Solar cell, preparation method thereof and photovoltaic module
By using plasma processes to form a tunneling layer and performing hydrogenation treatment in solar cells, combined with the design of doped semiconductor layers, the problem of insufficient passivation quality of the tunneling oxide layer is solved, which improves battery efficiency and reduces preparation costs.
Patent Information
- Application Number
- CN202411183417.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The contact composite of metal and silicon contact areas in existing solar cells and the Auger composite and deep energy level composite in silicon matrix due to diffusion are the main factors restricting the improvement of battery efficiency, and the passivation quality and performance of the tunneled oxide layer need to be promote.
A plasma process is used to form a tunnel layer on the semiconductor substrate, and the density of unsaturated hanging bonds on the surface of the tunnel layer is reduced by hydrogenation treatment, forming a doped semiconductor layer to improve passivation performance.
It improves the passivation quality and performance of the tunnel layer, improves the efficiency of the solar cell, and reduces process costs and preparation time.
Smart Images

Figure CN119008780A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar photovoltaic cells, and in particular to a solar cell and a preparation method thereof, and a photovoltaic module. Background Art
[0002] With the continuous development of solar cell technology, people have higher and higher requirements for the photoelectric conversion efficiency of cells. However, the improvement of industrial cell efficiency is still facing many challenges. Among them, the contact recombination between metal and silicon contact area and the Auger recombination and deep energy level recombination caused by diffusion in the silicon matrix are the main factors restricting the improvement of cell efficiency. The related technology reduces the recombination of surface carriers by setting a passivation contact structure on the surface of the silicon substrate, wherein the passivation contact structure is composed of a tunneling oxide layer and a doped polysilicon layer. However, the passivation quality and passivation performance of the current tunneling oxide layer need to be further improved. Summary of the invention
[0003] Based on this, it is necessary to provide a solar cell and a preparation method thereof, and a photovoltaic module to address the above problems.
[0004] In a first aspect, an embodiment of the present application provides a method for preparing a solar cell, comprising:
[0005] Providing a semiconductor substrate, the semiconductor substrate comprising a first surface and a second surface arranged opposite to each other;
[0006] forming a first tunneling layer on at least a portion of the first surface using a first plasma process;
[0007] Performing a hydrogenation treatment on the first tunneling layer using a second plasma process;
[0008] forming a first doped semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate;
[0009] A first electrode in ohmic contact with the first doped semiconductor layer is formed on a side of the first doped semiconductor layer away from the semiconductor substrate.
[0010] In one embodiment, the process gas of the second plasma process includes ammonia and argon, and the volume flow ratio of the ammonia and argon is between 3:1 and 2:1;
[0011] And / or, the chamber pressure of the second plasma process is between 1200 mbar and 1500 mbar;
[0012] And / or, the power of the second plasma process is between 11000W and 13000W;
[0013] And / or, the processing time of the second plasma process is between 50s and 60s;
[0014] And / or, the processing temperature of the second plasma process is between 440° C. and 455° C.
[0015] In one embodiment, forming a first doped semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate includes:
[0016] forming a doped amorphous semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate by a third plasma process;
[0017] forming a protective layer on a side of the doped amorphous semiconductor layer away from the semiconductor substrate;
[0018] The doped amorphous semiconductor layer is crystallized to form the first doped semiconductor layer.
[0019] In one embodiment, the first plasma process, the second plasma process and the third plasma process all use the same plasma equipment.
[0020] In one embodiment, the process gas of the third plasma process includes monosilane, argon and phosphine, and the volume flow ratio of monosilane, argon and phosphine is between 22:40:1 and 22:55:1;
[0021] And / or, the chamber pressure of the third plasma process is between 2700 mbar and 2900 mbar;
[0022] And / or, the power of the third plasma process is between 12000W and 13000W;
[0023] And / or, the processing time of the third plasma process is between 3450s and 3550s;
[0024] And / or, the processing temperature of the third plasma process is between 440° C. and 455° C.
[0025] In one embodiment, the process gas of the first plasma process includes nitrous oxide, and the volume flow rate of the nitrous oxide is between 10000 sccm and 12000 sccm;
[0026] And / or, the chamber pressure of the first plasma process is between 2700 mbar and 2900 mbar;
[0027] And / or, the power of the first plasma process is between 15000W and 16000W;
[0028] And / or, the processing time of the first plasma process is between 100s and 140s;
[0029] And / or, the processing temperature of the first plasma process is between 430°C and 450°C.
[0030] In one embodiment, the semiconductor substrate is provided with a first conductive region and a second conductive region arranged along a first direction; the first direction is perpendicular to a thickness direction of the semiconductor substrate;
[0031] The step of forming a first tunneling layer on at least a portion of the first surface using a first plasma process comprises:
[0032] A first tunneling layer is formed on the first surface of the first conductive region by using a first plasma process.
[0033] In one embodiment, after providing the semiconductor substrate and before forming the first tunneling layer on at least a portion of the first surface using a first plasma process, the method includes:
[0034] forming a second tunneling layer on the first surface located in the second conductive region;
[0035] A second doped semiconductor layer is formed on a side of the second tunneling layer away from the semiconductor substrate.
[0036] In one embodiment, an isolation region is further provided on the semiconductor substrate, and the isolation region is located between the first conductive region and the second conductive region;
[0037] The step of forming a first tunneling layer on the first surface of the first conductive region using a first plasma process comprises: forming a first tunneling material layer on the first surfaces of the first conductive region and the isolation region using a first plasma process; wherein the first tunneling material layer located in the first conductive region and on the first surface forms the first tunneling layer;
[0038] After forming a first doped semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate, and before forming a first electrode in ohmic contact with the first doped semiconductor layer on a side of the first doped semiconductor layer away from the semiconductor substrate, the method comprises:
[0039] removing the first tunneling material layer located in the isolation region, and forming an isolation trench on the first surface located in the isolation region;
[0040] Performing a texturing process on the semiconductor substrate;
[0041] A first passivation layer group is formed on a side of the first doped semiconductor layer away from the semiconductor substrate, and a second passivation layer group is formed on the second surface.
[0042] In a second aspect, an embodiment of the present application provides a solar cell, comprising:
[0043] A semiconductor substrate comprising a first surface and a second surface arranged opposite to each other;
[0044] A first tunneling layer, disposed on at least a portion of the first surface;
[0045] A first doped semiconductor layer, disposed on a side of the first tunneling layer away from the semiconductor substrate; and
[0046] A first electrode is disposed on a side of the first doped semiconductor layer away from the semiconductor substrate and is in ohmic contact with the first doped semiconductor layer;
[0047] The first tunneling layer is configured to be hydrogenated by a plasma process after being formed by plasma deposition.
[0048] In one embodiment, the semiconductor substrate is provided with a first conductive region, a second conductive region and an isolation region arranged along a first direction, and the isolation region is located between the first conductive region and the second conductive region; the first direction is perpendicular to the thickness direction of the semiconductor substrate; the first tunneling layer is provided on the first surface of the first conductive region;
[0049] The solar cell further comprises:
[0050] A second tunneling layer, disposed on the first surface located in the second conductive region;
[0051] A second doped semiconductor layer, disposed on a side of the second tunneling layer away from the semiconductor substrate;
[0052] An isolation groove, provided on the first surface located in the isolation area;
[0053] A first passivation layer group is provided on a side of the first doped semiconductor layer and the second doped semiconductor layer away from the semiconductor substrate;
[0054] A second passivation layer group is provided on the second surface;
[0055] The second electrode penetrates the first passivation layer group and is in ohmic contact with the second doped semiconductor layer.
[0056] In one embodiment, the solar cell further includes a nitrogen-rich layer, and the nitrogen-rich layer is disposed on at least a portion of the surface of the first tunneling layer away from the semiconductor substrate.
[0057] In a third aspect, an embodiment of the present application provides a photovoltaic assembly, comprising the solar cell in any embodiment of the second direction.
[0058] The solar cell and its preparation method, as well as the photovoltaic module provided in the embodiments of the present application, after a first tunneling layer is deposited by a plasma process, the first tunneling layer is hydrogenated by a plasma process, which can reduce the density of unsaturated dangling bonds on the surface of the first tunneling layer, improve the passivation quality and passivation performance of the first tunneling layer, and thus help improve the battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] In order to more clearly illustrate the technical solutions in the embodiments or exemplary embodiments of the present application, the drawings required for use in the description of the embodiments or exemplary embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0060] Figure 1 A schematic diagram of a process for preparing a solar cell provided in one embodiment of the present application.
[0061] Figure 2 Another schematic diagram of a process for preparing a solar cell provided in an embodiment of the present application.
[0062] Figure 3 for Figure 2 A schematic diagram of the local cross-sectional structure after the second tunneling material layer and the second intrinsic semiconductor material layer are formed during the preparation method shown.
[0063] Figure 4 for Figure 2 A schematic diagram of the local cross-sectional structure after the second doped semiconductor material layer and the borosilicate glass layer are formed during the preparation method shown.
[0064] Figure 5 for Figure 2 A schematic diagram of a local cross-sectional structure after a mask layer is formed during the preparation method shown.
[0065] Figure 6 for Figure 2 Schematic diagram of the local cross-sectional structure after a portion of the borosilicate glass layer is removed during the preparation method shown.
[0066] Figure 7 for Figure 2 A schematic diagram of a local cross-sectional structure after the second doped semiconductor material layer and the second tunneling material layer in a partial area are removed during the preparation method shown.
[0067] Figure 8for Figure 2 A schematic diagram of a partial cross-sectional structure after the first tunneling material layer, the doped amorphous semiconductor layer and the protective layer are formed during the preparation method shown.
[0068] Fig. 9 for Figure 2 Schematic diagram of the local cross-sectional structure after the protective layer in a part of the area is removed during the preparation method shown.
[0069] Fig.10 for Figure 2 A schematic diagram of the local cross-sectional structure after the isolation groove is formed during the preparation method shown.
[0070] Fig.11 for Figure 2 A schematic diagram of the local cross-sectional structure of a semiconductor substrate after texturing during the preparation method shown.
[0071] Fig.12 for Figure 2 Schematic diagram of the local cross-sectional structure after the protective layer and the borosilicate glass layer are removed during the preparation method shown.
[0072] Fig.13 for Figure 2 A schematic diagram of the local cross-sectional structure after the passivation material layer is formed during the preparation method shown.
[0073] Fig.14 A schematic diagram of a partial cross-sectional structure of a solar cell provided in one embodiment of the present application.
[0074] Reference numerals:
[0075] 1. Solar cell; 11. Semiconductor substrate; 11a. First conductive region; 11b. Second conductive region; 11c. Isolation region; 111. First surface; 112. Second surface; 121. First tunneling layer; 122. First doped semiconductor layer; 131. Second tunneling layer; 132. Second doped semiconductor layer; 141. First electrode; 142. Second electrode; 15. Isolation groove; 16. First passivation layer group; 161. First passivation layer; 162. First anti-reflection layer; 17. Second passivation layer group; 171. Second passivation layer; 172. Second anti-reflection layer; 21. Second tunneling material layer; 22. Second intrinsic semiconductor material layer; 23. Second doped semiconductor material layer; 24. Borosilicate glass layer; 25. Mask layer; 26. First tunneling material layer; 27. Doped amorphous semiconductor layer; 28. Protective layer; 29. Passivation material layer. DETAILED DESCRIPTION
[0076] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0077] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0078] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present application, the first element, component, region, layer, doping type or part discussed below can be represented as a second element, component, region, layer or part.
[0079] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.
[0080] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include / comprise" or "have" and the like specify the presence of stated features, wholes, steps, operations, components, parts, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, wholes, steps, operations, components, parts, or combinations thereof. At the same time, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.
[0081] Embodiments of the application are described herein with reference to cross-sectional views that are schematic diagrams of ideal embodiments (and intermediate structures) of the application, so that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances can be expected. Therefore, embodiments of the application should not be limited to the specific shapes of the zones shown herein, but rather include shape deviations due to, for example, manufacturing techniques. For example, an implanted region shown as a rectangle typically has rounded or curved features and / or an implant concentration gradient at its edges, rather than a binary change from an implanted region to a non-implanted region. Similarly, a buried region formed by implantation may result in some implantation in the region between the buried region and the surface through which the implantation is performed. Therefore, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shape of the region of the device, and do not limit the scope of the application.
[0082] First, refer to Figure 1 , and combined with Figure 3-Figure 14 As shown, an embodiment of the present application provides a method for preparing a solar cell 1, which can be used to prepare a back contact (BC) cell, a tunnel oxide passivating contact (TOPCon) cell, etc.
[0083] The preparation method specifically comprises the following steps:
[0084] S100: Provide a semiconductor substrate 11, the semiconductor substrate 11 includes a first surface 111 and a second surface 112 arranged opposite to each other. Here, one of the first surface 111 and the second surface 112 is a light-facing surface, and the other is a backlight surface. It can be understood that the material of the semiconductor substrate 11 can be silicon, a compound semiconductor, and a wide bandgap semiconductor material. Exemplarily, silicon includes crystalline silicon and amorphous silicon. Compound semiconductors include selenium, selenide, etc. Wide bandgap semiconductor materials include silicon carbide, gallium nitride, diamond, etc. It should be noted that the semiconductor substrate 11 can be double-sided polished in this step. For example: after being treated with an alkaline polishing solution at 60°C-80°C for 200s-250s, a block structure with a size of 13μm-18μm is formed on the surface of the semiconductor substrate 11. The alkaline polishing solution may include tetramethylamino hydroxide, potassium hydroxide, a polishing agent, and the like.
[0085] S400: Form a first tunneling layer 121 on at least a portion of the first surface 111 using a first plasma process. Exemplarily, the material of the first tunneling layer 121 may be a dielectric material, such as silicon oxide, aluminum oxide, silicon nitride, silicon oxynitride, magnesium fluoride, amorphous silicon, polycrystalline silicon, silicon carbide or titanium oxide, etc. Specifically, the first tunneling layer 121 may be deposited using a PECVD (Plasma Enhanced Chemical Vapor Deposition) process.
[0086] S500: The first tunneling layer 121 is hydrogenated by a second plasma process. The first tunneling layer 121 is hydrogenated to saturate the dangling bonds on the surface of the first tunneling layer 121 with hydrogen, thereby reducing the density of unsaturated dangling bonds and improving the passivation quality and passivation performance of the first tunneling layer 121. In addition, after the first plasma process is completed, the second plasma process is then performed, which is beneficial to reducing process costs. For example, the first plasma process and the second plasma process can be performed in the same chamber without transferring the semiconductor substrate 11 from one chamber to another, thereby eliminating the need to repeatedly construct the vacuum environment required for the plasma process.
[0087] S600: forming a first doped semiconductor layer 122 on a side of the first tunneling layer 121 away from the semiconductor substrate 11. The material of the first doped semiconductor layer 122 may be amorphous silicon, polycrystalline silicon, microcrystalline silicon, silicon carbide, etc. It is understandable that the first doped semiconductor layer 122 may be prepared by processes such as ALD (Atomic Layer Deposition), PECVD (Plasma Enhanced Chemical Vapor Deposition), PEALD (Plasma Enhanced Atomic Layer Deposition), and LPCVD (Low Pressure Chemical Vapor Deposition). The doping type of the first doped semiconductor layer 122 may be N-type or P-type.
[0088] S1000: Forming a first electrode 141 in ohmic contact with the first doped semiconductor layer 122 on a side of the first doped semiconductor layer 122 away from the semiconductor substrate 11. The material of the first electrode 141 includes, but is not limited to, one or more of aluminum, titanium, nickel, cobalt, silver, copper, and tin. The first electrode 141 may be formed by coating and sintering.
[0089] In one embodiment, the process gas of the second plasma process includes ammonia and argon. Thus, in the second plasma process, the bombardment of Ar ions can enhance the NH 3 The ionized H in the first tunneling layer 121 can reduce the density of unsaturated dangling bonds on the surface of the first tunneling layer 121. 3 The neutralized N can form a nitrogen-rich layer on the surface of the first tunneling layer 121, which blocks H seepage during metallization sintering and inhibits the degradation of the passivation quality of the first tunneling layer 121 during the sintering process. In addition, the N in the nitrogen-rich layer can enhance the energy of the Si-H bond, further improving the electrical properties and thermal stability of the first doped semiconductor layer 122.
[0090] In one embodiment, the volume flow ratio of ammonia gas to argon gas is between 3:1 and 2:1. For example, the volume flow ratio of ammonia gas to argon gas may be 3:1, 2.5:1, 2:1, etc. By making the volume flow ratio of ammonia gas to argon gas within the above range, it is beneficial to better reduce the density of unsaturated dangling bonds on the surface of the first tunneling layer 121, and further improve the electrical properties and thermal stability of the first doped semiconductor layer 122.
[0091] In one embodiment, the chamber pressure of the second plasma process is between 1200 mbar and 1500 mbar. For example, the chamber pressure of the second plasma process can be 1200 mbar, 1300 mbar, 1400 mbar, 1500 mbar, etc.
[0092] In one embodiment, the power of the second plasma process is between 11000 W and 13000 W. For example, the power of the second plasma process may be 11000 W, 12000 W, 13000 W, etc.
[0093] In one embodiment, the processing time of the second plasma process is between 50s and 60s. For example, the processing time of the second plasma process can be 50s, 55s, 58s, 60s, etc.
[0094] In one embodiment, the processing temperature of the second plasma process is between 440° C. and 455° C. For example, the processing temperature of the second plasma process may be 440° C., 450° C., 455° C., etc.
[0095] By making the process parameters of the second plasma process within the above range, it is beneficial to reduce the density of unsaturated dangling bonds on the surface of the first tunneling layer 121 and further improve the electrical properties and thermal stability of the first doped semiconductor layer 122 .
[0096] In one embodiment, S600: forming a first doped semiconductor layer 122 on a side of the first tunneling layer 121 away from the semiconductor substrate 11, specifically includes the following steps:
[0097] S610: Using a third plasma process to form a doped amorphous semiconductor layer 27 on the side of the first tunneling layer 121 away from the semiconductor substrate 11. Exemplarily, the doped amorphous semiconductor layer 27 may be a phosphorus-containing amorphous silicon layer, and further, the phosphorus-containing amorphous silicon layer may be deposited using a PECVD process. It should be noted that in the process of depositing the doped amorphous semiconductor layer 27, a step-by-step deposition method may be used.
[0098] S620: forming a protective layer 28 on the side of the doped amorphous semiconductor layer 27 away from the semiconductor substrate 11. Exemplarily, the protective layer 28 may be a silicon oxide layer, and further, the silicon oxide layer may be deposited by a PECVD process. Specifically, monosilane and nitrous oxide may be introduced to deposit a silicon oxide layer on the surface of the doped amorphous semiconductor layer 27. The volume flow ratio of monosilane and nitrous oxide may be 2:9, 1:4.8, 1:5, etc.; the chamber pressure may be 1400mbar-1600mbar; the power may be 8500W-9500W; the temperature may be 430℃-440℃; and the deposition time may be 40s-50s.
[0099] S630: Crystallize the doped amorphous semiconductor layer 27 to form a first doped semiconductor layer 122. Exemplarily, the semiconductor substrate 11 can be placed in an annealing furnace with a constant temperature of 900°C-930°C, a constant temperature time of 40s-60s, a heating rate of 0.1°C / s, and a heating time of 250s-350s. It should be noted that the initial temperature in the annealing furnace can be between 810°C-825°C, and the temperature can be increased multiple times during the heating process, with each heating time being 250s-350s. The structure after the formation of the protective layer 28 and the first doped semiconductor layer 122 is as follows: Figure 8 shown.
[0100] In one embodiment, the first plasma process, the second plasma process, and the third plasma process all use the same plasma equipment. Specifically, PECVD equipment is used to perform the first plasma process, the second plasma process, and the third plasma process. In this way, in the process of preparing the first tunneling layer 121 and the first doped semiconductor layer 122, the preparation process has good continuity, and the first plasma process, the second plasma process, and the third plasma process are successively performed in the same chamber, without the need to transfer the semiconductor substrate 11 from one chamber to another, thereby eliminating the need to repeatedly construct the vacuum environment required for the plasma process, thereby reducing the process cost. In addition, during the entire process, there is no need to take the semiconductor substrate 11 from the chamber to the air environment, thereby avoiding the contamination of the semiconductor substrate 11, the first tunneling layer 121, and the first doped semiconductor layer 122 by impurities in the external environment.
[0101] In one embodiment, the process gas of the third plasma process includes monosilane, argon and phosphine. It should be noted that monosilane can provide a silicon source and phosphine can provide a doping source. The use of argon can, on the one hand, promote the ionization of monosilane to increase the deposition rate, and on the other hand, reduce the H content in the doped amorphous semiconductor layer 27, control the porosity, and reduce the probability of film explosion of the doped amorphous semiconductor layer 27 during the crystallization process.
[0102] In one embodiment, the volume flow ratio of monosilane, argon and phosphine is between 22:40:1 and 22:55:1. For example, the volume flow ratio of monosilane, argon and phosphine can be 22:40:1, 22:48:1, 22:52:1, 22:55:1, etc.
[0103] In one embodiment, the chamber pressure of the third plasma process is between 2700 mbar and 2900 mbar. For example, the chamber pressure of the third plasma process can be 2700 mbar, 2800 mbar, 2900 mbar, etc.
[0104] In one embodiment, the power of the third plasma process is between 12000 W and 13000 W. For example, the power of the third plasma process may be 12000 W, 12500 W, 12800 W, 13000 W, etc.
[0105] In one embodiment, the processing time of the third plasma process is between 3450s and 3550s. For example, the processing time of the third plasma process can be 3450s, 3500s, 3550s, etc.
[0106] In one embodiment, the processing temperature of the third plasma process is between 440° C. and 455° C. For example, the processing temperature of the third plasma process may be 440° C., 450° C., 455° C., etc.
[0107] By making the process parameters of the third plasma process within the above range, on the one hand, the ionization of monosilane can be promoted to increase the deposition rate, and on the other hand, the H content in the doped amorphous semiconductor layer 27 can be reduced, the porosity can be controlled, and the probability of film explosion of the doped amorphous semiconductor layer 27 during the crystallization process can be reduced.
[0108] In one embodiment, the process gas of the first plasma process includes nitrous oxide, and the volume flow rate of the nitrous oxide is between 10000 sccm and 12000 sccm. For example, the volume flow rate of the nitrous oxide can be 10000 sccm, 11000 sccm, or 12000 sccm.
[0109] In one embodiment, the chamber pressure of the first plasma process is between 2700 mbar and 2900 mbar. For example, the chamber pressure of the first plasma process can be 2700 mbar, 2800 mbar, 2900 mbar, etc.
[0110] In one embodiment, the power of the first plasma process is between 15000 W and 16000 W. For example, the power of the first plasma process may be 15000 W, 15500 W, 16000 W, etc.
[0111] In one embodiment, the processing time of the first plasma process is between 100s and 140s. For example, the processing time of the first plasma process can be 100s, 120s, 130s, 140s, etc.
[0112] In one embodiment, the processing temperature of the first plasma process is between 430° C. and 450° C. For example, the processing temperature of the first plasma process may be 430° C., 440° C., 450° C., etc.
[0113] By making the process parameters of the first plasma process within the above range, it is beneficial to form the first tunneling layer 121 with good film quality and relatively uniform thickness.
[0114] It should be noted that the processing temperatures of the first plasma process, the second plasma process and the third plasma process are all between 400° C. and 500° C. The first plasma process, the second plasma process and the third plasma process are successively performed in the same chamber. Since the processing temperatures of each process are close, there is no need to repeatedly increase the temperature, which is beneficial to reducing the preparation time and preparation cost of the solar cell 1.
[0115] In one embodiment, referring to Figure 5 As shown, the semiconductor substrate 11 is provided with a first conductive region 11a and a second conductive region 11b arranged along a first direction X. The first direction X is perpendicular to the thickness direction of the semiconductor substrate 11. Furthermore, the semiconductor substrate 11 is further provided with an isolation region 11c, which is located between the first conductive region 11a and the second conductive region 11b.
[0116] S400: forming a first tunneling layer 121 on at least a portion of the first surface 111 using a first plasma process, specifically comprising the following steps:
[0117] S410: Forming a first tunneling layer 121 on the first surface 111 of the first conductive region 11a using a first plasma process. Figure 8 As shown, a first tunneling material layer 26 is deposited on a side of the semiconductor substrate 11 close to the first surface 111 , and the first tunneling material layer 26 covers the first conductive region 11 a , the second conductive region 11 b and the isolation region 11 c , wherein the first tunneling material layer 26 covering the first conductive region 11 a forms a first tunneling layer 121 .
[0118] In one embodiment, referring to Figure 2As shown, after S100: providing a semiconductor substrate 11, S400: before forming a first tunneling layer 121 on at least a portion of the first surface 111 using a first plasma process, the following steps are also included:
[0119] S200: forming a second tunneling layer 131 on the first surface 111 located in the second conductive region 11b. Figure 3 As shown, a second tunneling material layer 21 is formed on the first surface 111 and the second surface 112 . The second tunneling material layer 21 located in the second conductive region 11 b and on the first surface 111 forms a second tunneling layer 131 .
[0120] For example, the second tunneling layer 131 may be deposited by LPCVD process. The second tunneling layer 131 may be made of a dielectric material, such as silicon oxide, aluminum oxide, silicon nitride, silicon oxynitride, magnesium fluoride, amorphous silicon, polycrystalline silicon, silicon carbide or titanium oxide.
[0121] S300: forming a second doped semiconductor layer 132 on a side of the second tunneling layer 131 away from the semiconductor substrate 11. Figure 3 As shown, first, a second intrinsic semiconductor material layer 22 (eg, an intrinsic microcrystalline amorphous mixed layer) is deposited on the second tunneling material layer 21 by an LPCVD process, and then, referring to Figure 4 As shown, the semiconductor substrate 11 is placed in an annealing furnace, a borosilicate glass layer 24 is deposited on the second intrinsic semiconductor material layer 22, the second intrinsic semiconductor material layer 22 is crystallized at a high temperature, and the boron in the borosilicate glass layer 24 is doped into the second intrinsic semiconductor material layer 22, thereby forming a second doped semiconductor material layer 23. Figure 5 As shown, a mask layer 25 is formed on the side where the first surface 111 is located, so that the second doped semiconductor material layer 23 located in the isolation region 11c and the first conductive region 11a is exposed. Figure 6 As shown, the borosilicate glass layer 24 on the second surface 112 and the borosilicate glass layer 24 on the first surface 111 and located in the isolation region 11c and the first conductive region 11a are removed. For example, a hydrofluoric acid solution or a laser may be used to remove the borosilicate glass layer 24. Next, referring to Figure 7 As shown, an alkaline solution is used to remove the mask layer 25, and the retained borosilicate glass layer 24 is used as a mask, and an alkaline solution with a polishing agent added thereto is used to remove the second tunneling material layer 21 and the second doped semiconductor material layer 23 in other regions, so that the second tunneling material layer 21 and the second doped semiconductor material layer 23 in the second conductive region 11b are retained. Next, the semiconductor substrate 11 is sequentially placed in an ammonia solution for cleaning for 5 minutes, in a hydrochloric acid solution for cleaning for 5 minutes, and in a hydrofluoric acid solution for cleaning for 10 seconds, and subsequent steps are performed after the cleaning is completed.
[0122] In one embodiment, S410: forming a first tunneling layer 121 on the first surface 111 of the first conductive region 11a by using a first plasma process, comprising the following steps:
[0123] S411: Form a first tunneling material layer 26 on the first surface 111 located in the first conductive region 11a and the isolation region 11c using a first plasma process. Figure 8 As shown, the first tunneling material layer 26 located in the first conductive region 11 a and on the first surface 111 forms a first tunneling layer 121 , wherein the first tunneling material layer 26 also covers the retained borosilicate glass layer 24 .
[0124] S600: after forming the first doped semiconductor layer 122 on the side of the first tunneling layer 121 away from the semiconductor substrate 11, S1000: before forming the first electrode 141 in ohmic contact with the first doped semiconductor layer 122 on the side of the first doped semiconductor layer 122 away from the semiconductor substrate 11, the following steps are also included:
[0125] S700: removing the first tunneling material layer 26 located in the isolation region 11c, and forming an isolation trench 15 on the first surface 111 located in the isolation region 11c. Fig. 9 As shown, firstly, a laser is used to open the protective layer 28 of the isolation region 11c. During this process, a single-sided chain HF cleaning machine can also be used to remove the protective layer 28 plated around the edge and side of the second surface 112 of the semiconductor substrate 11. Fig.10 As shown, the semiconductor substrate 11 is placed in an alkaline solution containing a polishing agent (such as ammonia water and potassium hydroxide solution), the first tunneling layer 121 and the first doped semiconductor layer 122 of the isolation region 11c are removed, and an isolation groove 15 is etched on the semiconductor substrate 11, and the depth of the isolation groove 15 is about 3μm.
[0126] S800: Performing a texturing process on the semiconductor substrate 11. Fig.11 As shown, firstly, the semiconductor substrate 11 is placed in an alkaline solution (such as an ammonia solution) containing a texturing additive to perform a texturing treatment. Fig.12 As shown, the borosilicate glass layer 24 and the protective layer 28 are removed using a hydrofluoric acid solution.
[0127] S900: forming a first passivation layer group 16 on a side of the first doped semiconductor layer 122 away from the semiconductor substrate 11, and forming a second passivation layer group 17 on the second surface 112. Exemplarily, a passivation material layer 29 may be deposited on the first surface 111 and the second surface 112, respectively, the passivation material layer 29 on the first surface 111 forms the first passivation layer group 16, and the passivation material layer 29 on the second surface 112 forms the second passivation layer group 17.
[0128] Optionally, firstly, an aluminum oxide layer with a thickness of 5 nm to 10 nm is deposited on the first surface 111 and the second surface 112 respectively by using an ALD process, and then, a plurality of silicon nitride layers are deposited on the first surface 111 and the second surface 112 respectively by using a PECVD process, wherein the refractive index of the silicon nitride layer is between 2 and 2.3. The aluminum oxide layer and the silicon nitride layer on the first surface 111 constitute the first passivation layer group 16, and the aluminum oxide layer and the silicon nitride layer on the second surface 112 constitute the second passivation layer group 17.
[0129] After S900 is completed, S1000 is performed. It can be understood that in S1000, the first electrode 141 and the second electrode 142 can be formed simultaneously. Fig.14 As shown, the first electrode 141 penetrates the first passivation layer group 16 and is in ohmic contact with the first doped semiconductor layer 122, and the second electrode 142 penetrates the first passivation layer group 16 and is in ohmic contact with the second doped semiconductor layer 132. The first electrode 141 and the second electrode 142 can be formed by coating and sintering, wherein the sintering temperature can be between 840°C and 850°C.
[0130] It should be noted that the inventors have found through testing that the PL brightness of the solar cell prepared by the preparation method provided in the embodiment of the present application is improved by about 5000 compared with the solar cell prepared by the traditional method.
[0131] Second, refer to Fig.14 As shown, the embodiment of the present application provides a solar cell 1, which can be prepared by the preparation method described above. The solar cell 1 can be a back contact (BC) cell, a tunnel oxide passivating contact (TOPCon) cell, etc.
[0132] Specifically, the solar cell 1 includes a semiconductor substrate 11, a first tunneling layer 121, a first doped semiconductor layer 122 and a first electrode 141. The semiconductor substrate 11 includes a first surface 111 and a second surface 112 that are arranged opposite to each other. The first tunneling layer 121 is arranged on at least a portion of the first surface 111. The first doped semiconductor layer 122 is arranged on a side of the first tunneling layer 121 away from the semiconductor substrate 11. The first electrode 141 is arranged on a side of the first doped semiconductor layer 122 away from the semiconductor substrate 11, and is in ohmic contact with the first doped semiconductor layer 122.
[0133] The first tunnel layer 121 is configured to be hydrogenated by a plasma process after being deposited by a plasma process.
[0134] The solar cell 1 provided in the embodiment of the present application, after the first tunnel layer 121 is deposited by a plasma process, is subjected to a hydrogenation treatment by a plasma process, which can reduce the density of unsaturated dangling bonds on the surface of the first tunnel layer 121, improve the passivation quality and passivation performance of the first tunnel layer 121, and thus help improve the battery efficiency.
[0135] In one embodiment, a first conductive region 11a, a second conductive region 11b, and an isolation region 11c are arranged along a first direction X on the semiconductor substrate 11, and the isolation region 11c is located between the first conductive region 11a and the second conductive region 11b. The first direction X is perpendicular to the thickness direction of the semiconductor substrate 11. The first tunneling layer 121 is disposed on the first surface 111 located on the first conductive region 11a.
[0136] The solar cell 1 further includes a second tunneling layer 131, a second doped semiconductor layer 132, an isolation groove 15, a first passivation layer group 16, a second passivation layer group 17, and a second electrode 142. The second tunneling layer 131 is disposed on the first surface 111 located in the second conductive region 11b. The second doped semiconductor layer 132 is disposed on a side of the second tunneling layer 131 away from the semiconductor substrate 11. The isolation groove 15 is disposed on the first surface 111 located in the isolation region 11c. The first passivation layer group 16 is disposed on a side of the first doped semiconductor layer 122 and the second doped semiconductor layer 132 away from the semiconductor substrate 11, and the first passivation layer group 16 also covers the groove wall of the isolation groove 15. The second passivation layer group 17 is disposed on the second surface 112. The second electrode 142 penetrates the first passivation layer group 16 and is in ohmic contact with the second doped semiconductor layer 132.
[0137] Optionally, the first passivation layer group 16 includes a first passivation layer 161 and a first anti-reflection layer 162 which are stacked, and the second passivation layer group 17 includes a second passivation layer 171 and a second anti-reflection layer 172 which are stacked. The material of the first passivation layer 161 and the second passivation layer 171 may be aluminum oxide, and the material of the first anti-reflection layer 162 and the second anti-reflection layer 172 may include silicon nitride and silicon oxynitride.
[0138] In one embodiment, the solar cell 1 further comprises a nitrogen-rich layer, and the nitrogen-rich layer is provided on at least a portion of the surface of the first tunnel layer 121 away from the semiconductor substrate 11. It should be noted that during the process of hydrogenating the first tunnel layer 121 using the second plasma process, the bombardment of Ar ions can enhance the NH 3 The ionized H in the first tunneling layer 121 can reduce the density of unsaturated dangling bonds on the surface of the first tunneling layer 121. 3The ionized N can form a nitrogen-rich layer on the surface of the first tunneling layer 121, which blocks H from seeping out during metallization sintering, inhibits the degradation of the passivation quality of the first tunneling layer 121 during the sintering process, and the N in the nitrogen-rich layer can enhance the energy of the Si-H bond, further improving the electrical properties and thermal stability of the first doped semiconductor layer 122. It can be understood that the nitrogen-rich layer is a film layer containing nitrogen.
[0139] In a third aspect, an embodiment of the present application provides a photovoltaic assembly, comprising the solar cell in any embodiment of the second direction.
[0140] For example, the photovoltaic module includes a plurality of solar cells, which can be connected in series by welding ribbons, so that the electricity generated by the individual solar cells can be collected for subsequent transmission. Of course, the solar cells can be arranged at intervals or stacked in a shingled form.
[0141] Furthermore, the photovoltaic module also includes an encapsulation layer and a cover plate, wherein the encapsulation layer is used to cover the surface of the battery string, and the cover plate is used to cover the surface of the encapsulation layer away from the battery string. The solar cells are electrically connected in the form of a whole piece or multiple pieces to form a plurality of battery strings, and the plurality of battery strings are electrically connected in series and / or in parallel. Specifically, in some embodiments, the plurality of battery strings can be electrically connected by a conductive tape. The encapsulation layer covers the surface of the solar cell. Exemplarily, the encapsulation layer can be an organic encapsulation film such as an ethylene-vinyl acetate copolymer film, a polyethylene octene co-elastic film, or a polyethylene terephthalate film. The cover plate can be a cover plate with a light-transmitting function such as a glass cover plate, a plastic cover plate, etc.
[0142] It should be understood that in the embodiments of the present application, at least part of the steps in the drawings may include multiple steps or multiple stages, and these steps or stages are not necessarily performed at the same time, but may be performed at different times. The execution order of these steps or stages is not necessarily sequential, but may be performed in turn or alternately with other steps or at least part of the steps or stages in other steps.
[0143] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0144] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A method for preparing a solar cell, characterized in that: include: Providing a semiconductor substrate, the semiconductor substrate comprising a first surface and a second surface arranged opposite to each other; forming a first tunneling layer on at least a portion of the first surface using a first plasma process; Performing a hydrogenation treatment on the first tunneling layer using a second plasma process; forming a first doped semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate; A first electrode in ohmic contact with the first doped semiconductor layer is formed on a side of the first doped semiconductor layer away from the semiconductor substrate.
2. The method for preparing a solar cell according to claim 1, characterized in that: The process gas of the second plasma process includes ammonia and argon, and the volume flow ratio of the ammonia and argon is between 3:1 and 2:1; And / or, the chamber pressure of the second plasma process is between 1200 mbar and 1500 mbar; And / or, the power of the second plasma process is between 11000W and 13000W; And / or, the processing time of the second plasma process is between 50s and 60s; And / or, the processing temperature of the second plasma process is between 440° C. and 455° C.
3. The method for preparing a solar cell according to claim 1, characterized in that: The step of forming a first doped semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate comprises: forming a doped amorphous semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate by a third plasma process; forming a protective layer on a side of the doped amorphous semiconductor layer away from the semiconductor substrate; The doped amorphous semiconductor layer is crystallized to form the first doped semiconductor layer.
4. The method for preparing a solar cell according to claim 3, characterized in that: The first plasma process, the second plasma process and the third plasma process all use the same plasma equipment.
5. The method for preparing a solar cell according to claim 3, characterized in that: The process gas of the third plasma process includes monosilane, argon and phosphine, and the volume flow ratio of monosilane, argon and phosphine is between 22:40:1 and 22:55:1; And / or, the chamber pressure of the third plasma process is between 2700 mbar and 2900 mbar; And / or, the power of the third plasma process is between 12000W and 13000W; And / or, the processing time of the third plasma process is between 3450s and 3550s; And / or, the processing temperature of the third plasma process is between 440° C. and 455° C.
6. The method for preparing a solar cell according to claim 1, characterized in that: The process gas of the first plasma process includes nitrous oxide, and the volume flow rate of the nitrous oxide is between 10000 sccm and 12000 sccm; And / or, the chamber pressure of the first plasma process is between 2700 mbar and 2900 mbar; And / or, the power of the first plasma process is between 15000W and 16000W; And / or, the processing time of the first plasma process is between 100s and 140s; And / or, the processing temperature of the first plasma process is between 430°C and 450°C.
7. The method for preparing a solar cell according to any one of claims 1 to 6, characterized in that: The semiconductor substrate is provided with a first conductive region and a second conductive region arranged along a first direction; the first direction is perpendicular to the thickness direction of the semiconductor substrate; The step of forming a first tunneling layer on at least a portion of the first surface using a first plasma process comprises: A first tunneling layer is formed on the first surface of the first conductive region by using a first plasma process.
8. The method for preparing a solar cell according to claim 7, characterized in that: After providing the semiconductor substrate and before forming the first tunneling layer on at least a portion of the first surface using the first plasma process, the method includes: forming a second tunneling layer on the first surface located in the second conductive region; A second doped semiconductor layer is formed on a side of the second tunneling layer away from the semiconductor substrate.
9. The method for preparing a solar cell according to claim 7, characterized in that: An isolation region is also provided on the semiconductor substrate, and the isolation region is located between the first conductive region and the second conductive region; The step of forming a first tunneling layer on the first surface of the first conductive region using a first plasma process comprises: forming a first tunneling material layer on the first surfaces of the first conductive region and the isolation region using a first plasma process; wherein the first tunneling material layer located in the first conductive region and on the first surface forms the first tunneling layer; After forming a first doped semiconductor layer on a side of the first tunneling layer away from the semiconductor substrate, and before forming a first electrode in ohmic contact with the first doped semiconductor layer on a side of the first doped semiconductor layer away from the semiconductor substrate, the method comprises: removing the first tunneling material layer located in the isolation region, and forming an isolation trench on the first surface located in the isolation region; Performing a texturing process on the semiconductor substrate; A first passivation layer group is formed on a side of the first doped semiconductor layer away from the semiconductor substrate, and a second passivation layer group is formed on the second surface.
10. A solar cell, characterized in that: include: A semiconductor substrate comprising a first surface and a second surface arranged opposite to each other; A first tunneling layer, disposed on at least a portion of the first surface; A first doped semiconductor layer, disposed on a side of the first tunneling layer away from the semiconductor substrate; as well as A first electrode is disposed on a side of the first doped semiconductor layer away from the semiconductor substrate and is in ohmic contact with the first doped semiconductor layer; The first tunneling layer is configured to be hydrogenated by a plasma process after being formed by plasma deposition.
11. The solar cell according to claim 10, characterized in that The semiconductor substrate is provided with a first conductive region, a second conductive region and an isolation region arranged along a first direction, and the isolation region is located between the first conductive region and the second conductive region; the first direction is perpendicular to the thickness direction of the semiconductor substrate; The first tunneling layer is disposed on the first surface of the first conductive region; The solar cell further comprises: A second tunneling layer, disposed on the first surface located in the second conductive region; A second doped semiconductor layer, disposed on a side of the second tunneling layer away from the semiconductor substrate; An isolation groove, provided on the first surface located in the isolation area; A first passivation layer group is provided on a side of the first doped semiconductor layer and the second doped semiconductor layer away from the semiconductor substrate; A second passivation layer group is provided on the second surface; The second electrode penetrates the first passivation layer group and is in ohmic contact with the second doped semiconductor layer.
12. The solar cell according to claim 10, characterized in that: The solar cell further includes a nitrogen-rich layer, and the nitrogen-rich layer is disposed on at least a portion of the surface of the first tunneling layer on a side away from the semiconductor substrate.
13. A photovoltaic module, characterized in that: Comprising the solar cell according to any one of claims 10 to 12.
Citation Information
Patent Citations
Passivation process for solar cell fabrication
CN102414839A
Solar cell with silicon oxynitride dielectric layer
CN105144396A
Preparation method of silicon oxide and doped amorphous silicon film layer in TOPCon battery
CN112420881A
Back contact cell and manufacturing method thereof
CN113921625A
Solar cell, manufacturing method thereof and solar module
CN115036375A
Cited By
Solar cell and manufacturing method thereof, laminated cell and photovoltaic module
CN120857699A
Solar cell and method of manufacturing the same, stacked cell, and photovoltaic module
CN120857699B