Modified phosphorus-carbon composite material, preparation method thereof, negative electrode, battery and electric device
Through the preparation method of modified phosphorus-carbon composite materials, the combination of red phosphorus and porous hard carbon and soft carbon coating are used to solve the problem of insufficient capacity and circulation performance of traditional hard carbon in sodium ion batteries, achieving efficient Battery performance is improved.
Patent Information
- Application Number
- CN202411107540.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional hard carbon cannot take into account both capacity and circulation performance in sodium ion batteries, and there is a problem of insufficient performance.
By using the preparation method of modified phosphorus-carbon composite material, the first heat treatment is performed by mixing red phosphorus with porous hard carbon, the red phosphorus is deposited on the inner and outer surfaces of the porous hard carbon, and impregnated with the soft carbon precursor and the first heat treatment is carried out. Second, heat treatment forms a soft carbon coating, limiting the volume expansion of red phosphorus, and improving gram capacity and cycling performance.
The modified phosphorus-carbon composite material has a high capacity and circulation performance, and is suitable as the negative electrode material of sodium ion battery, improving the overall performance of the battery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and in particular to a modified phosphorus-carbon composite material and a preparation method thereof, a negative electrode, a battery and an electrical device. Background Art
[0002] With the development of electrification, more and more application scenarios require the use of electrochemical energy storage products. Currently, electrochemical energy storage is mainly based on lithium-ion batteries, but lithium resources are limited and unevenly distributed, so it is necessary to find an electrochemical energy storage product that can complement lithium-ion batteries. Sodium-ion batteries and lithium-ion batteries are both alkali metal ion batteries with similar working principles. Sodium has the advantages of higher abundance and more uniform distribution, making it more suitable for large-scale applications.
[0003] In sodium-ion batteries, commonly used positive electrode materials include layered oxides, polyanions, and Prussian materials, and traditional negative electrode materials include hard carbon. However, traditional hard carbon cannot take into account both gram capacity and cycle performance.
[0004] Therefore, it is necessary to improve the traditional technology. Summary of the invention
[0005] Based on this, the present application provides a modified phosphorus-carbon composite material with high specific capacity and cycle performance, and its preparation method, negative electrode, battery and electrical device.
[0006] The technical solution of this application to solve the above technical problems is as follows.
[0007] The first aspect of the present application provides a method for preparing a modified phosphorus-carbon composite material, comprising the following steps:
[0008] Mixing red phosphorus and porous hard carbon and performing a first heat treatment to deposit the red phosphorus into the pores and outer surface of the porous hard carbon to prepare a phosphorus-carbon composite material;
[0009] The phosphorus-carbon composite material is mixed with a soft carbon precursor for impregnation to prepare a modified phosphorus-carbon composite material precursor;
[0010] The modified phosphorus-carbon composite material precursor is subjected to a second heat treatment to prepare the modified phosphorus-carbon composite material.
[0011] In some of the embodiments, in the method for preparing the modified phosphorus-carbon composite material, the impregnation includes one of positive pressure impregnation and normal pressure impregnation.
[0012] In some embodiments, in the method for preparing the modified phosphorus-carbon composite material, the positive pressure impregnation satisfies at least one of the following characteristics:
[0013] (1) The pressure of the positive pressure impregnation is 0.7 MPa to 1.2 MPa;
[0014] (2) The positive pressure impregnation temperature is 100°C to 300°C, and the time is 2 h to 4 h;
[0015] (3) The pressurized gas used in the positive pressure impregnation includes at least one of nitrogen and inert gas.
[0016] In some of the embodiments, in the method for preparing the modified phosphorus-carbon composite material, the mass of the red phosphorus accounts for 1% to 50% of the total mass of the red phosphorus and the porous hard carbon.
[0017] In some of the embodiments, in the method for preparing the modified phosphorus-carbon composite material, the mass of the soft carbon precursor accounts for 1% to 10% of the total mass of the phosphorus-carbon composite material and the soft carbon precursor.
[0018] In some embodiments, in the method for preparing the modified phosphorus-carbon composite material, the first heat treatment satisfies at least one of the following characteristics:
[0019] (1) The temperature of the first heat treatment is 460°C to 600°C, and the time is 0.5 h to 2 h;
[0020] (2) The first heat treatment is performed under vacuum conditions.
[0021] In some embodiments, in the method for preparing the modified phosphorus-carbon composite material, the second heat treatment satisfies at least one of the following characteristics:
[0022] (1) The temperature of the second heat treatment is 300°C to 450°C, and the time is 2 h to 6 h;
[0023] (2) The second heat treatment is performed under nitrogen or an inert atmosphere.
[0024] In some of the embodiments, in the method for preparing the modified phosphorus-carbon composite material, the soft carbon precursor includes at least one of ethylene tar and coal tar.
[0025] In some embodiments, in the method for preparing the modified phosphorus-carbon composite material, the preparation of the phosphorus-carbon composite material further includes a step of washing with carbon disulfide after the first heat treatment step is completed.
[0026] In some embodiments, in the method for preparing the modified phosphorus-carbon composite material, the preparation of the porous hard carbon comprises the following steps:
[0027] The sodium lignin sulfonate, sodium chloride and water are mixed and freeze-dried to obtain a porous hard carbon precursor powder;
[0028] The porous hard carbon precursor powder is subjected to a third heat treatment and acid cleaning to prepare pre-carbonized porous hard carbon;
[0029] The pre-carbonized porous hard carbon is subjected to a fourth heat treatment to prepare the porous hard carbon; wherein the temperature of the fourth heat treatment is higher than the temperature of the third heat treatment.
[0030] In some embodiments, in the method for preparing the modified phosphorus-carbon composite material, the step of preparing the porous hard carbon satisfies at least one of the following characteristics:
[0031] (1) The mass ratio of the sodium lignin sulfonate to the sodium chloride is (0.1-9):1;
[0032] (2) The temperature of the third heat treatment is 400°C to 800°C, and the time is 2 h to 6 h;
[0033] (3) The temperature of the fourth heat treatment is 900°C to 1500°C, and the time is 2 h to 10 h;
[0034] (4) The freeze-drying treatment comprises: freezing the mixture of sodium lignin sulfonate, sodium chloride and water at -60°C to -50°C for 12 h to 24 h, and then drying it under vacuum conditions for 24 h to 48 h;
[0035] (5) The acid used for the acid cleaning includes at least one of a hydrochloric acid solution and a sulfuric acid solution;
[0036] (6) The acid concentration used in the acid cleaning is 0.01 mol / L~10 mol / L.
[0037] A second aspect of the present application provides a modified phosphorus-carbon composite material, which is prepared by the above-mentioned preparation method of the modified phosphorus-carbon composite material.
[0038] The third aspect of the present application provides a modified phosphorus-carbon composite material, comprising porous hard carbon, red phosphorus and a soft carbon layer, wherein the red phosphorus is arranged inside the pores and on the outer surface of the porous hard carbon, and the soft carbon layer covers at least part of the surface of the porous hard carbon and the red phosphorus.
[0039] In some of the embodiments, in the modified phosphorus-carbon composite material, the red phosphorus accounts for 0.5% to 30% of the total mass of the modified phosphorus-carbon composite material.
[0040] In some of the embodiments, in the modified phosphorus-carbon composite material, the mass of the soft carbon layer accounts for 0.5% to 5% of the total mass of the modified phosphorus-carbon composite material.
[0041] The fourth aspect of the present application provides the use of the above-mentioned modified phosphorus-carbon composite material in the preparation of a negative electrode.
[0042] In a fifth aspect, the present application provides a negative electrode, comprising a current collector and a negative electrode active layer disposed on the surface of the current collector, wherein the negative electrode active layer comprises the above-mentioned modified phosphorus-carbon composite material.
[0043] A sixth aspect of the present application provides a battery, comprising a positive electrode, a separator and the above-mentioned negative electrode arranged in a stacked manner.
[0044] A seventh aspect of the present application provides an electrical device comprising the above-mentioned battery.
[0045] Compared with the prior art, the preparation method of the modified phosphorus-carbon composite material of the present application has the following beneficial effects:
[0046] The preparation method of the modified phosphorus-carbon composite material of the present application is as follows: red phosphorus and porous hard carbon are mixed and subjected to a first heat treatment, wherein the pores of the porous hard carbon provide sites for the deposition of red phosphorus, so that the red phosphorus is deposited in the pores and on the outer surface of the porous hard carbon, and the red phosphorus deposited in the pores is limited by the pore walls, thereby reducing the volume expansion of the red phosphorus; the prepared phosphorus-carbon composite material is then mixed with a soft carbon precursor and impregnated, and the soft carbon precursor enters the pores and on the surface of the phosphorus-carbon composite material; a second heat treatment is performed to form a soft carbon coating layer on the surface of the phosphorus-carbon composite material, and the soft carbon coating layer can further limit the volume expansion of red phosphorus, thereby enabling the prepared modified phosphorus-carbon composite material to have both higher gram capacity and cycle performance, while also having higher first efficiency. DETAILED DESCRIPTION
[0047] References to embodiments of the present invention will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present invention. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present invention without departing from the scope or spirit of the present invention. For example, a feature illustrated or described as part of one embodiment may be used in another embodiment to produce a further embodiment.
[0048] Therefore, it is intended that the present invention covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present invention are disclosed in or are obvious from the following detailed description. Those of ordinary skill in the art will appreciate that this discussion is only a description of exemplary embodiments and is not intended to limit the broader aspects of the present invention.
[0049] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0050] The term "comprises", "comprising" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprising one..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements. The indefinite articles "a kind of" and "an" before the elements or components of the present invention are not restrictive to the quantity requirements (i.e., the number of occurrences) of the elements or components. Therefore, "a" or "a kind of" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number clearly refers only to the singular form. The meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0051] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0052] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. For example, therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0053] An embodiment of the present application provides a method for preparing a modified phosphorus-carbon composite material, comprising steps S10 to S30:
[0054] Step S10: Mix red phosphorus and porous hard carbon and perform a first heat treatment to deposit the red phosphorus inside the pores and on the outer surface of the porous hard carbon to prepare a phosphorus-carbon composite material.
[0055] The red phosphorus and porous hard carbon are mixed and subjected to a first heat treatment, and the red phosphorus is deposited inside the pores and on the outer surface of the porous hard carbon by utilizing a capillary effect.
[0056] In some of the examples, in step S10, the mass of the red phosphorus accounts for 1% to 50% of the total mass of the red phosphorus and the porous hard carbon.
[0057] It can be understood that the percentage of the mass of red phosphorus to the total mass of red phosphorus and porous hard carbon includes but is not limited to 1%, 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%. In some examples, any two of these point values can be used as the range of end values, the same below.
[0058] In some of the examples, in step S10, the mass of the red phosphorus accounts for 10% to 30% of the total mass of the red phosphorus and the porous hard carbon.
[0059] In some of the examples, in step S10, the temperature of the first heat treatment is 460° C. to 600° C., and the time is 0.5 h to 2 h.
[0060] It can be understood that the temperature of the first heat treatment includes but is not limited to 460℃, 470℃, 480℃, 490℃, 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, and 600℃, and the time includes but is not limited to 0.5 h, 0.8 h, 1 h, 1.2 h, 1.5 h, 1.8 h, and 2 h.
[0061] Optionally, the temperature of the first heat treatment is 480° C. to 550° C., and the time is 1 h to 2 h.
[0062] In some examples, in step S10 , the first heat treatment is performed under vacuum conditions.
[0063] The red phosphorus and porous hard carbon are mixed and subjected to the first heat treatment under vacuum conditions. The red phosphorus is converted into white phosphorus vapor at 416°C. The white phosphorus vapor is loaded in the pores and outer surface of the porous hard carbon by capillary effect. After cooling, the white phosphorus is converted into red phosphorus to obtain a phosphorus-carbon composite material.
[0064] In some examples, in step S10, the red phosphorus and porous hard carbon are mixed and vacuum-sealed in a quartz tube for a first heat treatment.
[0065] In some of the examples, in step S10, after the first heat treatment step is completed, a cleaning step using carbon disulfide is also included.
[0066] It is understood that the number of cleaning times is not limited. Optionally, the number of cleaning times using carbon disulfide is 3 times or more.
[0067] It is understood that carbon disulfide can wash away white phosphorus that has not been converted to red phosphorus.
[0068] In some of the examples, in step S10 , the step of cleaning with carbon disulfide is performed under an inert atmosphere.
[0069] It can be understood that the present application does not limit the source of the porous hard carbon, which can be commercially available or homemade, and the method of homemade is not limited.
[0070] In some examples, in step S10, the preparation of porous hard carbon includes steps S11 to S13:
[0071] Step S11: Sodium lignin sulfonate, sodium chloride and water are mixed and freeze-dried to obtain porous hard carbon precursor powder.
[0072] In some of the examples, in step S11, the mass ratio of sodium lignin sulfonate to sodium chloride is (0.1-9):1.
[0073] It will be appreciated that the mass ratio of sodium lignin sulfonate to sodium chloride includes, but is not limited to, 0.1:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, and 9:1.
[0074] Optionally, the mass ratio of sodium lignin sulfonate to sodium chloride is (0.25~4):1.
[0075] In some of the examples, in step S11, the freeze-drying treatment includes: freezing a mixture of sodium lignin sulfonate, sodium chloride and water at -60°C to -50°C for 12 h to 24 h, and then drying it under vacuum conditions for 24 h to 48 h.
[0076] It is understood that the freezing temperature includes but is not limited to -60°C, -58°C, -55°C, -52°C, and -50°C; the freezing time includes but is not limited to 12 h, 15 h, 18 h, 20 h, and 24 h; the drying temperature includes but is not limited to 24 h, 30 h, 35 h, 40 h, 45 h, and 48 h.
[0077] In some specific examples, in step S11, the freeze-drying treatment includes: freezing the mixture of sodium lignin sulfonate, sodium chloride and water at -55°C for 12 hours, and then drying it under vacuum conditions for 48 hours.
[0078] Step S12: subjecting the porous hard carbon precursor powder to a third heat treatment and acid cleaning to prepare pre-carbonized porous hard carbon.
[0079] In some of the examples, in step S12, the temperature of the third heat treatment is lower than the melting point of sodium chloride.
[0080] In some of the examples, in step S12, the temperature of the third heat treatment is 400° C. to 800° C., and the time is 2 h to 6 h.
[0081] It can be understood that the temperature of the third heat treatment includes but is not limited to 400℃, 450℃, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, 800℃, and the time includes but is not limited to 2 h, 3 h, 4 h, 5 h, 6 h.
[0082] In some of the examples, in step S12, the temperature of the third heat treatment is 500° C. to 600° C., and the time is 2 h to 4 h.
[0083] The sodium chloride template and sodium lignin sulfonate are compounded by freeze drying and carbonized and solidified at a temperature below the melting point of sodium chloride, and then the excess sodium chloride is washed away to obtain pre-carbonized porous hard carbon.
[0084] In some of the examples, in step S12, the acid used for acid cleaning includes at least one of a hydrochloric acid solution and a sulfuric acid solution.
[0085] In some of the examples, in step S12, the acid concentration used for acid cleaning is 0.01 mol / L~10 mol / L.
[0086] It will be appreciated that the acid concentration used for acid cleaning includes but is not limited to 0.01 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, and 10 mol / L.
[0087] It is understandable that water can be used for further cleaning after acid cleaning.
[0088] Step S13: subjecting the pre-carbonized porous hard carbon to a fourth heat treatment to prepare porous hard carbon; wherein the temperature of the fourth heat treatment is higher than the temperature of the third heat treatment.
[0089] In some of the examples, in step S13, the temperature of the fourth heat treatment is 900° C. to 1500° C., and the time is 2 h to 10 h.
[0090] It can be understood that the temperature of the fourth heat treatment includes but is not limited to 900°C~1500°C, and the time includes but is not limited to 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, and 10h.
[0091] Optionally, the temperature of the fourth heat treatment is 1000° C. to 1400° C., and the time is 2 h to 5 h.
[0092] The low-cost porous hard carbon prepared by the sodium chloride template has abundant pores, which can provide sites for the deposition of red phosphorus, and can effectively improve the gram capacity of the modified phosphorus-carbon composite material; and the red phosphorus deposited in the pores is restricted by the pore wall and the soft carbon coating layer, which can reduce the volume expansion of red phosphorus, and further promote the modified phosphorus-carbon composite material to take into account both high gram capacity and cycle performance. The template used in the sodium chloride template method is sodium chloride, which is environmentally friendly and reusable; and sodium lignin sulfonate is a by-product of the papermaking industry, and the use of sodium lignin sulfonate as waste has high economic value.
[0093] Step S20: mixing the phosphorus-carbon composite material and the soft carbon precursor and impregnating them to prepare a modified phosphorus-carbon composite material precursor.
[0094] In some examples, in step S20, the impregnation includes one of positive pressure impregnation and normal pressure impregnation.
[0095] Preferably, in step S20, the impregnation is positive pressure impregnation.
[0096] Mixing the phosphorus-carbon composite material with a soft carbon precursor and performing positive pressure impregnation can effectively fill the soft carbon precursor in the pores after the porous hard carbon is deposited with red phosphorus, thereby achieving dual confinement of the pore wall and the soft carbon coating layer, thereby effectively inhibiting the volume expansion of red phosphorus.
[0097] In some of the examples, in step S20, the pressure of the positive pressure impregnation is 0.7 MPa to 1.2 MPa.
[0098] It can be understood that the pressure of positive pressure impregnation includes but is not limited to 0.7 Mpa, 0.8 Mpa, 0.9 Mpa, 1.0 Mpa, 1.1 Mpa, and 1.2 Mpa.
[0099] In some examples, in step S20 , the pressurized gas used in the positive pressure impregnation includes at least one of nitrogen and an inert gas.
[0100] It can be understood that the inert gas includes but is not limited to helium, neon, argon, krypton, xenon, etc.
[0101] In some of the examples, in step S20, the positive pressure impregnation is performed at a temperature of 100° C. to 300° C. and for a time of 2 h to 4 h.
[0102] In some of the examples, in step S20, the temperature of the positive pressure impregnation includes but is not limited to 100°C, 120°C, 150°C, 180°C, 200°C, 220°C, 250°C, 280°C, and 300°C, and the time includes but is not limited to 2 h, 2.5 h, 3 h, 3.5 h, and 4 h.
[0103] Optionally, the temperature of the positive pressure impregnation is 100°C to 200°C.
[0104] In some of the examples, in step S20, the mass of the soft carbon precursor accounts for 1% to 10% of the total mass of the phosphorus-carbon composite material and the soft carbon precursor.
[0105] It can be understood that the percentage of the mass of the soft carbon precursor to the total mass of the phosphorus-carbon composite material and the soft carbon precursor includes but is not limited to 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.
[0106] In some of the examples, in step S20, the mass of the soft carbon precursor accounts for 5% to 10% of the total mass of the phosphorus-carbon composite material and the soft carbon precursor.
[0107] In some examples, in step S20, the soft carbon precursor includes at least one of ethylene tar and coal tar.
[0108] Highly fluid ethylene tar can better fill the pores after red phosphorus is deposited on porous hard carbon, forming a soft carbon coating on the surface of the phosphorus-carbon composite material, further limiting the volume expansion of red phosphorus.
[0109] Step S30: subjecting the modified phosphorus-carbon composite material precursor to a second heat treatment to prepare a modified phosphorus-carbon composite material.
[0110] The preparation method of the above-mentioned modified phosphorus-carbon composite material is to mix red phosphorus and porous hard carbon for a first heat treatment, the pores of the porous hard carbon provide sites for the deposition of red phosphorus, so that the red phosphorus is deposited in the pores and on the outer surface of the porous hard carbon, and the red phosphorus deposited in the pores is limited by the pore walls, which can reduce the volume expansion of the red phosphorus; then the prepared phosphorus-carbon composite material is mixed with a soft carbon precursor for impregnation, and the soft carbon precursor enters the pores and surface of the phosphorus-carbon composite material, and after a second heat treatment, a soft carbon coating layer is formed on the surface of the phosphorus-carbon composite material, and the soft carbon coating layer can further limit the volume expansion of red phosphorus, so that the prepared modified phosphorus-carbon composite material has both high gram capacity and cycle performance, and also has a high first effect.
[0111] In some of the examples, in step S30, the temperature of the second heat treatment is 300° C. to 450° C., and the time is 2 h to 6 h.
[0112] It can be understood that the temperature of the second heat treatment includes but is not limited to 300°C, 320°C, 350°C, 380°C, 400°C, 420°C, 450°C, and the time includes but is not limited to 2 h, 3 h, 4 h, 5 h, 6 h.
[0113] In some of the examples, in step S30, the temperature of the second heat treatment is 350° C. to 420° C., and the time is 2 h to 4 h.
[0114] In some examples, in step S30 , the second heat treatment is performed under nitrogen or an inert atmosphere.
[0115] An embodiment of the present application provides a modified phosphorus-carbon composite material, which is prepared by the preparation method of the modified phosphorus-carbon composite material.
[0116] It can be understood that the modified phosphorus-carbon composite material provided in the present application has both high gram capacity and cycle performance, and also has a high first efficiency, and is particularly suitable for use as a negative electrode for sodium ion batteries.
[0117] An embodiment of the present application provides a modified phosphorus-carbon composite material, including porous hard carbon, red phosphorus and a soft carbon layer, wherein the red phosphorus is arranged inside the pores and on the outer surface of the porous hard carbon, and the soft carbon layer covers at least part of the surface of the porous hard carbon and the red phosphorus.
[0118] In some of these examples, in the modified phosphorus-carbon composite material, red phosphorus accounts for 0.5% to 30% of the total mass of the modified phosphorus-carbon composite material.
[0119] It will be appreciated that the percentage of red phosphorus in the total mass of the modified phosphorus-carbon composite material includes but is not limited to 0.5%, 1%, 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, and 30%.
[0120] In some of these examples, in the modified phosphorus-carbon composite material, the mass of the soft carbon layer accounts for 0.5%~5% of the total mass of the modified phosphorus-carbon composite material.
[0121] It can be understood that the percentage of the mass of the soft carbon layer to the total mass of the modified phosphorus-carbon composite material includes but is not limited to 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, and 5%.
[0122] It can be understood that red phosphorus is provided on at least part of the inner and outer areas of the pores of the porous hard carbon, and the soft carbon layer covers at least part of the surface of the porous hard carbon and the red phosphorus, including red phosphorus deposited on the inner or outer surfaces of the porous hard carbon pores and the inner or outer surfaces of the porous hard carbon pores where red phosphorus is not deposited.
[0123] One embodiment of the present application provides the use of the modified phosphorus-carbon composite material in preparing a negative electrode.
[0124] One embodiment of the present application provides a negative electrode, including a current collector and a negative electrode active layer disposed on the surface of the current collector, wherein the negative electrode active layer includes the above-mentioned modified phosphorus-carbon composite material.
[0125] The negative electrode provided in the present application comprises the above-mentioned modified phosphorus-carbon composite material, which can give the negative electrode higher gram capacity, cycle performance and first effect.
[0126] In some of the examples, the negative electrode includes a negative electrode active material, a conductive filler, a dispersant and a binder, and the negative electrode active material includes the modified phosphorus-carbon composite material.
[0127] It is to be understood that the present application does not limit the types of current collectors, conductive agents, dispersants, binders and solvents, and conventional ones may be used.
[0128] In some examples, in the negative electrode, the conductive agent includes, but is not limited to, conductive carbon black.
[0129] In some examples, in the negative electrode, the dispersant includes but is not limited to hydroxymethyl cellulose.
[0130] In some of the examples, in the negative electrode, the binder includes but is not limited to styrene-butadiene rubber.
[0131] In some of these examples, in the negative electrode, the current collector includes, but is not limited to, copper foil.
[0132] An embodiment of the present application provides a battery, comprising a positive electrode, a separator and the above-mentioned negative electrode arranged in sequence.
[0133] The battery provided in the present application comprises the above-mentioned negative electrode, which gives the battery the same advantages as the above-mentioned negative electrode.
[0134] It will be appreciated that batteries include but are not limited to sodium ion batteries, lithium ion batteries, and the like.
[0135] In some of these examples, the battery is a sodium-ion battery.
[0136] In some examples, the positive electrode includes a positive electrode active material, a conductive agent, and a binder.
[0137] It can be understood that the present application does not limit the types of the isolation membrane, positive electrode active material, conductive agent and binder, and conventional ones are sufficient.
[0138] In some of the examples, the positive electrode active material includes but is not limited to at least one of transition metal layered oxides, polyanionic compounds and Prussian blue compounds; the positive electrode active material can reversibly remove and insert sodium; the conductive agent includes but is not limited to at least one of conductive carbon black, carbon fiber, acetylene black, Ketjen black, graphene and carbon nanotubes; the binder includes but is not limited to at least one of fluorine-containing resin, polypropylene resin, fiber-type binder, rubber-type binder and polyimide-type binder; the isolation membrane includes but is not limited to at least one of polyethylene, polypropylene and glass fiber.
[0139] In some of these examples, the battery also includes an electrolyte.
[0140] In some of these examples, the electrolyte includes an organic solvent and a sodium salt. Further, the organic solvent includes at least one of a carbonate-based solvent, an ether-based solvent, and a ketone-based solvent. In particular, the organic solvent can be an aprotic organic solvent, such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate. At least one of the like. The sodium salt is a material soluble in the above-mentioned organic solvent, including but not limited to at least one of NaCl, NaBr, NaI, NaClO4, NaBF4, NaPF6, NaCF3SO3, NaCF3CO2, NaAsF6, NaSbF6, NaAlCl4, CH3SO3Na and (CF3SO2)2NNa.
[0141] An embodiment of the present application provides an electrical device, comprising the above-mentioned battery.
[0142] The battery provided in this application can be used in, but is not limited to, electrical devices such as vehicles, ships or aircraft.
[0143] An embodiment of the present application provides an electrical device, comprising the above-mentioned battery.
[0144] Furthermore, the electric device may be, but is not limited to, a mobile phone, a tablet, a laptop, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft, etc.
[0145] The present application is further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present application are not limited thereto.
[0146] Example 1
[0147] 1. Preparation of soft carbon confined high-capacity phosphorus-carbon composite materials
[0148] (1) Dissolve 20 g of sodium lignin sulfonate and 40 g of sodium chloride in 1000 mL of deionized water to obtain a precursor solution; freeze the precursor solution in a freeze dryer at -55 °C for 12 h, and then evacuate the mixture for 48 h to obtain a white precursor powder; heat treat the white precursor powder at 500 °C for 3 h in a nitrogen atmosphere, and wash it with deionized water three times to obtain a pre-carbonized porous hard carbon; heat treat the pre-carbonized porous hard carbon at 1200 °C for 3 h in an argon atmosphere to obtain a porous hard carbon.
[0149] (2) 9 g of the porous hard carbon prepared in step (1) and 1 g of red phosphorus were sealed in a vacuum quartz tube, heat treated at 500° C. for 2 h, and washed with CS2 for 3 times to obtain a phosphorus-carbon composite material;
[0150] (3) 9.5 g of the phosphorus-carbon composite material prepared in step (2) was mixed with 0.5 g of ethylene tar, and the resulting mixture was immersed in a hydrothermal reactor under a nitrogen atmosphere at 0.9 MPa and 150°C for 3 h to obtain a modified phosphorus-carbon composite material precursor; the modified phosphorus-carbon composite material precursor was heat treated at 400°C for 2 h under a nitrogen atmosphere to form a soft carbon coating layer, thereby obtaining a modified phosphorus-carbon composite material.
[0151] Example 2
[0152] The method is basically the same as Example 1, except that in step (1), the amount of sodium lignin sulfonate is 30 g and the amount of sodium chloride is 30 g.
[0153] Example 3
[0154] The method is basically the same as Example 1, except that in step (1), the amount of sodium lignin sulfonate is 40 g and the amount of sodium chloride is 20 g.
[0155] Example 4
[0156] The method is basically the same as Example 1, except that in step (2), the porous hard carbon prepared in step (1) is 8 g and the red phosphorus is 2 g.
[0157] Example 5
[0158] The method is basically the same as Example 1, except that in step (2), the porous hard carbon prepared in step (1) is 7 g and the red phosphorus is 3 g.
[0159] Example 6
[0160] The method is basically the same as Example 1, except that in step (3), the phosphorus-carbon composite material prepared in step (2) is 9.2 g and the ethylene tar is 0.8 g.
[0161] Example 7
[0162] The method is basically the same as Example 1, except that in step (3), the phosphorus-carbon composite material prepared in step (2) is 9 g and the ethylene tar is 1 g.
[0163] Example 8
[0164] The method is basically the same as Example 1, except that in step (3), the pressure of the positive pressure impregnation is 0.7 MPa.
[0165] Example 9
[0166] The method is basically the same as Example 1, except that in step (3), the pressure of the positive pressure impregnation is 1.0 MPa.
[0167] Example 10
[0168] The method is basically the same as Example 1, except that in step (3), 9.5 g of the phosphorus-carbon composite material prepared in step (2) is mixed with 0.5 g of ethylene tar and then immersed at normal pressure (0.1013 MPa) and 150°C for 3 h.
[0169] Embodiment 11
[0170] The method is basically the same as Example 1, except that in step (3), the positive pressure impregnation temperature is 300° C. and the time is 2 h.
[0171] Example 12
[0172] The method is basically the same as Example 1, except that in step (3), the heat treatment temperature is 300° C. and the time is 6 h.
[0173] Comparative Example 1
[0174] Porous hard carbon prepared in step (1) of Example 1.
[0175] Comparative Example 2
[0176] The phosphorus-carbon composite material prepared in step (2) of Example 1.
[0177] Comparative Example 3
[0178] Red phosphorus is directly used as the negative electrode active material.
[0179] Comparative Example 4
[0180] The method is basically the same as Example 1, except that in step (3), after 9.5 g of the phosphorus-carbon composite material prepared in step (2) is mechanically mixed with 0.5 g of ethylene tar, it is not impregnated and is directly heat-treated at 400°C for 2 h in a nitrogen atmosphere to obtain a modified phosphorus-carbon composite material.
[0181] Comparative Example 5
[0182] The method is basically the same as Example 1, except that in step (3), 9.5 g of the phosphorus-carbon composite material prepared in step (2) and an ethylene tar dilution (0.5 g of ethylene tar is dispersed in 200 mL of tetrahydrofuran solution) are ultrasonically dispersed for 3 h and then filtered and dried instead of impregnating.
[0183] Some parameters of the modified phosphorus-carbon composite materials prepared in various embodiments and comparative examples are shown in Table 1.
[0184] Preparation of negative electrode
[0185] The modified phosphorus-carbon composite material or phosphorus-carbon composite material prepared in each embodiment and comparative example was used as a negative electrode active material, and was dispersed in deionized water with conductive carbon black, hydroxymethyl cellulose and styrene-butadiene rubber to form a negative electrode slurry; wherein the mass ratio of the negative electrode active material, the conductive carbon black, the hydroxymethyl cellulose and the styrene-butadiene rubber was 92%:3%:2%:3%, and the negative electrode slurry was coated on a copper foil and then dried at 100°C for 10 minutes to form a negative electrode active material layer, and the surface density after drying was 8 mg / cm 2 , compacted density is 0.9 g / cm 3 .
[0186] Preparation of sodium secondary batteries
[0187] The negative electrode sheets obtained above were assembled in the order of negative electrode shell, spring sheet, gasket, sodium sheet, electrolyte, separator, electrolyte, negative electrode sheet, and positive electrode shell to make button batteries, and the gram capacity and cycle tests were carried out: 12 h of storage → 0.1 C constant current discharge to 0 V → rest for 5 min → 0.1 C constant current charge to 2 V → rest for 5 min → 1 C constant current charge to 2 V → rest for 5 min → 1 C constant current discharge to 0 V → rest for 5 min; 0.1 C constant current discharge to 0 V → rest for 5 min → 0.1 C constant current charge to 2 V → rest for 5 min was repeated 500 times, and the 500th discharge capacity was recorded as C 500 The test results are shown in Table 1.
[0188] Table 1
[0189]
[0190] Among them, the mass of the soft carbon precursor accounts for m1% of the total mass of the phosphorus-carbon composite material and the soft carbon precursor, the mass of red phosphorus accounts for m2% of the total mass of red phosphorus and porous hard carbon, and "sodium lignin sulfonate: sodium chloride" refers to the mass ratio of sodium lignin sulfonate to sodium chloride.
[0191] As can be seen from Table 1, compared with the comparative examples, the modified phosphorus-carbon composite materials prepared in each embodiment have better comprehensive performance in terms of gram capacity and cycle performance; among them, compared with the impregnation under normal pressure in step (3) of Example 10, the modified phosphorus-carbon composite materials obtained by positive pressure impregnation in Example 1 and Examples 8-9 have better cycle performance. In Comparative Example 1, porous hard carbon is directly used as the negative electrode active material, and its gram capacity is low, which cannot meet the requirements of high energy density; in Comparative Example 2, the phosphorus-carbon composite material with red phosphorus deposited on the surface of the hard carbon porous material is directly used as the negative electrode active material, and no soft carbon coating layer is formed, and its cycle performance is significantly poor; in Comparative Example 3, high-capacity red phosphorus is directly used as the negative electrode material, and its cycle performance is extremely poor; in Comparative Example 4, the phosphorus-carbon composite material and ethylene tar are mixed without impregnation, and heat treatment is directly performed, the soft carbon coating layer cannot be filled, and the coating layer is uneven, and the cycle performance is poor; in Comparative Example 5, ultrasonic dispersion is used, and the soft carbon coating layer is a porous structure, which has limited ability to limit the volume expansion of red phosphorus.
[0192] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0193] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A method for preparing a modified phosphorus-carbon composite material, characterized in that: The following steps are involved: Mixing red phosphorus and porous hard carbon and performing a first heat treatment to deposit the red phosphorus into the pores and outer surface of the porous hard carbon to prepare a phosphorus-carbon composite material; The phosphorus-carbon composite material is mixed with a soft carbon precursor for impregnation to prepare a modified phosphorus-carbon composite material precursor; The modified phosphorus-carbon composite material precursor is subjected to a second heat treatment to prepare the modified phosphorus-carbon composite material.
2. The preparation method according to claim 1, characterized in that The impregnation includes one of positive pressure impregnation and normal pressure impregnation.
3. The preparation method according to claim 2, characterized in that The positive pressure impregnation satisfies at least one of the following characteristics: (1) The pressure of the positive pressure impregnation is 0.7 MPa to 1.2 MPa; (2) The positive pressure impregnation temperature is 100°C to 300°C, and the time is 2 h to 4 h; (3) The pressurized gas used in the positive pressure impregnation includes at least one of nitrogen and inert gas.
4. The preparation method according to claim 1, characterized in that: The preparation method meets at least one of the following characteristics: (1) The mass of the red phosphorus accounts for 1% to 50% of the total mass of the red phosphorus and the porous hard carbon; (2) The mass of the soft carbon precursor accounts for 1% to 10% of the total mass of the phosphorus-carbon composite material and the soft carbon precursor.
5. The preparation method according to claim 1, characterized in that: The preparation method meets at least one of the following characteristics: (1) The temperature of the first heat treatment is 460°C to 600°C, and the time is 0.5 h to 2 h; (2) The first heat treatment is performed under vacuum conditions; (3) The temperature of the second heat treatment is 300°C to 450°C, and the time is 2 h to 6 h; (4) The second heat treatment is performed under nitrogen or an inert atmosphere.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The soft carbon precursor includes at least one of ethylene tar and coal tar.
7. The preparation method according to any one of claims 1 to 5, characterized in that In the preparation of the phosphorus-carbon composite material, after the first heat treatment step is completed, a step of washing with carbon disulfide is also included.
8. The preparation method according to any one of claims 1 to 5, characterized in that: The preparation of the porous hard carbon comprises the following steps: The sodium lignin sulfonate, sodium chloride and water are mixed and freeze-dried to obtain a porous hard carbon precursor powder; The porous hard carbon precursor powder is subjected to a third heat treatment and acid cleaning to prepare pre-carbonized porous hard carbon; The pre-carbonized porous hard carbon is subjected to a fourth heat treatment to prepare the porous hard carbon; wherein the temperature of the fourth heat treatment is higher than the temperature of the third heat treatment.
9. The preparation method according to claim 8, characterized in that: The preparation step of the porous hard carbon satisfies at least one of the following characteristics: (1) The mass ratio of the sodium lignin sulfonate to the sodium chloride is (0.1-9):1; (2) The temperature of the third heat treatment is 400°C to 800°C, and the time is 2 h to 6 h; (3) The temperature of the fourth heat treatment is 900°C to 1500°C, and the time is 2 h to 10 h; (4) The freeze-drying treatment comprises: freezing the mixture of sodium lignin sulfonate, sodium chloride and water at -60°C to -50°C for 12 h to 24 h, and then drying it under vacuum conditions for 24 h to 48 h; (5) The acid used for the acid cleaning includes at least one of a hydrochloric acid solution and a sulfuric acid solution; (6) The acid concentration used in the acid cleaning is 0.01 mol / L~10 mol / L.
10. A modified phosphorus-carbon composite material, characterized in that: The modified phosphorus-carbon composite material is prepared by the preparation method according to any one of claims 1 to 9.
11. A modified phosphorus-carbon composite material, characterized in that: The invention comprises porous hard carbon, red phosphorus and a soft carbon layer. The red phosphorus is arranged inside the pores and on the outer surface of the porous hard carbon, and the soft carbon layer covers at least part of the surface of the porous hard carbon and the red phosphorus.
12. The modified phosphorus-carbon composite material according to claim 11, characterized in that: The modified phosphorus-carbon composite material meets at least one of the following characteristics: (1) The red phosphorus accounts for 0.5% to 30% of the total mass of the modified phosphorus-carbon composite material; (2) The mass of the soft carbon layer accounts for 0.5% to 5% of the total mass of the modified phosphorus-carbon composite material.
13. Use of the modified phosphorus-carbon composite material according to any one of claims 11 to 12 in preparing a negative electrode.
14. A negative electrode, characterized in that: It comprises a current collector and a negative electrode active layer arranged on the surface of the current collector, wherein the negative electrode active layer comprises the modified phosphorus-carbon composite material according to any one of claims 11 to 12.
15. A battery, characterized in that: The invention comprises a positive electrode, a separator and the negative electrode as claimed in claim 14 which are stacked.
16. An electrical device, characterized in that: Comprising the battery of claim 15.
Citation Information
Cited By
Composite material as well as preparation method and application thereof