymer of the above-mentioned polyurethane PU and polymethyl methacrylate PMMA, as a matrix and hollow glass microspheres as fillers. The main problem to be solved is to prepare a buoyancy material having both damping performance (mainly provided by PU) and rigidity (mainly provided by PMMA and hollow glass microspheres). The innovation of the present invention is reflected in the use of PU / PMMA blended polymer as the matrix of the buoyancy material; the creativity is reflected in the fact that the PU / PMMA blended polymer forms an interpenetrating network structure, giving play to their respective advantages, and achieving the beneficial effect of making the final product have both damping properties and rigidity.

[0057] In some preferred embodiments of the present invention, the high damping solid buoyancy material comprises the following raw materials in parts by weight:

[0058] 100 parts of polyether polyol;

[0059] 2-4 parts of trimethylolpropane;

[0060] 80-120 parts of diphenylmethane diisocyanate;

[0061] 30-80 parts of methyl methacrylate;

[0062] 0.2-4.0 parts of azobisisobutyronitrile;

[0063] 30-120 parts of hollow glass microspheres.

[0064] In a preferred embodiment of the present invention, the high damping solid buoyancy material comprises the following raw materials in parts by weight:

[0065] 100 parts of polyether polyol;

[0066] 3 parts of trimethylolpropane;

[0067] 110 parts of diphenylmethane diisocyanate;

[0068] 40 parts of methyl methacrylate;

[0069] 0.5 parts of azobisisobutyronitrile;

[0070] 80 parts of hollow glass microspheres.

[0071] After the polymer components of the present invention are mixed and reacted, a polyurethane / polymethyl methacrylate blend polymer matrix is ​​formed, which has the characteristics of high damping; the hollow glass microspheres play the role of reducing density and ensuring rigidity. The damping coefficient (loss factor) of the solid buoyancy material can reach more than 0.1, and it has the functions of low density, high pressure resistance, sound insulation, vibration reduction, and impact resistance, and can be applied to submersibles, submarines, etc.

[0072] The present invention provides a method for preparing a high-damping solid buoyancy material according to any one of the above technical solutions, comprising the following steps:

[0073] A) mixing polyether polyol, trimethylolpropane and methyl methacrylate, adding into a stirring device, heating and stirring under vacuum;

[0074] B) adding diphenylmethane diisocyanate and hollow glass microspheres into a stirring device, and heating and stirring under vacuum;

[0075] C) adding azobisisobutyronitrile to a stirring device, heating and stirring under vacuum to obtain a mixed material;

[0076] D) The mixed material is placed in a mold, heated and solidified, and cooled to obtain the product.

[0077] The present invention has clearly described the components and proportions of the above raw materials above, which will not be repeated here.

[0078] The preparation method of the high damping solid buoyancy material provided by the invention firstly mixes polyether polyol, trimethylolpropane and methyl methacrylate, adds them into a stirring device, and then heats and stirs them in vacuum.

[0079] The present invention does not limit the stirring device, including but not limited to a stirring kettle.

[0080] The vacuum degree is -0.08 to -0.1 MPa; the heating temperature is 30 to 50° C., more preferably 35 to 45° C.; the stirring time is 10 to 20 minutes, specifically 10 minutes, 15 minutes or 20 minutes.

[0081] Add diphenylmethane diisocyanate and hollow glass microspheres into a stirring device and heat and stir under vacuum.

[0082] The vacuum degree is -0.08 to -0.1 MPa; the heating temperature is 30 to 50° C., more preferably 35 to 45° C.; the stirring time is 10 to 20 min, specifically 10 min, 15 min or 20 min.

[0083] Add azobisisobutyronitrile into a stirring device, heat and stir under vacuum to obtain a mixed material.

[0084] The vacuum degree is -0.08 to -0.1 MPa; the heating temperature is 30 to 50°C, more preferably 35 to 45°C; the stirring time is 5 to 10 minutes, specifically 5 minutes, 8 minutes or 10 minutes.

[0085] The mixed material is placed in a mold, heated and solidified, and cooled to obtain the product.

[0086] Transfer the mixed material into the preheated mold.

[0087] The mold needs to be preheated, and the preheating temperature is 80-120° C., specifically 80° C., 90° C., 100° C., 110° C., 120° C.; or a range between any two of the above.

[0088] The mold is placed in a static state and heated to cure. The temperature for heating and curing is 80-120°C, specifically 80°C, 90°C, 100°C, 110°C, 120°C, or any range between the above two.

[0089] The time is 0.5 to 24 hours; specifically, the time is 0.5 hours, 1 hour, 2 hours, 5 hours, 10 hours, 15 hours, 18 hours, 20 hours or 24 hours; or a range between any two of the above.

[0090] After cooling, the material is removed from the mold to obtain a high-damping solid buoyancy material. The cooling is cooling to below 70°C.

[0091] The present invention provides a diving device, the raw materials of which include the materials described in any one of the above technical solutions. The diving device of the present invention includes but is not limited to a submersible or a submarine.

[0092] The present invention provides a high-damping solid buoyancy material, comprising the following raw materials in parts by weight: 100 parts of polyether polyol; 1 to 5 parts of trimethylolpropane; 70 to 130 parts of diphenylmethane diisocyanate; 20 to 90 parts of methyl methacrylate; 0.1 to 5 parts of azobisisobutyronitrile; 20 to 150 parts of hollow glass microspheres. The present invention adopts a technical route of using polyurethane / polymethyl methacrylate blended polymer as a matrix and hollow glass microspheres as lightweight pressure-resistant fillers. The polyurethane / polymethyl methacrylate blended polymer has an interpenetrating network structure, and has high damping properties and good rigidity; the hollow glass microspheres reduce the density of the material on the basis of ensuring the pressure-resistant properties, so that it has buoyancy properties. The solid buoyancy material product finally formed has the characteristics of light weight, pressure resistance and high damping, and meets the use requirements of submersibles and submarines.

[0093] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0094] The numerical ranges and parameters involved in the present invention have presented the relevant numerical values ​​in the specific embodiments as accurately as possible. However, any numerical value essentially inevitably contains standard deviations due to individual testing methods. Therefore, unless otherwise explicitly stated, it should be understood that all numerical ranges or specific data used in this disclosure may have certain reasonable deviations within a certain range, for example: within 1% or 0.5%.

[0095] Some cases are recorded in the embodiments and comparative examples of the present invention, wherein the embodiments show certain implementation modes of the present invention. However, this does not mean that the effects of the present invention can only be achieved in these cases.

[0096] In order to further illustrate the present invention, a high damping solid buoyancy material and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments.

[0097] Embodiment 1:

[0098] 5 kg of polyether polyol, 150 g of trimethylolpropane, and 2 kg of methyl methacrylate were added to a stirred kettle and stirred for 10 minutes at 45 degrees Celsius under vacuum. 5.5 kg of diphenylmethane diisocyanate, 4 kg of diphenylmethane with a true density of 0.46 g / cm 3 The hollow glass microspheres are added to a stirring kettle and stirred at 45 degrees Celsius under vacuum for 15 minutes. 25 g of azobisisobutyronitrile is added to a stirring kettle and stirred at 45 degrees Celsius under vacuum for 5 minutes. The mixed material is moved into a mold preheated to 90 degrees Celsius, and the mold is placed at a constant temperature of 110 degrees Celsius for 2 hours. When the material is solidified and cooled to below 50 degrees Celsius, the material is removed from the mold to obtain a high damping buoyancy material product based on PU / PMMA blended polymer.

[0099] Comparative Example 1:

[0100] Add 6.5 kg epoxy resin and 6 kg methyltetrahydrophthalic anhydride into a stirred kettle and stir for 10 minutes at 50 degrees Celsius under vacuum. 3The hollow glass microspheres are added to the stirring kettle and stirred at 50 degrees Celsius under vacuum for 15 minutes. 90g of DMP-30 accelerator is added to the stirring kettle and stirred at 50 degrees Celsius under vacuum for 5 minutes. The mixed materials are transferred into a mold, and the mold is placed at a constant temperature of 140 degrees Celsius for 6 hours. When the material is solidified and cooled to below 50 degrees Celsius, the material is removed from the mold to obtain a buoyancy material product based on epoxy resin.

[0101] Comparative Example 2:

[0102] 6 kg of polyether polyol, 300 g of trimethylolpropane and 6.5 kg of diphenylmethane diisocyanate were added into a stirred kettle and stirred for 5 minutes at 40 degrees Celsius under vacuum. 3 The hollow glass microspheres are added into a stirring kettle and stirred for 10 minutes at 40 degrees Celsius under vacuum. The uniformly mixed material is transferred into a mold, and the mold is placed in a constant temperature environment of 80 degrees Celsius for 6 hours. When the material is solidified and cooled to below 50 degrees Celsius, the material is removed from the mold to obtain a buoyancy material product with polyurethane as the matrix.

[0103] The density, elastic modulus and damping coefficient (loss factor) of the products in the embodiments and comparative examples were tested, and the following Table 1 was obtained:

[0104] Table 1

[0105]

[0106] From the above comparison, it can be seen that: at the same density, (1) Example 1 (buoyancy material based on PU / PMMA blended polymer) has greatly improved the damping coefficient while maintaining most of the compressive strength and stiffness (elastic modulus) compared to Comparative Example 1 (buoyancy material based on epoxy resin), and is suitable for sound insulation, vibration reduction and impact resistance; (2) Compared with Comparative Example 2 (buoyancy material based on polyurethane PU), the embodiment has higher compressive strength and stiffness (elastic modulus) on the basis of having a similar damping coefficient, and is suitable for the high-pressure environment of the deep sea.

[0107] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high damping solid buoyancy material, It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of polyether polyol; 1 to 5 parts of trimethylolpropane; 70-130 parts of diphenylmethane diisocyanate; 20-90 parts of methyl methacrylate; 0.1 to 5 parts of azobisisobutyronitrile; 20 to 150 parts of hollow glass microspheres.

2. The material according to claim 1, It is characterized in that The high damping solid buoyancy material comprises the following raw materials in parts by weight: 100 parts of polyether polyol; 2-4 parts of trimethylolpropane; 80-120 parts of diphenylmethane diisocyanate; 30-80 parts of methyl methacrylate; 0.2-4.0 parts of azobisisobutyronitrile; 30-120 parts of hollow glass microspheres.

3. The material according to claim 2, It is characterized in that The high damping solid buoyancy material comprises the following raw materials in parts by weight: 100 parts of polyether polyol; 3 parts of trimethylolpropane; 110 parts of diphenylmethane diisocyanate; 40 parts of methyl methacrylate; 0.5 parts of azobisisobutyronitrile; 80 parts of hollow glass microspheres.

4. The material according to any one of claims 1 to 3, It is characterized in that The density of the hollow glass microspheres is in the range of 0.1 to 0.6 g / cm 3 .

5. The material according to any one of claims 1 to 3, It is characterized in that The average functionality of the polyether polyol is 3-4.

6. A method for preparing the high damping solid buoyancy material according to any one of claims 1 to 5, It is characterized in that The steps include: A) adding polyether polyol, trimethylolpropane and methyl methacrylate into a stirring device and heating under vacuum and stirring; B) adding diphenylmethane diisocyanate and hollow glass microspheres into a stirring device, and heating and stirring under vacuum; C) adding azobisisobutyronitrile to a stirring device, heating and stirring under vacuum to obtain a mixed material; D) The mixed material is placed in a mold, heated and solidified, and cooled to obtain the product.

7. The preparation method according to claim 6, It is characterized in that Step A): the vacuum degree is -0.08 to -0.1 MPa; the heating temperature is 30 to 50° C., and the stirring time is 10 to 20 min.

8. The preparation method according to claim 6, It is characterized in that The vacuum degree of step B) is -0.08 to -0.1 MPa; the heating temperature is 30 to 50°C, and the stirring time is 10 to 20 minutes; Step C) The vacuum degree is -0.08 to -0.1 MPa; the heating temperature is 30 to 50° C., and the stirring time is 5 to 10 minutes.

9. The preparation method according to claim 6, It is characterized in that Step D) the mold needs to be preheated, the preheating temperature is 80-120°C, the heating curing temperature is 80-120°C, and the time is 0.5-24h; the cooling is cooling to below 70°C.

10. A diving device, It is characterized in that The raw material includes the material according to any one of claims 1 to 5.

Citation Information

Cited By

  • High-strength and high-damping solid buoyancy material based on interpenetrating network structure and preparation method of high-strength and high-damping solid buoyancy material

    CN120535917A

  • Functionalized hollow filler-based damping solid buoyancy material and preparation method thereof

    CN122563275A

  • A high-damping sound-absorbing polyurea-based solid buoyancy material and its preparation method

    CN122726658A