Method for preparing aerogel dielectric layer by using wet process and aerogel dielectric layer

Preparation of the silica aerogel dielectric layer through wet process, solving the poor insulation environment and thermal conductivity problems in semiconductor processes, and achieving a porous structure with high resistance characteristics and low thermal conductivity. It is suitable for semiconductor processes, compatibility and scope of application wide.

CN119008513APending Publication Date: 2024-11-22CHONGQING XINLIAN MICROELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074355.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The use of low-dielectric materials in existing semiconductor processes leads to poor insulation environment, and high temperatures have a great impact on other membranes, making it difficult to effectively reduce the heat conduction effect.

Method used

The silicon dioxide aerogel dielectric layer is prepared by wet process. By coating the silica gel on the substrate and aging and modification treatment, combined with carbon dioxide supercritical drying or hot nitrogen drying, a porous structure is formed to improve the Resistance characteristics and reduced thermal conduction.

Benefits of technology

It achieves a better insulation environment and reduces thermal effects, improves the uniformity and performance of the aerogel dielectric layer, has high compatibility, does not require too much equipment modification, and has a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008513A_ABST
    Figure CN119008513A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing an aerogel dielectric layer by using a wet process and the aerogel dielectric layer, and the method comprises the following steps: providing a substrate, and coating the substrate with silicon dioxide gel to form a wet silicon dioxide gel layer; the silicon dioxide gel is a mixture comprising a silicon source, absolute ethyl alcohol and deionized water; coating the surface of the wet silicon dioxide gel layer with absolute ethyl alcohol for aging treatment, and coating the surface of the aged wet silicon dioxide gel layer with a modifier for modification treatment; and carrying out drying treatment on the treated wet silicon dioxide gel layer to obtain the silicon dioxide aerogel dielectric layer. The invention relates to an aerogel dielectric layer prepared by a method for preparing the aerogel dielectric layer by using a wet process. Preparation of the aerogel dielectric layer by using a wet-process machine has high compatibility with the existing process, and equipment transformation is not needed; the formed porous aerogel dielectric layer can effectively prevent electric leakage, can effectively reduce heat conduction, and reduces the influence of high temperature on other films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a method for preparing an aerogel dielectric layer using a wet process and the aerogel dielectric layer. Background Art

[0002] Aerogel is a porous structure formed by colloidal particles or polymers. The dielectric constant of silica aerogel is very low, only 1.008C. 2 / (N·M 2 ) (The dielectric constant of silicon dioxide itself is 3.9). The high resistance of silica aerogel can effectively prevent leakage. In addition, more than 98% of the porous material is air, so it can also effectively reduce thermal conductivity (thermal conductivity is about 0.014W / mK) and reduce the impact of high temperature on other membranes. Through doping or manufacturing with different chemicals, the original properties of silica aerogel can also be changed, such as changing the mechanical structure, hydrophilicity, and void ratio, and enhancing its own water absorption by more than 100 times its volume. This mainly depends on the different properties caused by the way the material is bonded and the force generated by the bond.

[0003] The low dielectric material used in the current import price process (12-inch 28nm logic process) is about 2.5C 2 / (N·M 2 ), if this aerogel can be used in semiconductor technology, it can achieve a better insulation environment and reduce the impact of thermal effects (thermal budget). Summary of the invention

[0004] In order to solve all or part of the problems of the above-mentioned prior art, the present invention provides a method for preparing an aerogel dielectric layer using a wet process and an aerogel dielectric layer, so as to form a silica aerogel dielectric layer through a wet process, provide a good insulation environment and reduce the influence of thermal effects.

[0005] In order to achieve the above object, the present invention provides a method for preparing an aerogel dielectric layer by a wet process, comprising the following steps:

[0006] S1. providing a substrate, coating silica gel on the substrate to form a wet silica gel layer; the silica gel is a mixture including a silicon source, anhydrous ethanol and deionized water;

[0007] S2, coating the surface of the wet silica gel layer with anhydrous ethanol for aging treatment, and coating the surface of the wet silica gel layer after aging with a modifier for modification treatment;

[0008] S3, drying the wet silica gel layer after the treatment in step S2 to obtain a silica aerogel dielectric layer. The function design of the wet process machine itself is to coat chemicals on the substrate, so it has complete functions in terms of coating uniformity, temperature control, and seconds. This application uses the advantages of the wet process machine in this aspect to form an aerogel dielectric layer, which has greater advantages in the preparation of high-performance aerogel dielectric layers. At the same time, the modification treatment helps the silica gel layer to form a porous structure, so that it can be used as various dielectric layers, which can achieve a better insulation environment and reduce the impact of thermal effects.

[0009] In step S1, before coating, the silica gel is stored in a storage tank of a wet process machine and mixed through a circulation pipeline of the wet process machine. A large amount of raw materials can be stored in the storage tank, and when the silica gel is transported through the circulation pipeline, it can be further mixed evenly, thereby improving the quality of the prepared aerogel medium layer.

[0010] In step S1, when applying the silica gel, the substrate is rotated at a speed of 300-500 rpm. The substrate is placed on a silicon wafer carrier of a wet process machine, and the rotation of the substrate is achieved by rotating the silicon wafer carrier. By selecting a suitable rotation speed, the uniformity of the wet silica gel layer can be improved.

[0011] In the step S1, when the silica gel is applied, the silica gel is applied in a swinging manner above the substrate. The silica gel application port is set at one end of the robotic arm, and the relative position of the nozzle and the substrate can be adjusted by controlling the robotic arm to swing on the substrate, thereby improving the uniformity of the wet silica gel layer.

[0012] In step S2, the aging treatment is carried out under normal pressure at a temperature of 30-48° C. This process condition is easy to implement, and can accelerate the aging process, reduce the process time, and obtain an aging effect of good quality.

[0013] In step S2, the modifier is a mixed solution of trimethylsilyl chloride, anhydrous ethanol and n-hexane, wherein the volume ratio of trimethylsilyl chloride: anhydrous ethanol: n-hexane is 1:1:8. The modifier can effectively promote the formation of a porous structure of the silica gel layer, thereby effectively reducing heat conduction.

[0014] In step S3, the drying process is carbon dioxide supercritical drying, and the temperature of the carbon dioxide supercritical drying is 200-350° C. and the pressure is 75-80 atmospheres. The carbon dioxide supercritical drying method can achieve efficient drying of the wet silica gel layer to obtain a solid silica aerogel layer with excellent performance.

[0015] In step S3, the drying process is performed by hot nitrogen, and the temperature of the hot nitrogen is 400-800° C. Hot nitrogen can also achieve rapid drying, and the process is simple and easy to implement.

[0016] In step S1, the silica gel is a mixture of ethyl orthosilicate, dimethylformamide, anhydrous ethanol and deionized water, and the pH value is adjusted to between 2 and 3 by hydrochloric acid and / or ammonia. The aerogel layer formed by this process can form a porous structure to reduce thermal conductivity.

[0017] In the silica gel, the mass ratio of ethyl orthosilicate: dimethylformamide: anhydrous ethanol: deionized water is 1:0.5:6:4.

[0018] An aerogel medium layer is prepared according to the above-mentioned method for preparing an aerogel medium layer using a wet process.

[0019] The aerogel medium layer is an interlayer medium layer, and the aerogel medium layer is a porous structure.

[0020] Compared with the prior art, the beneficial effects of the present invention mainly include the following: the wet process machine itself has good temperature control, flow control, concentration control, and chemical spraying time control, and can remove particles or impurities during the chemical transmission process, thereby providing a better manufacturing environment and parameter control, that is, the preparation of a high-performance aerogel dielectric layer can be easily achieved through the wet process machine, which is highly compatible with the existing process and does not require excessive equipment modification; silica gel can be obtained by using different raw materials, and a porous structure can be formed by combining various modifiers, so the process has a wide range of applicability and is easy to adjust; the formed aerogel dielectric layer has high resistance characteristics, which can effectively prevent leakage, and the layer is made of porous material, which can effectively reduce heat conduction and reduce the impact of high temperature on other membrane qualities. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the specific embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The present invention provides a flow chart for preparing an aerogel dielectric layer using a wet process. DETAILED DESCRIPTION

[0023] The above and other technical contents, features and effects of the present invention will be clearly presented in the following detailed description of a preferred embodiment with reference to the drawings. The directional terms mentioned in the following embodiments, such as up, down, left, right, front or back, etc., are only referenced to the directions of the attached drawings. Therefore, the directional terms used are used to illustrate and not to limit the present invention.

[0024] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.

[0025] The steps in the following embodiments do not correspond one to one with the summary of the invention.

[0026] Embodiment 1:

[0027] like Figure 1 The figure shows a flow chart of preparing an aerogel dielectric layer by a wet process provided by an embodiment of the present invention. In this embodiment, silica gel is first prepared, and then the silica gel is evenly coated on a substrate (the substrate may include various preset structures according to the different positions of the structures to be formed) using a wet process machine. During the entire preparation process, the prepared silica gel mixture is in a solution or gel state before drying, and thus can be used in a wet process. After drying, a solid silica aerogel layer is formed, which can be used in the formation of semiconductor structures, especially dielectric layer structures.

[0028] The present invention adopts a wet process machine to prepare the aerogel dielectric layer because the wet process machine is designed to coat chemicals on the substrate and has complete supporting facilities. The wet process machine has good temperature control, flow control, concentration control, and chemical spraying time control functions, and can remove particles or impurities during the chemical transmission process, so it can provide a good manufacturing environment and parameter control. The present invention does not limit the type of wet process machine used, nor does it limit the field of use of the formed silica aerogel layer. In this embodiment, the wet process machine used is a single-chip wet process machine, and the semiconductor structure formed is an ILD (interlayer dielectric layer) as an example.

[0029] The present invention provides a method for preparing an aerogel dielectric layer by a wet process and an aerogel dielectric layer, wherein the preparation method comprises the following steps:

[0030] Step 1: Prepare silica gel and place it in the wet process machine storage tank.

[0031] In this embodiment, silica gel is first prepared. The preparation method is to mix tetraethyl orthosilicate, dimethylformamide, anhydrous ethanol and deionized water, and then adjust the pH value to 2-3 with hydrochloric acid and / or ammonia water; wherein the mass ratio of tetraethyl orthosilicate: dimethylformamide: anhydrous ethanol: deionized water is 1:0.5:6:4. Then the prepared silica gel is fully mixed and added to the storage tank of the wet machine. It should be noted that the mixed solution is in a sol state at the beginning, but as the reaction proceeds, it will gradually change from a sol state to a gel state, so it can be considered that the final storage tank is silica gel, but at this time there is still a large amount of solvent, and the silica gel still has a certain fluidity and can be used in a wet machine.

[0032] In the silica gel formed above, tetraethyl orthosilicate, as a silicon source, is the basic raw material for producing silica; after adding deionized water, tetraethyl orthosilicate will undergo hydrolysis and condensation reactions to generate silanol (Si-OH) and further form silicon-oxygen bonds (Si-O-Si) through condensation reactions, ultimately forming a three-dimensional silicon-oxygen network structure, while dimethylformamide can control the hydrolysis rate and the degree of polymerization, thereby affecting the particle size and dispersion of the gel; and by adding acidic or alkaline additives, the pH value of the solution can be adjusted to control the reaction rate and stability, thereby coordinating different process times.

[0033] The present invention does not strictly limit the raw materials for forming silica gel. In other embodiments, the selected silicon source material can be one or more of methyl orthosilicate (MTMS), tetraethoxysilane (TEOS), tetramethoxysilane (TMOS), methyltrimethoxysilane, 3-aminopropyltriethoxysilane or vinyltrimethoxysilane. In this embodiment, the acidic additive used is hydrochloric acid solution. In other embodiments, the acidic additive can also use one or more of citric acid, tartaric acid, and acetic acid; the alkaline additive used is one or more of ammonia water or sodium hydroxide.

[0034] Step 2: Provide a substrate, mix the silica gel in the storage tank in step 1 through a circulation pipeline of a wet process machine, and then coat it on the substrate to form a wet silica gel layer.

[0035] The wet process machine itself is equipped with a circulation pipeline. During the coating operation, the silica gel in the storage tank will be transported to the coating port of the machine (i.e., the nozzle of the wet process machine) through the circulation pipeline. During this transportation process, the silica gel can be further fully mixed, and then the silica gel can be coated on the provided substrate through the coating port of the wet process machine. In the wet process, the substrate is placed on the silicon wafer carrier of the wet process machine. The uniformity of the silica gel coating can be further improved by the slow rotation of the silicon wafer carrier in the machine and the swing of the robotic arm (robotic arm with a coating port). The rotation speed of the silicon wafer carrier is 300-500rpm (1rpm means 1 rotation per minute).

[0036] Step 3: Anhydrous ethanol is coated on the surface of the wet silica gel layer obtained after step 2 to age the wet silica gel layer.

[0037] After step 2 is completed, anhydrous ethanol is coated on the surface of the wet silica gel layer through a wet machine and the wet silica gel layer is aged, thereby improving the mechanical strength of the wet silica gel layer. Aging treatment is an important step. Aging treatment is to let the gel stand for a long time under certain temperature and humidity conditions so that the network structure inside the wet silica gel layer can be further stabilized and homogenized. Through the aging process, the stress concentration in the wet silica gel layer can be reduced, and its mechanical strength and dimensional stability can be improved. In this embodiment, the aging process can be carried out under normal pressure, the temperature can be controlled at 30 to 48°C, and the aging time can be determined according to the process conditions.

[0038] Step 4: Modifying the aged wet silica gel layer.

[0039] Silica aerogel is a porous structure formed by colloidal particles or polymers. The porous structural characteristics are the important reasons for its high electrical resistance and low thermal conductivity. Therefore, in order to obtain a high-performance aerogel dielectric layer, the formation of a porous structure of the aerogel layer must be ensured. To this end, the above purpose can be achieved through modification treatment.

[0040] In this embodiment, after step 3 is completed, the modifier can be applied to the surface of the aged wet silica gel layer by a wet machine to modify it. In this embodiment, the modifier used is a mixed solution of trimethylchlorosilane (TMCS), anhydrous ethanol and n-hexane, wherein the volume ratio of trimethylchlorosilane: anhydrous ethanol: n-hexane is 1:1:8. By modifying the mixed solution, the properties of the wet silica gel layer can be changed, and the formation of a porous structure of the silica gel layer during drying can be effectively promoted, thereby effectively reducing heat conduction. The specific composition of the modifier can also be selected according to actual needs.

[0041] Step 5: Dry the wet silica gel layer obtained after step 4 to obtain a solid silica aerogel medium layer.

[0042] The wet silica gel layer obtained in the previous step still contains a solvent (mainly ethanol), and here the ethanol in the wet silica gel layer needs to be dried to obtain a solid silica aerogel medium layer.

[0043] In this embodiment, a carbon dioxide supercritical drying method is used to completely dry the wet silica gel layer. The temperature of carbon dioxide supercritical drying is 200-350° C. and the pressure is above 75 atmospheres, generally 75-80 atmospheres.

[0044] Supercritical drying uses the properties of supercritical fluids to replace traditional liquid solvent drying. The substrate with a wet silica gel layer formed on the surface is placed in a high-pressure and high-temperature environment of supercritical CO2 (temperature is 240°C, pressure is 80 atmospheres). In this state, CO2 has both high diffusivity and can penetrate the wet silica gel layer on the substrate, and high solubility, which can effectively dissolve the solvent (i.e. ethanol) from the wet silica gel layer, thereby removing excess ethanol in the network structure and preventing the shrinkage of the wet gel layer, and obtaining a solid silica aerogel medium layer.

[0045] In other embodiments, drying may be performed by hot nitrogen, where the temperature of the hot nitrogen is between 400-800°C.

[0046] The present invention also provides an aerogel dielectric layer, which is prepared according to the above-mentioned method for preparing an aerogel dielectric layer using a wet process. The aerogel dielectric layer can be used as various dielectric layers, such as an ILD (interlayer dielectric layer), and the aerogel dielectric layer is a porous structure. The thickness of the aerogel dielectric layer prepared by the wet process machine can at least reach the centimeter level, and in the semiconductor field, various semiconductor structures are at most 5000nm at the application level. The wet process is fully sufficient to achieve various process requirements, and has high compatibility and application range.

[0047] In order to facilitate the description, some common English nouns or letters used in the present invention are only used for exemplary reference rather than restrictive interpretation or specific usage, and the protection scope of the present invention should not be limited by their possible Chinese translations or specific letters.

[0048] It should also be noted that, in this document, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations.

Claims

1. A method for preparing an aerogel dielectric layer using a wet process, characterized in that: include: S1. providing a substrate, coating silica gel on the substrate to form a wet silica gel layer; the silica gel is a mixture including a silicon source, anhydrous ethanol and deionized water; S2, coating the surface of the wet silica gel layer with anhydrous ethanol for aging treatment, and coating the surface of the wet silica gel layer after aging with a modifier for modification treatment; S3, drying the wet silica gel layer after the treatment in step S2 to obtain a silica aerogel medium layer.

2. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In the step S1, before coating, the silica gel is stored in a storage tank of a wet process machine and mixed through a circulation pipeline of the wet process machine.

3. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In the step S1, when the silica gel is applied, the substrate is rotated at a speed of 300-500 rpm.

4. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In the step S1, when the silica gel is applied, the application is performed in a swaying manner above the substrate.

5. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In the step S2, the aging treatment is carried out under normal pressure and at a temperature of 30-48°C.

6. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In the step S2, the modifier is a mixed solution of trimethylchlorosilane, anhydrous ethanol and n-hexane, wherein the volume ratio of trimethylchlorosilane: anhydrous ethanol: n-hexane is 1:1:

8.

7. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In step S3, the drying process is carbon dioxide supercritical drying, and the temperature of the carbon dioxide supercritical drying is 200-350° C. and the pressure is 75-80 atmospheres.

8. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In the step S3, the drying process is performed by drying with hot nitrogen, and the temperature of the hot nitrogen is 400-800°C.

9. The method for preparing an aerogel dielectric layer by a wet process according to claim 1, characterized in that: In the step S1, the silica gel is a mixture of tetraethyl orthosilicate, dimethylformamide, anhydrous ethanol and deionized water, and the pH value is adjusted to between 2 and 3 by hydrochloric acid and / or ammonia water.

10. The method for preparing an aerogel dielectric layer by wet process according to claim 9, characterized in that: In the silica gel, the mass ratio of ethyl orthosilicate: dimethylformamide: anhydrous ethanol: deionized water is 1:0.5:6:

4.

11. An aerogel medium layer, characterized in that: The aerogel dielectric layer is prepared according to the method for preparing the aerogel dielectric layer by a wet process according to any one of claims 1 to 10.