Method for extracting lithium from waste lithium battery positive electrode material through low-temperature roasting

Through the use of low-temperature roasting technology and molasses in conjunction with molasses, the problem of low lithium recovery and high energy consumption of the positive electrode material of lithium-ion batteries is solved, and efficient and low-cost lithium recycling is achieved, which avoids harmful gas emissions and improves lithium-ion recovery and Reduced process costs.

CN118996153APending Publication Date: 2024-11-22BEIJING MINING & METALLURGICAL TECH GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411118653.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the lithium recovery rate of the cathode material of lithium-ion batteries is low, has high energy consumption and high cost, and harmful gases may be generated during the roasting process, which poses a risk of environmental pollution.

Method used

Using low-temperature roasting technology, waste lithium battery positive electrode material is mixed with molasses as additives, and then calcined in an inert atmosphere. Lithium-rich filtrate is obtained through water leaching and solid-liquid separation. Lithium products are extracted using precipitant agents, and the baking temperature is controlled. At 200-450°C, avoid using acid and alkali reagents and high-value reducing agents.

Benefits of technology

The lithium recovery rate is achieved above 95%, reducing energy consumption and cost, avoiding harmful gas emissions, simple and safe process, and utilizing food industry waste, improving lithium ion recycling efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996153A_ABST
    Figure CN118996153A_ABST
Patent Text Reader

Abstract

The invention provides a method for extracting lithium from a waste lithium battery positive electrode material through low-temperature roasting, and relates to the field of resource recovery. The method for extracting lithium from the waste lithium battery positive electrode material through low-temperature roasting comprises the following steps: mixing the waste lithium battery positive electrode material with an additive, preparing into pellets, drying, and roasting in an inert atmosphere to obtain roasted balls; crushing the roasted balls to obtain roasted clinker, then leaching the roasted clinker by using water, and then carrying out first solid-liquid separation to obtain lithium-rich filtrate and leaching residues; after the lithium-rich filtrate is circularly leached for multiple times to reach the target lithium concentration, adding a precipitator, and carrying out second solid-liquid separation to obtain a lithium product; the additive comprises molasses; the roasting temperature ranges from 200 DEG C to 450 DEG C. According to the method provided by the invention, the characteristics of the food industry waste molasses and the waste lithium ion positive electrode material are utilized for mixing granulation and low-temperature roasting lithium extraction, the waste molasses is secondarily utilized, the recovery rate of lithium is improved, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of resource recovery, and in particular to a method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting. Background Art

[0002] The positive electrode of discarded lithium-ion batteries contains a large amount of recyclable valuable metal elements, of which lithium usually contains 5% to 7%. In recent years, the recovery of lithium has received more and more attention. In traditional pyrometallurgical processes, lithium usually enters the slag, and slag-making agents are required to separate the lithium later. In the typical hydrometallurgical steps at this stage, the valuable metals (lithium, nickel, cobalt and manganese) in the positive electrode materials of discarded lithium-ion batteries are completely leached-excessively metal extracted and separated, and lithium is retained in the raffinate. The lithium concentration is only 0.5 to 2 g / L. Lithium is recovered in the form of crude lithium carbonate at the end of the process, resulting in a lithium recovery rate of only about 80% and high energy consumption for lithium recovery. Therefore, prioritizing lithium extraction has become an urgent industry demand.

[0003] Invention patent CN115747494A discloses a method for extracting metallic lithium from waste lithium-ion battery positive electrode materials. The patent mixes waste lithium-ion positive electrode materials with thiourea or thiosemicarbazide, and performs roasting treatment at a temperature of 400-700°C. The roasted product is leached with water-activated weak acid to obtain a lithium salt aqueous solution. This method can achieve selective leaching of lithium, but the additives thiourea or thiosemicarbazide used in this process are expensive, which increases the cost of lithium extraction, and the roasting temperature is 400-700°C, which consumes a lot of energy.

[0004] Invention patent CN117144149A discloses a method for preferentially extracting lithium from waste lithium-ion batteries as raw materials. This method mixes waste ternary lithium-ion positive electrode materials and carbon powder, performs high-temperature roasting in a carbon dioxide atmosphere, and then extracts lithium metal preferentially through carbonization water leaching treatment. This method effectively improves the recovery rate of lithium metal, is simple in method, and has low recovery cost. However, this method uses carbon powder as an additive, and the mass ratio of positive electrode powder to carbon powder is 1:5 to 1:30, which is relatively costly; and it needs to be roasted at a temperature of 500 to 900°C for 2 to 6 hours, which has high energy consumption cost.

[0005] Invention patent CN117344155A discloses a method for preferentially extracting lithium from waste lithium-ion battery positive electrode materials, the method comprising: mixing waste lithium-ion battery positive electrode materials and plant waste residues, roasting at 500℃~600℃ to obtain a roasted product; at 20℃70℃, the roasted product is subjected to water immersion treatment to obtain a lithium-containing solution; wherein the plant waste residue is one or more of isatis plant waste residues, hawthorn plant waste residues, mint plant waste residues, forsythia plant waste residues, and citron plant waste residues, and the carbon content is greater than 35wt%. The method has a simple process and low operating cost. It does not generate waste pollution problems during the lithium extraction process, can reduce the loss rate of lithium, and improve the purity and recovery rate of lithium. However, the roasting parameters of the method are kept at 500-600℃ for 120~150min, and the energy consumption is relatively high.

[0006] Invention patent application CN109935922A discloses a method for recovering valuable metals from waste lithium-ion battery materials. The patent mixes waste lithium-ion battery positive electrode materials with low-valent sulfates such as sulfur and sulfide, performs sulfurization roasting at a temperature of 300 to 900°C, and obtains a lithium salt aqueous solution after the roasting product is soaked in water. The problem with this method is that the efficiency of lithium extraction by sulfurization is low (<90%) and the roasting process produces toxic and harmful gases SO x , further purification is required.

[0007] In summary, there is an urgent need to develop a method for preferentially extracting lithium from waste lithium-ion battery positive electrode materials with high recovery rate, low cost and low energy consumption. Summary of the invention

[0008] The purpose of this application is to provide a method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting to solve the above-mentioned problems.

[0009] To achieve the above objectives, this application adopts the following technical solutions:

[0010] A method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting, comprising:

[0011] The waste lithium battery positive electrode material is mixed with an additive to form pellets, which are then dried and calcined in an inert atmosphere to obtain calcined balls;

[0012] The roasted balls are crushed to obtain roasted clinker, and then the roasted clinker is leached with water, and then a first solid-liquid separation is performed to obtain a lithium-rich filtrate and leached residue;

[0013] After the lithium-rich filtrate reaches the target lithium concentration through multiple cycles of leaching, a precipitant is added to perform a second solid-liquid separation to obtain a lithium product;

[0014] The additive includes molasses; and the roasting temperature is 200-450°C.

[0015] Preferably, the molasses comprises one or more of beet molasses, cane molasses, grape molasses, corn molasses, invert molasses and refined molasses.

[0016] Preferably, the molasses is waste molasses with a water content of 10%-30%.

[0017] Preferably, the usage amount of the molasses is 10%-40% of the mass of the waste lithium battery positive electrode material.

[0018] Preferably, the particle size of the waste lithium battery positive electrode material is 100-300 mesh;

[0019] and / or,

[0020] The waste lithium battery positive electrode material includes one or more of lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium cobalt oxide, lithium nickel manganese oxide, and lithium nickel cobalt aluminum oxide.

[0021] Preferably, the pellets have a particle size of 5-20 mm.

[0022] Preferably, the pulverizing includes crushing and grinding, and the particle size of the roasted clinker after grinding is 100-300 meshes.

[0023] Preferably, the calcination time is 0.5-3h.

[0024] Preferably, the method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting satisfies one or more of the following conditions:

[0025] A. The solid-liquid ratio of the leaching is 20-500g / L;

[0026] B. the leaching temperature is 20-85°C;

[0027] C. the leaching is carried out under stirring conditions;

[0028] D. the leaching time is 10-120min;

[0029] E The target lithium concentration is 15-25 g / L.

[0030] Preferably, the precipitant comprises sodium carbonate and / or carbon dioxide;

[0031] and / or,

[0032] The inert atmosphere includes nitrogen atmosphere and / or argon atmosphere, and the gas flow rate is 5-100 mL / min.

[0033] Compared with the prior art, the beneficial effects of this application include:

[0034] The method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting provided by the present application does not use acid-base reagents and high-value reducing agents to achieve the purpose of preferential lithium extraction, thereby effectively reducing costs; the characteristics of food industry product molasses or waste molasses can be used to mix and granulate with waste lithium ion positive electrode materials for coordinated low-temperature roasting and lithium extraction, thereby reusing the waste molasses; the roasting temperature is low and the energy consumption is low. Compared with the existing roasting and lithium extraction technology, the roasting temperature is significantly reduced (100-400°C), effectively reducing energy consumption; the lithium recovery rate is high, molasses and positive electrode powder are mixed and granulated evenly, the molasses pyrolysis gas is in full contact with the positive electrode powder, the reduction reaction is fully carried out, the lithium ion recovery rate is effectively improved, and the lithium recovery rate of the overall process route can reach more than 95%; no harmful gases are emitted during the roasting process. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0036] Figure 1 A schematic diagram of the process flow of a method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting provided in an embodiment. DETAILED DESCRIPTION

[0037] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:

[0038] A method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting, comprising:

[0039] The waste lithium battery positive electrode material is mixed with an additive to form pellets, which are then dried and calcined in an inert atmosphere to obtain calcined balls;

[0040] The roasted balls are crushed to obtain roasted clinker, and then the roasted clinker is leached with water, and then a first solid-liquid separation is performed to obtain a lithium-rich filtrate and leached residue;

[0041] After the lithium-rich filtrate reaches the target lithium concentration through multiple cycles of leaching, a precipitant is added to perform a second solid-liquid separation to obtain a lithium product;

[0042] The additive includes molasses; and the roasting temperature is 200-450°C.

[0043] Optionally, the calcination temperature may be 200°C, 300°C, 400°C, 450°C or any value between 200-450°C.

[0044] In an alternative embodiment, the molasses includes one or more of beet molasses, cane molasses, grape molasses, corn molasses, invert molasses and refined molasses.

[0045] In an optional embodiment, the molasses is waste molasses with a water content of 10%-30%.

[0046] Optionally, the water content (mass content) of the waste molasses may be 10%, 20%, 30% or any value between 10% and 30%.

[0047] In an optional embodiment, the amount of molasses used is 10%-40% of the mass of the waste lithium battery positive electrode material.

[0048] Optionally, the usage amount of the molasses may be 10%, 15%, 20%, 25%, 30%, 35%, 40% or any value between 10% and 40% of the mass of the waste lithium battery positive electrode material.

[0049] In an optional embodiment, the particle size of the waste lithium battery positive electrode material is 100-300 mesh;

[0050] Optionally, the particle size of the waste lithium battery positive electrode material can be 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh or any value between 100-300 mesh;

[0051] and / or,

[0052] The waste lithium battery positive electrode material includes one or more of lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium cobalt oxide, lithium nickel manganese oxide, and lithium nickel cobalt aluminum oxide.

[0053] In an optional embodiment, the particle size of the pellets is 5-20 mm.

[0054] Optionally, the particle size of the pellets can be 5 mm, 10 mm, 15 mm, 20 mm or any value between 5-20 mm.

[0055] In an optional embodiment, the pulverizing includes crushing and grinding, and the particle size of the roasted clinker after grinding is 100-300 mesh.

[0056] Optionally, the particle size of the ground roasted clinker can be 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh or any value between 100-300 mesh.

[0057] In an optional embodiment, the calcination time is 0.5-3h.

[0058] Optionally, the calcination time may be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h or any value between 0.5 and 3 h.

[0059] In an optional embodiment, the method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting satisfies one or more of the following conditions:

[0060] A. The solid-liquid ratio of the leaching is 20-500g / L;

[0061] Optionally, the leaching solid-liquid ratio may be 20 g / L, 50 g / L, 100 g / L, 150 g / L, 200 g / L, 300 g / L, 400 g / L, 500 g / L or any value between 20-500 g / L;

[0062] B. the leaching temperature is 20-85°C;

[0063] Optionally, the leaching temperature may be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 85°C or any value between 20-85°C;

[0064] C. the leaching is carried out under stirring conditions;

[0065] D. the leaching time is 10-120min;

[0066] E The target lithium concentration is 15-25 g / L.

[0067] Optionally, the leaching time can be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min or any value between 10 and 120 min; the target lithium concentration can be 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L, 25 g / L or any value between 15 and 25 g / L.

[0068] In an optional embodiment, the precipitant comprises sodium carbonate and / or carbon dioxide;

[0069] and / or,

[0070] The inert atmosphere includes nitrogen atmosphere and / or argon atmosphere, and the gas flow rate is 5-100 mL / min.

[0071] Optionally, the gas flow rate can be 5mL / min, 10mL / min, 20mL / min, 30mL / min, 40mL / min, 50mL / min, 60mL / min, 70mL / min, 80mL / min, 90mL / min, 100mL / min or any value between 5-100mL / min.

[0072] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0073] Example 1

[0074] like Figure 1 As shown, this embodiment provides a method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting, and the specific steps are as follows:

[0075] Step 1: 30g of waste ternary lithium-ion positive electrode powder and 9.5g of waste sugarcane molasses are mixed evenly, granulated and dried; the pellets are placed in a crucible and placed in a tubular furnace, and roasted in a nitrogen atmosphere with a nitrogen flow rate of 10ml / min and a temperature of 450°C for 150min. After the roasting is completed, wait for the furnace temperature to cool to room temperature and take out the roasted balls;

[0076] Step 2: Grind the roasting balls to 300 meshes to obtain roasted clinker;

[0077] Step 3: adding the roasted clinker into a water leaching device, leaching at a liquid-to-solid ratio of 50 g / L, a leaching water bath temperature of 75°C, and a leaching time of 90 min, and filtering to obtain a lithium-containing leachate and a filter residue. At this time, the leaching rate of lithium in the leachate reaches 95.68%, and the leaching rates of nickel, cobalt, and manganese are 0.0002%, 0.0001%, and 0.0002%, respectively.

[0078] Example 2

[0079] This embodiment provides a method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting, and the specific steps are as follows:

[0080] Step 1: 100g of waste lithium cobalt oxide positive electrode powder and 28g of waste sugarcane molasses are mixed evenly, granulated and dried; the pellets are placed in a crucible and placed in a tubular furnace, and roasted in a nitrogen atmosphere with a nitrogen flow rate of 50ml / min and a temperature of 400°C for 120min. After the roasting is completed, wait for the furnace temperature to cool to room temperature and take out the roasted balls;

[0081] Step 2: Grind the roasting balls to 300 meshes to obtain roasted clinker;

[0082] Step 3: adding the roasted clinker into a water leaching device, leaching at a liquid-to-solid ratio of 35 g / L, a leaching water bath temperature of 45°C, and a leaching time of 120 min, and filtering to obtain a lithium-containing leaching solution and a filter residue. At this time, the leaching rate of lithium in the leaching solution reaches 96.02%, and the leaching rate of cobalt is 0.0003%.

[0083] Example 3

[0084] This embodiment provides a method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting, and the specific steps are as follows:

[0085] Step 1: 50g of waste lithium manganese oxide positive electrode powder and 17.5g of waste beet molasses are mixed evenly, granulated and then dried; the pellets are placed in a crucible and placed in a tube furnace, and roasted in a nitrogen atmosphere with a nitrogen flow rate of 20ml / min and a temperature of 400°C for 100min. After the roasting is completed, wait for the furnace temperature to cool to room temperature and take out the roasted balls;

[0086] Step 2: Grind the roasting balls to 300 meshes to obtain roasted clinker;

[0087] Step 3: adding the roasted clinker into a water leaching device, leaching at a liquid-to-solid ratio of 20 g / L, a leaching water bath temperature of 40° C., and a leaching time of 30 min, and filtering to obtain a lithium-containing leaching solution and a filter residue. At this time, the leaching rate of lithium in the leaching solution reaches more than 95%, and the leaching rate of manganese is less than 0.01%.

[0088] Example 4

[0089] This embodiment provides a method for extracting lithium from waste lithium battery positive electrode materials by low-temperature roasting, and the specific steps are as follows:

[0090] Step 1: 20g of waste ternary lithium-ion positive electrode powder and 6g of waste sugarcane molasses are mixed evenly, granulated and dried; the pellets are placed in a crucible and placed in a tubular furnace, and roasted in a nitrogen atmosphere with a nitrogen flow rate of 5ml / min and a temperature of 380°C for 180min. After the roasting is completed, wait for the furnace temperature to cool to room temperature and take out the roasted balls;

[0091] Step 2: Grind the roasting balls to 300 meshes to obtain roasted clinker;

[0092] Step 3: adding the roasted clinker into a water leaching device, leaching at a liquid-to-solid ratio of 40 g / L, a leaching water bath temperature of 25° C., and a leaching time of 90 min, and filtering to obtain a lithium-containing leachate and a filter residue. At this time, the leaching rate of lithium in the leachate reaches 97.04%, and the leaching rates of nickel, cobalt, and manganese are less than 0.0005%.

[0093] Comparative Example 1

[0094] The difference from Example 1 is that glucose is used instead of waste cane molasses.

[0095] The leaching rate of lithium in the leaching solution is 8.36%.

[0096] Comparative Example 2

[0097] The difference from Example 1 is that the calcination temperature is 700°C.

[0098] The leaching rate of lithium in the leaching solution is 94.02%.

[0099] Comparative Example 3

[0100] The difference from Example 1 is that the pelletizing is not performed but directly calcined.

[0101] The leaching rate of lithium in the leaching solution is 88.56%.

[0102] Comparative Example 4

[0103] The difference from Example 1 is that the amount of waste sugarcane molasses used is 55wt% of the waste ternary lithium ion positive electrode powder.

[0104] The leaching rate of lithium in the leaching solution is 58.66%.

[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting, characterized in that: include: The waste lithium battery positive electrode material is mixed with an additive to form pellets, which are then dried and calcined in an inert atmosphere to obtain calcined balls; The roasted balls are crushed to obtain roasted clinker, and then the roasted clinker is leached with water, and then a first solid-liquid separation is performed to obtain a lithium-rich filtrate and leached residue; After the lithium-rich filtrate reaches the target lithium concentration through multiple cycles of leaching, a precipitant is added to perform a second solid-liquid separation to obtain a lithium product; The additive includes molasses; and the roasting temperature is 200-450°C.

2. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 1, characterized in that: The molasses includes one or more of beet molasses, cane molasses, grape molasses, corn molasses, invert molasses and refined molasses.

3. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 2, characterized in that: The molasses is waste molasses with a water content of 10%-30%.

4. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 2, characterized in that: The usage amount of the molasses is 10%-40% of the mass of the waste lithium battery positive electrode material.

5. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 1, characterized in that: The particle size of the waste lithium battery positive electrode material is 100-300 mesh; and / or, The waste lithium battery positive electrode material includes one or more of lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium cobalt oxide, lithium nickel manganese oxide, and lithium nickel cobalt aluminum oxide.

6. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 1, characterized in that: The particle size of the pellets is 5-20 mm.

7. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 1, characterized in that: The pulverization includes crushing and grinding, and the particle size of the roasted clinker after grinding is 100-300 meshes.

8. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 1, characterized in that: The calcination time is 0.5-3h.

9. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to claim 1, characterized in that: One or more of the following conditions are met: A. The solid-liquid ratio of the leaching is 20-500g / L; B. the leaching temperature is 20-85°C; C. the leaching is carried out under stirring conditions; D. the leaching time is 10-120min; E The target lithium concentration is 15-25 g / L.

10. The method for extracting lithium from waste lithium battery positive electrode materials by low temperature roasting according to any one of claims 1 to 9, characterized in that: The precipitant comprises sodium carbonate and / or carbon dioxide; and / or, The inert atmosphere includes nitrogen atmosphere and / or argon atmosphere, and the gas flow rate is 5-100 mL / min.

Citation Information

Patent Citations

  • Method for recovering valuable metal from waste lithium ion battery material

    CN109935922A

  • Method for extracting metal lithium from positive electrode material of waste lithium ion battery

    CN115747494A

  • Preparation method for preferentially extracting lithium from waste ternary lithium ion battery

    CN117144149A

  • Method for preferentially extracting lithium from positive electrode material of waste lithium ion battery

    CN117344155A