Ink varnish as well as preparation method and application thereof
By combining cellulose resin and other additives, high stability ink oil was prepared, which solved the problem of existing ink oil settling and poor storage stability at high temperatures, and achieved stability at room temperature and high temperatures and enhance adhesion, suitable for tempered glass ink.
Patent Information
- Application Number
- CN202411239202.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
AI Technical Summary
The existing ink oil is prone to settle and coarse in high-temperature storage environments, difficult to disperse, and has poor storage stability, requiring low temperature conditions, and cannot be dispersed again through conventional dispersion machines.
Using cellulose resins, especially the combination of hydroxyethyl cellulose and hydroxypropyl methyl cellulose, combined with an appropriate amount of dispersant, defoaming agent and leveling agent, uniformly stirring through specific heating and cooling processes. Ink oil improves storage stability and adds ink oil to the ink to improve adhesion and sintering performance.
The storage stability of ink-adjusting oil at room temperature and high temperature is achieved, and can be redispersed by manual stirring. It is suitable for oily and water-based systems, improves the ease of use and adhesion of ink, and does not affect the sintering performance of tempered ink.
Smart Images

Figure BDA0005028701710000071 
Figure BDA0005028701710000081 
Figure BDA0005028701710000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of varnishing oil, in particular to the field of IPCC09D11, and more specifically to a varnishing oil and a preparation method and application thereof. Background Art
[0002] Varnish is widely used in various ink products. The current varnish products on the market are divided into the following categories: acrylic, cellulose, aldehydes and ketones, and epoxy vinyl. The production method is to use the above resin as the main body and formulate it with other various additives. However, there are common problems with storage stability in the current products on the market, which are mainly manifested in easy sedimentation and coarsening, and difficulty in dispersion. A large amount of hard sediment appears at the bottom of the packaging barrel, especially in high-temperature storage environments. This phenomenon is more obvious and cannot be dispersed again by using a dispersing / stirring machine. All currently available products require manufacturers to have low-temperature storage conditions.
[0003] CN107964275A discloses a water-based environmentally friendly ink varnish for tempered glass, which belongs to the field of new materials; it is composed of the following raw materials in mass percentage: water: 1-95%, environmentally friendly solvent: 0-95%, film former: 0.1-5%, defoamer: 0.1-2%, wetting dispersant: 0.1-5%, leveling agent: 0.1-2%, adhesive: 2-30%, anti-settling agent: 1-10%. The water-based ink varnish of the present invention uses water as the basic solvent, which is economical and environmentally friendly; it has good dispersibility with inorganic glass pigments, the ink film is smooth and bright, resistant to low temperature weather, and has good leveling properties; equipment, tools, containers, floors, clothes, etc. that come into contact with the ink can be cleaned with tap water. However, the ink varnish made of the above-mentioned types of resins does not involve solving the problem of the storage stability of the ink under natural storage conditions or hot storage experimental conditions. Summary of the invention
[0004] The first aspect of the present invention provides a varnish, which comprises, by weight, 0.5-3 parts of cellulose, 0.1-1 parts of a dispersant, 0.1-1 parts of a defoamer, 0.05-0.1 parts of a leveling agent and 5-30 parts of a solvent.
[0005] The cellulose includes hydroxyethyl cellulose and hydroxypropyl methyl cellulose, and the weight ratio of the hydroxyethyl cellulose to the hydroxypropyl methyl cellulose is (0.4-1.2): (0.4-0.8).
[0006] Preferably, the cellulose comprises hydroxyethyl cellulose and hydroxypropyl methyl cellulose, and the weight ratio of the hydroxyethyl cellulose to the hydroxypropyl methyl cellulose is 1:(0.5-1.2).
[0007] Further preferably, the cellulose comprises hydroxyethyl cellulose and hydroxypropyl methyl cellulose, and the weight ratio of the hydroxyethyl cellulose to the hydroxypropyl methyl cellulose is 1:(0.7-0.9).
[0008] The applicant has found that the cellulose includes hydroxyethyl cellulose and hydroxypropyl methyl cellulose, and the weight ratio of hydroxyethyl cellulose and hydroxypropyl methyl cellulose is (0.4-1.2): (0.4-0.8), which can improve the storage stability at room temperature and high temperature, and will not affect the sintering performance of tempered ink. Hydroxyethyl cellulose and hydroxypropyl methyl cellulose both have excellent water solubility, but their viscosity characteristics are different. Hydroxyethyl cellulose dissolves quickly at high temperatures, and its viscosity is more sensitive to temperature, while the viscosity of hydroxypropyl methyl cellulose is relatively stable. It may be the high viscosity of hydroxypropyl methyl cellulose and the viscosity stability of hydroxyethyl cellulose that achieve a better rheological control effect.
[0009] The viscosity of the hydroxyethyl cellulose at 20° C. is 2-10 cP.
[0010] Preferably, the viscosity of the hydroxyethyl cellulose at 20° C. is 2-6 cP.
[0011] The viscosity of the hydroxypropyl methylcellulose at 20° C. is 200-1000 cP.
[0012] Preferably, the viscosity of the hydroxypropyl methylcellulose at 20° C. is 200-600 cP.
[0013] The weight ratio of the dispersant, defoamer and leveling agent is (0.2-0.6): (0.2-0.8): (0.1-0.6).
[0014] Preferably, the weight ratio of the dispersant, defoamer and leveling agent is (0.3-0.5): (0.2-0.4): (0.3-0.6).
[0015] The solvent includes at least one of terpineol, dimethyl nylonate, ethylene glycol, dimethylformamide, ethylene glycol monomethyl ether, diethylene glycol butyl ether, and N-methylpyrrolidone.
[0016] Preferably, the solvent includes at least one of diethylene glycol butyl ether and terpineol.
[0017] The second aspect of the present invention provides a method for preparing varnish, comprising the following steps: heating a solvent to 90-100°C, adding cellulose into the solvent for heating and dissolving; after cooling, adding a dispersant, a defoaming agent and a leveling agent, and stirring evenly to obtain the varnish.
[0018] A third aspect of the present invention provides an application of varnish oil for screen printing ink.
[0019] Preferably, the ink is applied to one of automotive glass and photovoltaic glass.
[0020] The amount of the varnish added to the ink is 5-50wt%.
[0021] Preferably, the amount of the varnish added to the ink is 10-40wt%.
[0022] The ink also includes glass powder and pigment with a melting point of 350-550°C.
[0023] Preferably, the ink comprises, by weight: 10-30 parts of varnish, 50-70 parts of glass powder having a melting point of 350-550° C., and 15-35 parts of pigment.
[0024] Preferred pigments include copper chrome black.
[0025] Beneficial Effects
[0026] 1. The varnish prepared in the present application has excellent printing properties, and the ink produced can be stored at room temperature, has low requirements for the ink storage environment, and has excellent storage stability.
[0027] 2. The ink varnish prepared in the present application can be stable without sedimentation or coarsening under the conditions of hot storage experiments, and the ink can be redispersed by manual stirring, thereby improving the ease of use of the ink.
[0028] 3. The ink varnish of this application is applied to tempered glass to improve adhesion and solve the problem of product fading during transportation.
[0029] 4. The ink varnish of the present application is applied to tempered glass without affecting the sintering performance of the tempered ink. There is basically no residue after decomposition. The low-temperature (550-640°C) and high-temperature (650-720°C) inks produced have good performance after sintering.
[0030] 5. The ink varnish prepared in this application can be applied to both oily and water-based systems. DETAILED DESCRIPTION
[0031] Example 1
[0032] A varnish, comprising the following components by weight:
[0033] 0.8 parts of hydroxyethyl cellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 4-5 cP);
[0034] 0.6 parts of hydroxypropyl methylcellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 300-500 cP);
[0035] Dispersant 0.3 parts, BYK-2015;
[0036] Defoaming agent 0.2 parts, BYK-055;
[0037] 0.3 parts of leveling agent, BYK-354;
[0038] 17.8 parts of diethylene glycol butyl ether, Dow Chemical, USA;
[0039] A method for preparing varnish oil comprises the following steps:
[0040] 1. Add diethylene glycol butyl ether into the reactor according to the formula and heat to 95°C under stirring;
[0041] 2. Under stirring, add hydroxyethyl cellulose and hydroxypropyl methyl cellulose into the reaction kettle in turn and heat to dissolve for 2 hours;
[0042] 3. After the cellulose is completely dissolved, cool it to room temperature, add the dispersant, defoamer and leveling agent into the cooled reactor in turn, stir at a constant speed for 30 minutes, and stir evenly to obtain the ink oil.
[0043] An application of varnish oil is applied to ink for tempered glass. The ink for tempered glass has the following components in parts by weight:
[0044] 20 parts of varnish;
[0045] 60 parts of low melting point glass powder, with a melting point of 480°C;
[0046] Copper chrome black 20 parts, American Shet 1G;
[0047] The method for preparing the ink for tempered glass comprises the following steps: putting materials into a stirring kettle in sequence, stirring them evenly, and grinding them with a three-roll mill until the fineness is less than 5 μm.
[0048] Example 2
[0049] A varnish, comprising the following components by weight:
[0050] 1.0 part of hydroxyethyl cellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 4-5 cP);
[0051] 0.8 parts of hydroxypropyl methylcellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 300-500 cP);
[0052] Dispersant 0.4 parts, BYK-2015;
[0053] 0.3 parts of defoamer, BYK-055;
[0054] 0.3 parts of leveling agent, BYK-354;
[0055] 17.2 parts of diethylene glycol butyl ether, Dow Chemical, USA;
[0056] A method for preparing varnish oil comprises the following steps:
[0057] 1. Add diethylene glycol butyl ether into the reactor according to the formula and heat to 95°C under stirring;
[0058] 2. Under stirring, add hydroxyethyl cellulose and hydroxypropyl methyl cellulose into the reaction kettle in turn and heat to dissolve for 2 hours;
[0059] 3. After the cellulose is completely dissolved, cool it to room temperature, add the dispersant, defoamer and leveling agent into the cooled reactor in turn, stir at a constant speed for 30 minutes, and stir evenly to obtain the ink oil.
[0060] An application of varnish oil is applied to ink for tempered glass. The ink for tempered glass has the following components in parts by weight:
[0061] 20 parts of varnish;
[0062] 60 parts of low melting point glass powder, with a melting point of 480°C;
[0063] Copper chrome black 20 parts, American Shet 1G;
[0064] The method for preparing the ink for tempered glass comprises the following steps: putting materials into a stirring kettle in sequence, stirring them evenly, and grinding them with a three-roll mill until the fineness is less than 5 μm.
[0065] Example 3
[0066] A varnish, comprising the following components by weight:
[0067] 0.5 parts of hydroxyethyl cellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 4-5 cP);
[0068] 0.4 parts of hydroxypropyl methylcellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 300-500 cP);
[0069] Dispersant 0.5 parts, BYK-2015;
[0070] 0.4 parts of defoamer, BYK-055;
[0071] 0.5 parts of leveling agent, BYK-354;
[0072] 17.7 parts of diethylene glycol butyl ether, Dow Chemical, USA;
[0073] A method for preparing varnish oil comprises the following steps:
[0074] 1. Add diethylene glycol butyl ether into the reactor according to the formula and heat to 95°C under stirring;
[0075] 2. Under stirring, add hydroxyethyl cellulose and hydroxypropyl methyl cellulose into the reaction kettle in turn and heat to dissolve for 2 hours;
[0076] 3. After the cellulose is completely dissolved, cool it to room temperature, add the dispersant, defoamer and leveling agent into the cooled reactor in turn, stir at a constant speed for 30 minutes, and stir evenly to obtain the ink oil.
[0077] An application of varnish oil is applied to ink for tempered glass. The ink for tempered glass has the following components in parts by weight:
[0078] 20 parts of varnish;
[0079] 60 parts of low melting point glass powder, with a melting point of 480°C;
[0080] Copper chrome black 20 parts, American Shet 1G;
[0081] The method for preparing the ink for tempered glass comprises the following steps: putting materials into a stirring kettle in sequence, stirring them evenly, and grinding them with a three-roll mill until the fineness is less than 5 μm.
[0082] Example 4
[0083] A varnish, comprising the following components by weight:
[0084] 1.0 part of hydroxyethyl cellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 4-5 cP);
[0085] 0.2 parts of hydroxypropyl methylcellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 300-500 cP);
[0086] Dispersant 0.2 parts, BYK-2015;
[0087] Defoaming agent 0.2 parts, BYK-055;
[0088] 0.3 parts of leveling agent, BYK-354;
[0089] 18.1 parts of terpineol, Jiangxi Huajin;
[0090] A method for preparing varnish oil comprises the following steps:
[0091] 1. Add terpineol into the reactor according to the formula and heat to 95°C under stirring;
[0092] 2. Under stirring, add hydroxyethyl cellulose and hydroxypropyl methyl cellulose into the reaction kettle in turn and heat to dissolve for 2 hours;
[0093] 3. After the cellulose is completely dissolved, cool it to room temperature, add the dispersant, defoamer and leveling agent into the cooled reactor in turn, stir at a constant speed for 30 minutes, and stir evenly to obtain the ink oil.
[0094] An application of varnish oil is applied to ink for tempered glass. The ink for tempered glass has the following components in parts by weight:
[0095] 20 parts of varnish;
[0096] 60 parts of low melting point glass powder, with a melting point of 480°C;
[0097] Copper chrome black 20 parts, American Shet 1G;
[0098] The method for preparing the ink for tempered glass comprises the following steps: putting materials into a stirring kettle in sequence, stirring them evenly, and grinding them with a three-roll mill until the fineness is less than 5 μm.
[0099] Comparative Example 1
[0100] A varnish, comprising the following components by weight:
[0101] 1 part of alcohol-soluble acrylic resin, Guangzhou Changhao Trading Co., Ltd. (SGR-7120);
[0102] 0.3 parts of polyamide wax paste, Desbaron (6900-20X);
[0103] 0.2 parts of neutralizer, American Dow AMP-95;
[0104] Dispersant 0.3 parts, BYK-2015;
[0105] Defoaming agent 0.2 parts, BYK-055;
[0106] 0.3 parts of leveling agent, BYK-354;
[0107] 17.8 parts of diethylene glycol butyl ether, Dow Chemical, USA;
[0108] A method for preparing varnish oil comprises the following steps:
[0109] 1. Add diethylene glycol butyl ether into the reactor according to the formula and heat to 95°C under stirring;
[0110] 2. Under stirring, add alcohol-soluble acrylic resin and polyamide wax slurry into the reaction kettle in turn and heat to dissolve for 2 hours;
[0111] 3. After dissolution is complete, cool to room temperature, add neutralizer, dispersant, defoamer and leveling agent into the cooled reactor in turn, stir at a constant speed for 30 minutes, and stir evenly to obtain varnish.
[0112] An application of varnish oil is applied to ink for tempered glass. The ink for tempered glass has the following components in parts by weight:
[0113] 20 parts of varnish;
[0114] 60 parts of low melting point glass powder, with a melting point of 480°C;
[0115] Copper chrome black 20 parts, American Shet 1G;
[0116] The method for preparing the ink for tempered glass comprises the following steps: putting materials into a stirring kettle in sequence, stirring them evenly, and grinding them with a three-roll mill until the fineness is less than 5 μm.
[0117] Comparative Example 2
[0118] A varnish, comprising the following components by weight:
[0119] 2 parts of aldehyde-ketone resin, Jinan Yuantiao Aldehyde-Ketone Resin Co., Ltd. (KR80F);
[0120] 0.1 part of hydroxypropyl methylcellulose, Taian Ruitai Cellulose Co., Ltd. (viscosity 300-500 cP);
[0121] Dispersant 0.4 parts, BYK-2015;
[0122] 0.5 parts of defoamer, BYK-055;
[0123] 13.6 parts of terpineol, Jiangxi Huajin;
[0124] A method for preparing varnish oil comprises the following steps:
[0125] 1. Add terpineol into the reactor according to the formula and heat to 95°C under stirring;
[0126] 2. Under stirring, put aldehyde-ketone resin and hydroxypropyl methylcellulose into the reaction kettle in turn and heat to dissolve for 2 hours;
[0127] 3. After dissolution is complete, cool to room temperature, add dispersant and defoamer into the cooled reactor in turn, stir at a constant speed for 30 minutes, and stir evenly to obtain varnish.
[0128] An application of varnish oil is applied to ink for tempered glass. The ink for tempered glass has the following components in parts by weight:
[0129] 20 parts of varnish;
[0130] 60 parts of low melting point glass powder, with a melting point of 480°C;
[0131] Copper chrome black 20 parts, American Shet 1G;
[0132] The method for preparing the ink for tempered glass comprises the following steps: putting materials into a stirring kettle in sequence, stirring them evenly, and grinding them with a three-roll mill until the fineness is less than 5 μm.
[0133] Performance Testing Methods
[0134] The ink prepared in the example was subjected to a performance test, and the test data are listed in Table 1.
[0135] The ink prepared in the example was stored at 50°C for 30 days and then tested. The test data are listed in Table 2. Comparative Example 1-2 showed a sinking phenomenon, which is marked with "-". " / " in Table 1-2 means that the test was not performed.
[0136] Table 1
[0137]
[0138]
[0139] Table 2
[0140]
Claims
1. A varnish, It is characterized in that The components include, by weight: 0.5-3 parts of cellulose, 0.1-1 parts of dispersant, 0.1-1 parts of defoamer, 0.05-0.1 parts of leveling agent and 5-30 parts of solvent.
2. The varnish according to claim 1, It is characterized in that The cellulose includes hydroxyethyl cellulose and hydroxypropyl methyl cellulose, and the weight ratio of the hydroxyethyl cellulose to the hydroxypropyl methyl cellulose is (0.4-1.2): (0.4-0.8).
3. The varnish according to claim 2, It is characterized in that The viscosity of the hydroxyethyl cellulose at 20° C. is 2-10 cP.
4. The varnish according to claim 3, It is characterized in that The viscosity of the hydroxypropyl methylcellulose at 20° C. is 200-1000 cP.
5. The varnish according to claim 4, It is characterized in that The weight ratio of the dispersant, defoamer and leveling agent is (0.2-0.6): (0.2-0.8): (0.1-0.6).
6. The varnish according to claim 1 or 5, It is characterized in that The solvent includes at least one of terpineol, dimethyl nylonate, ethylene glycol, dimethylformamide, ethylene glycol monomethyl ether, diethylene glycol butyl ether, and N-methylpyrrolidone.
7. A method for preparing the varnish according to any one of claims 1 to 5, It is characterized in that The method comprises the following steps: heating the solvent to 90-100 DEG C, adding cellulose into the solvent for heating and dissolving; after cooling, adding a dispersant, a defoaming agent and a leveling agent, and stirring evenly to obtain the product.
8. A use of the varnish according to any one of claims 1 to 5, It is characterized in that Ink for screen printing.
9. The use of the varnish according to claim 8, It is characterized in that The amount of the varnish added to the ink is 5-50wt%.
10. The use of the varnish according to claim 9, It is characterized in that The ink also includes glass powder and pigment with a melting point of 350-550°C.