Lithium cobalt oxide 4.53 V high-voltage lithium ion battery electrolyte and lithium ion battery
By using isocyanate additives to form passivation films and fluorocarboxylate solvents in lithium-ion batteries, the impact of oxidation and decomposition of positive electrode materials and negative electrode interface morphology in lithium-ion batteries is solved. The problem of achieving higher electrochemical performance and capacity retention.
Patent Information
- Application Number
- CN202310535900.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
The positive electrode material of existing lithium-ion batteries is easily oxidized and decomposed at high voltages, generating gas and heat, and the interface morphology of the negative electrode affects the rapid charging performance. It is necessary to develop new film forming additives to protect the positive and negative electrode materials and reduce the interface impedance.
The isocyanate additive with the structure of formula (I) is used to form a passivation film at the positive electrode interface, and the fluorocarboxylate solvent with the structure of formula (II) is used to broaden the electrochemical window of the electrolyte solution, and combine it with non-water Organic solvents, electrolyte lithium salts and conventional additives form a non-aqueous electrolyte solution of lithium cobalt oxide 4.53V high-voltage lithium-ion battery.
Effectively protect the positive electrode material, inhibit solvent redox, improve the electrochemical performance and capacity retention rate of the battery, broaden the electrochemical window of the electrolyte, and enhance the cycle stability and high-temperature storage performance of the battery.
Smart Images

Figure BDA0004226173150000021 
Figure BDA0004226173150000031 
Figure BDA0004226173150000032
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium cobalt oxide 4.53V high-voltage lithium ion battery electrolyte and a lithium ion battery. Background Art
[0002] Lithium-ion batteries are widely used in 3C digital products due to their high operating voltage, high energy density, long life, wide operating temperature range and environmental friendliness. Nowadays, thinness and high energy density are gradually becoming the trend of battery development, especially for 3C digital products. With the intelligence and diversification of smartphones, people use their phones more and more frequently, so they require mobile phones to have more power, lighter weight, and fast charging performance.
[0003] In order to improve the energy density of lithium-ion batteries, a common measure is to increase the charging cut-off voltage of the positive electrode material, such as the voltage of commercial cobalt-acid lithium-ion batteries from 4.2V→4.35V→4.4V→4.45V→4.48V→4.55V. However, the positive electrode material will have certain defects under high voltage. For example, the high-voltage positive electrode active material has strong oxidizing properties when it is in a lithium-deficient state, and the electrolyte is easily oxidized and decomposed, generating a large amount of gas and heat; in addition, the high-voltage positive electrode active material itself is also very unstable when it is in a lithium-deficient state, and some side reactions are prone to occur, such as the release of oxygen and the dissolution of transition metal ions. Similarly, the quality of the negative electrode interface morphology also seriously affects the fast charging performance of the battery, requiring the additive to form a passivation film at the negative electrode reduction with better performance and better kinetic characteristics.
[0004] Therefore, it is necessary to develop new film-forming additives that can form a passivation film at the positive and negative electrodes to protect the positive electrode material or the negative electrode material, while reducing the interface impedance between the positive and negative electrodes and inhibiting solvent redox. Summary of the invention
[0005] In view of the deficiencies and needs of the prior art, the present invention provides a non-aqueous electrolyte for a lithium cobalt oxide 4.53V high-voltage lithium-ion battery. The isocyanate additive having a structure of formula (I) in the electrolyte can be oxidized and decomposed at the positive electrode interface under high voltage to form a passivation film, which has a certain protective effect on the positive electrode material. The fluorocarboxylic acid ester substance having a structure of formula (II) as a solvent can better broaden the electrochemical window of the electrolyte.
[0006] In order to achieve the above object, the non-aqueous electrolyte of the lithium cobalt oxide 4.53V high-voltage lithium ion battery of the present invention comprises a non-aqueous organic solvent, an electrolyte lithium salt and an additive, wherein the additive comprises a conventional additive and an isocyanate additive having a structure of formula (I), and the non-aqueous organic solvent comprises a fluorocarboxylate solvent having a structure of formula (II), and the structure of formula (I) and the structure of formula (II) are as follows:
[0007]
[0008] Wherein, R1 is independently selected from aromatic hydrocarbons, methyl, ethyl, trifluoromethyl, trifluoroethyl and other fluoroalkanes or other halogenated hydrocarbons, and the aromatic hydrocarbon ring may be connected with alkyl, alkenyl, alkynyl, aromatic group, isocyanate group, halogen, etc.; R2 and R3 are independently selected from aromatic hydrocarbons, methyl, ethyl and other alkyl groups, and any one of alkenyl, alkynyl and fluoroalkanes, and the number of carbon atoms in the alkyl and fluoroalkyl groups is less than 4.
[0009] Furthermore, in some embodiments of the present invention, the amount of the isocyanate additive having the structure of formula (I) added is 0.5% to 3% of the total mass of the electrolyte.
[0010] Furthermore, in some embodiments of the present invention, the amount of the fluorocarboxylic acid ester solvent having the structure of formula (II) added is 5.0% to 20.0% of the total mass of the electrolyte.
[0011] Furthermore, in some embodiments of the present invention, the isocyanate additive having the structure of formula (I) is selected from the compounds having the structures shown in (1)-(6):
[0012]
[0013] Furthermore, in some embodiments of the present invention, the fluorocarboxylic acid ester solvent having the structure of formula (II) is selected from the compounds having the structures shown in (7)-(9):
[0014]
[0015] Further, in some embodiments of the present invention, the conventional additives are selected from one or more of fluoroethylene carbonate (FEC), succinonitrile (SN), adiponitrile (ADN), 1,3,6-hexanetrinitrile (HTCN), 1,2-bis(cyanoethoxy)ethane (DENE), 1,3-propane sultone (PS), 1,3-propylene sultone (PST), vinyl vinylene carbonate (VEC), dithiodiphenylamine sulfate (DTD), tris(trimethyl)silane borate (TMSB) and tris(trimethyl)silanephosphine borate (TMSP), tris(tripropargyl) phosphate (TPP), tris(triallyl) phosphate (TAP), etc.
[0016] Furthermore, in some embodiments of the present invention, the amount of the conventional additive added is 5.0% to 30.0% of the total mass of the electrolyte.
[0017] Further, in some embodiments of the present invention, the conventional additives include fluoroethylene carbonate (FEC), 1,3-propane sultone (PS), adiponitrile (ADN) and 1,2-bis(cyanoethoxy)ethane (DENE).
[0018] Preferably, in some embodiments of the present invention, the conventional additives further include tris(tripropargyl) phosphate (TPP) and diethyl sulfate (DTD).
[0019] Furthermore, in some embodiments of the present invention, the conventional additives include 10.0% to 20.0% of fluoroethylene carbonate (FEC) accounting for the total mass of the electrolyte, 2.0% to 6.0% of 1,3-propane sultone (PS) accounting for the total mass of the electrolyte, 1.0% to 5.0% of adiponitrile (ADN) accounting for the total mass of the electrolyte, and 0.5% to 2.0% of 1,2-bis(cyanoethoxy)ethane (DENE) accounting for the total mass of the electrolyte.
[0020] Furthermore, in some embodiments of the present invention, the conventional additives include 10.0% to 20.0% of fluoroethylene carbonate (FEC), 2.0% to 6.0% of 1,3-propane sultone (PS), 1.0% to 5.0% of adiponitrile (ADN), 0.5% to 2.0% of 1,2-bis(cyanoethoxy)ethane (DENE), 0.1% to 0.5% of tris(tripropargyl) phosphate (TPP), and 0.5% to 2.0% of divinyl sulfate (DTD), based on the total mass of the electrolyte.
[0021] Furthermore, in some embodiments of the present invention, the electrolyte lithium salt is selected from one or more of lithium hexafluorophosphate, lithium difluorosulfonyl imide, lithium tetrafluoroborate and lithium difluorophosphate.
[0022] Furthermore, in some embodiments of the present invention, the amount of the electrolyte lithium salt added is 13.5% to 25.0% of the total mass of the electrolyte; preferably, the electrolyte lithium salt is a mixed lithium salt of lithium hexafluorophosphate, lithium difluorophosphate, and lithium bis(fluorosulfonyl)imide; more preferably, the amount of the lithium hexafluorophosphate added is 12.5% to 18.0% of the total mass of the electrolyte, the amount of the lithium difluorophosphate added is 0.5% to 2.0% of the total mass of the electrolyte, and the amount of the lithium bis(fluorosulfonyl)imide added is 1% to 5.0% of the total mass of the electrolyte.
[0023] Furthermore, in some embodiments of the present invention, the non-aqueous organic solvent is selected from carbonate solvents, carboxylate solvents, fluorinated carbonate solvents, fluorinated carboxylate solvents, fluorinated ether solvents and fluorinated nitrile solvents.
[0024] Furthermore, in some embodiments of the present invention, the carbonate solvent includes cyclic carbonate and chain carbonate solvent; wherein the cyclic carbonate solvent includes one or more of ethylene carbonate and propylene carbonate; the chain carbonate includes one or more of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; the carboxylate solvent includes one or more of ethyl acetate, n-propyl acetate, ethyl propionate and propyl propionate; the fluorocarboxylate solvent is selected from compounds (7) to (9).
[0025] Furthermore, in some embodiments of the present invention, the non-aqueous organic solvent contains ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate and fluorocarboxylate solvents; preferably, the mass ratio of ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate and fluorocarboxylate solvents in the non-aqueous organic solvent is 10-20:7-15:25-35:20-30:15-25.
[0026] Preferably, in some embodiments of the present invention, the non-aqueous organic solvent comprises ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate and compound (7) in a mass ratio of 15:10:30:25:20.
[0027] On the other hand, the present invention also provides the aforementioned lithium cobalt oxide 4.53V high-voltage lithium ion battery, wherein the lithium cobalt oxide 4.53V high-voltage lithium ion battery comprises a battery cell formed by lamination or winding of a positive electrode sheet, an isolation membrane and a negative electrode sheet, and the aforementioned lithium cobalt oxide 4.53V high-voltage lithium ion battery electrolyte of the present invention.
[0028] Furthermore, in some embodiments of the present invention, the positive electrode active material of the positive electrode sheet is a lithium cobalt oxide active material, and the compaction density of the positive electrode sheet is 4.1 to 4.45 g / cm 3 .
[0029] Furthermore, in some embodiments of the present invention, the negative electrode active material of the negative electrode sheet is artificial graphite and part of silicon-based materials, wherein the silicon-based materials are selected from silicon oxide, silicon monoxide, elemental silicon materials, etc., and the compaction density of the negative electrode sheet is 1.6-1.8 g / cm 3 .
[0030] Compared with the prior art, the advantages of the present invention mainly lie in that the isocyanate additive with the structure of formula (I) in the electrolyte can be oxidized and decomposed at the positive electrode interface at around 4.48V to form a passivation film, which has a certain protective effect on the positive electrode material; in addition, the fluorocarboxylic acid ester substance with the structure of formula (II) in the electrolyte as a solvent can better broaden the electrochemical window of the electrolyte. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Additional aspects and advantages of the present invention will be given in part in the following description, and part will become apparent from the following description, or will be understood through the practice of the present invention. It should be understood that the following description is only used to explain the present invention and is not intended to limit the present invention.
[0032] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0033] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.
[0034] Example 1
[0035] Preparation of electrolyte: In a glove box filled with argon, ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate and compound (7) were mixed in a mass ratio of EC:PC:EP:PP:compound (7) = 15:10:30:25:20, and then lithium hexafluorophosphate accounting for 15.0% of the total mass of the electrolyte and lithium difluorophosphate accounting for 1.0% of the total mass of the electrolyte, and lithium difluorosulfonyl imide accounting for 3.0% of the total mass of the electrolyte were slowly added to the mixed solution, and finally an isocyanate additive (compound 2) accounting for 1.0% of the total mass of the electrolyte was added, and the mixture was stirred evenly to obtain the lithium ion battery electrolyte of Example 1.
[0036] Preparation of lithium-ion batteries:
[0037] The positive electrode active material lithium cobalt oxide, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an N-methylpyrrolidone solvent system in a mass ratio of 95:3:2, and then coated on an aluminum foil, dried, and cold pressed to obtain a positive electrode sheet.
[0038] The negative electrode active material artificial graphite, silicon oxide, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are fully stirred and mixed in a deionized water solvent system in a mass ratio of 88:8:2.5:0.5:1, and then coated on a copper foil, dried, and cold pressed to obtain a negative electrode sheet.
[0039] Polyethylene (PE) is used as a base film and a nano-aluminum oxide coating is coated on the base film as an isolation film.
[0040] The positive electrode sheet, the isolation film and the negative electrode sheet are stacked in sequence and then wound in the same direction to obtain a bare cell, the bare cell is placed in an outer package, the prepared electrolyte is injected, and a high-voltage lithium cobalt oxide lithium-ion battery is obtained after packaging, 45°C storage, high-temperature fixture formation, secondary packaging, and capacity division.
[0041] Embodiment 2-9
[0042] In Examples 2-9 and Comparative Examples 1-5, except that the components of the electrolyte are added in the proportions shown in Table 1, the rest are the same as in Example 1.
[0043] Table 1 Composition ratio of each component of the electrolyte of Examples 1-9 and Comparative Examples 1-5
[0044]
[0045]
[0046] Effect test
[0047] 1) Normal temperature cycle performance test: At 25°C, charge the divided battery to 4.53V at 0.7C constant current and constant voltage, with a cut-off current of 0.02C, and then discharge it to 3.0V at 0.7C constant current. Repeat this cycle. After 300 charge / discharge cycles, calculate the 300th cycle capacity retention rate. The calculation formula is as follows:
[0048] 300th cycle capacity retention rate (%) = (300th cycle discharge capacity / first cycle discharge capacity) × 100%.
[0049] 2) 85℃ constant temperature storage capacity remaining rate test: First, the battery is charged and discharged once at 0.5C at room temperature (4.53V~3.0V), and the discharge capacity C0 of the battery before storage is recorded. Then the battery is charged to 4.53V at constant current and constant voltage. After that, the battery is placed in an 85℃ constant temperature box for 4h. After the storage is completed, the battery is taken out. After the battery is cooled at room temperature for 24h, the battery is discharged to 3.0V at 0.5C again. The discharge capacity C1 of the battery after storage is recorded, and the capacity remaining rate of the battery after 85℃ constant temperature storage for 4h is calculated. The calculation formula is as follows:
[0050] After 4 hours of constant temperature storage at 85°C, the remaining capacity = C1 / C0*100%.
[0051] 3) 45℃ cycle performance test: At 45℃, charge the divided battery to 4.53V at 0.7C constant current and constant voltage, with a cut-off current of 0.02C, and then discharge it to 3.0V at 0.7C constant current. Repeat this cycle. After 200 cycles of charge / discharge, calculate the 200th cycle capacity retention rate. The calculation formula is as follows:
[0052] 200th cycle capacity retention rate (%) = (200th cycle discharge capacity / first cycle discharge capacity) × 100%.
[0053] Table 2 Battery performance test results of each embodiment
[0054]
[0055]
[0056] From the electrochemical performance of Examples 1-5 and Comparative Example 1 in Table 2, it can be seen that the novel additive (I) of the present invention can improve the electrochemical performance of the 4.53V high-voltage lithium cobalt oxide battery, but the effect of using the novel additive of the present invention alone is not particularly good, mainly because the passivation film formed by oxidation of the single additive at the positive electrode interface has a single component, and only the solvent ethylene carbonate plays a role in the negative electrode film formation. The addition amount is as described in the text, and the expected experimental effect cannot be achieved if the addition amount exceeds the amount described in the present invention.
[0057] From the electrochemical properties of Examples 6-9 and Comparative Example 6 in Table 2, it can be seen that the new additives described in the present invention are used in combination with other types of additives, which has a better effect. This is mainly because the new additives described in the present invention can react and decompose at the interface of the positive electrode material to form a passivation film, inhibit the dissolution of cobalt in the positive electrode material, prevent the migration of cobalt ions to the interface of the negative electrode material, catalyze the reduction and decomposition of the solvent, and have a certain effect on the protection of the positive and negative electrodes.
[0058] It is easy for a person skilled in the art to understand that, according to the disclosure and teaching of the above description, a person skilled in the art to which the present invention belongs can also change and modify the above implementation mode, and any modification, equivalent replacement and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of explanation and do not constitute any limitation to the present invention.
Claims
1. A 4.53V high voltage lithium-ion battery non-aqueous electrolyte for lithium cobalt oxide, characterized in that: The lithium ion battery non-aqueous electrolyte comprises a non-aqueous organic solvent, an electrolyte lithium salt and an additive, wherein the additive comprises a conventional additive and an isocyanate additive having a structure of formula (I), and the non-aqueous organic solvent comprises a fluorocarboxylate solvent having a structure of formula (II), wherein the structure of formula (I) and the structure of formula (II) are as follows: Wherein, R1 is independently selected from aromatic hydrocarbons, methyl, ethyl, trifluoromethyl, trifluoroethyl or other halogenated hydrocarbons, and the aromatic hydrocarbon ring may be connected with alkyl, alkenyl, alkynyl, aromatic group, isocyanate group, halogen; R2 and R3 are independently selected from aromatic hydrocarbons, methyl, ethyl alkyl, and any one of alkenyl, alkynyl and fluoroalkane, and the number of carbon atoms in the alkyl and fluoroalkyl groups is less than 4.
2. The lithium cobalt oxide 4.53V high voltage lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The isocyanate additive having the structure of formula (I) is selected from the compounds having the structures shown in (1) to (6): Preferably, the amount of the isocyanate additive having the structure of formula (I) added is 0.5% to 3% of the total mass of the electrolyte.
3. The non-aqueous electrolyte for lithium cobalt oxide 4.53V high voltage lithium ion battery according to claim 1, characterized in that: The fluorocarboxylic acid ester solvent having the structure of formula (II) is selected from the compounds having the structures shown in (7) to (9): Preferably, the amount of the fluorocarboxylic acid ester solvent having the structure of formula (II) added is 5.0% to 20.0% of the total mass of the electrolyte.
4. The lithium cobalt oxide 4.53V high voltage lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The conventional additives are selected from one or more of fluoroethylene carbonate (FEC), succinonitrile (SN), adiponitrile (ADN), 1,3,6-hexanetrinitrile (HTCN), 1,2-bis(cyanoethoxy)ethane (DENE), 1,3-propane sultone (PS), 1,3-propylene sultone (PST), vinyl vinyl carbonate (VEC), divinyl sulfate (DTD), tris(trimethyl)silane borate (TMSB) and tris(trimethyl)silanephosphine borate (TMSP), tris(tripropargyl) phosphate (TPP), and tris(triallyl) phosphate (TAP); preferably, the addition amount of the conventional additives accounts for 5.0% to 30.0% of the total mass of the electrolyte.
5. The lithium cobalt oxide 4.53V high voltage lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The conventional additives include fluoroethylene carbonate (FEC), 1,3-propane sultone (PS), adiponitrile (ADN) and 1,2-bis(cyanoethoxy)ethane (DENE); preferably, the conventional additives further include tris(tripropargyl) phosphate (TPP) and divinyl sulfate (DTD).
6. The non-aqueous electrolyte for lithium cobalt oxide 4.53V high voltage lithium ion battery according to claim 1, characterized in that: The conventional additives include 10.0% to 20.0% of fluoroethylene carbonate (FEC) accounting for 10.0% to 20.0% of the total mass of the electrolyte, 2.0% to 6.0% of 1,3-propane sultone (PS) accounting for 2.0% to 6.0% of the total mass of the electrolyte, 1.0% to 5.0% of adiponitrile (ADN) accounting for 1.0% to 5.0% of the total mass of the electrolyte, and 0.5% to 2.0% of 1,2-bis(cyanoethoxy)ethane (DENE) accounting for 0.5% to 2.0% of the total mass of the electrolyte.
7. The lithium cobalt oxide 4.53V high voltage lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The conventional additives include 10.0% to 20.0% of fluoroethylene carbonate (FEC) accounting for 10.0% to 20.0% of the total mass of the electrolyte, 2.0% to 6.0% of 1,3-propane sultone (PS) accounting for 1.0% to 5.0% of the total mass of the electrolyte, 0.5% to 2.0% of 1,2-bis(cyanoethoxy)ethane (DENE) accounting for 0.1% to 0.5% of the total mass of the electrolyte, tris(tripropargyl) phosphate (TPP) accounting for 0.5% to 2.0% of the total mass of the electrolyte, and 0.5% to 2.0% of vinyl sulfate (DTD) accounting for 0.5% to 2.0% of the total mass of the electrolyte.
8. The non-aqueous electrolyte for lithium cobalt oxide 4.53V high voltage lithium ion battery according to claim 1, characterized in that: The electrolyte lithium salt is selected from one or more of lithium hexafluorophosphate, lithium difluorosulfonyl imide, lithium tetrafluoroborate and lithium difluorophosphate; preferably, the electrolyte lithium salt is added in an amount of 13.5% to 25.0% of the total mass of the electrolyte; preferably, the electrolyte lithium salt is a mixed lithium salt of lithium hexafluorophosphate, lithium difluorophosphate and lithium bisfluorosulfonyl imide; more preferably, the lithium hexafluorophosphate is added in an amount of 12.5% to 18.0% of the total mass of the electrolyte, the lithium difluorophosphate is added in an amount of 0.5% to 2.0% of the total mass of the electrolyte, and the lithium bisfluorosulfonyl imide is added in an amount of 1% to 5.0% of the total mass of the electrolyte.
9. The lithium cobalt oxide 4.53V high voltage lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The non-aqueous organic solvent is selected from carbonate solvents, carboxylate solvents, fluorinated carbonate solvents, fluorinated carboxylate solvents, fluorinated ether solvents and fluorinated nitrile solvents; preferably, the carbonate solvents include cyclic carbonates and chain carbonate solvents; wherein the cyclic carbonate solvents include one or more of ethylene carbonate and propylene carbonate; the chain carbonate includes one or more of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; the carboxylate solvents include one or more of ethyl acetate, n-propyl acetate, ethyl propionate and propyl propionate; the fluorinated carboxylate solvents Selected from compounds (7) to (9); preferably, the non-aqueous organic solvent comprises ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate and a fluorocarboxylic acid ester solvent; preferably, the mass ratio of ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate and a fluorocarboxylic acid ester solvent in the non-aqueous organic solvent is 10-20:7-15:25-35:20-30:15-25; preferably, the non-aqueous organic solvent comprises ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate and compound (7) in a mass ratio of 15:10:30:25:
20.
10. A 4.53V high voltage lithium-ion battery of lithium cobalt oxide, characterized in that: The cobalt oxide lithium 4.53V high voltage lithium ion battery comprises a battery cell formed by laminating or winding a positive electrode sheet, a separator and a negative electrode sheet, and a cobalt oxide lithium 4.53V high voltage lithium ion battery electrolyte according to any one of claims 1 to 9. Preferably, the positive electrode active material of the positive electrode sheet is a cobalt oxide lithium active material, and the compaction density of the positive electrode sheet is 4.1 to 4.45 g / cm 3 Preferably, the negative electrode active material of the negative electrode sheet is artificial graphite and part of silicon-based materials, wherein the silicon-based materials are selected from silicon oxide, silicon monoxide, elemental silicon materials, etc., and the compaction density of the negative electrode sheet is 1.6-1.8 g / cm 3 .
Citation Information
Cited By
High-safety lithium ion battery and preparation method thereof
CN119905641A
Electrolyte additive, composition for high-voltage electrolyte, high-voltage electrolyte and preparation method thereof, and lithium ion battery
CN120149543A
Electrolyte additive, composition for high-voltage electrolyte, high-voltage electrolyte and preparation method thereof, lithium ion battery
CN120149543B