Modified solid electrolyte as well as preparation method and application thereof
By coating the modified layers of polyvinylidene fluoride-hexafluoropropylene, lithium bistrifluoromethanesulfonimide and molybdenum disulfide on the surface of LATP solid electrolyte, the problem of instability of the interface between lithium metal anode and LATP electrolyte is solved, and the problem of instability of the lithium metal anode and LATP electrolyte is improved. The electrochemical and mechanical properties of lithium-ion batteries are provided.
Patent Information
- Application Number
- CN202411221011.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-22
AI Technical Summary
The interface contact between the LATP solid electrolyte and the lithium metal anode is poor and unstable, resulting in the growth of lithium dendrites and the irreversible reduction reaction of Ti elements, reducing ionic conductivity and battery performance.
Coating modified layers on the surface of LATP solid electrolytes, including polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), lithium bistrifluoromethanesulfonimide (LiTFSI), and molybdenum disulfide (MoS2) to improve the electrode interface Contact and stability.
The interface impedance is reduced, the ion conductivity and lithium ion migration number are improved, the growth of lithium dendrites is suppressed, and the circulation stability and discharge specific capacity of lithium ion batteries are increased.
Smart Images

Figure CN119009075A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a modified solid electrolyte and a preparation method and application thereof. Background Art
[0002] In today's mobile Internet environment, lithium-ion batteries are widely used in portable electronic devices and electric vehicles. However, traditional liquid electrolytes have the risk of leakage and explosion, which hinders their development. The severe short circuit caused by lithium dendrite growth and the capacity decay caused by interface failure in the battery hinder their further application. The demand for high energy density and high safety has promoted the development of solid-state lithium batteries. As a key component of solid-state lithium-ion batteries, solid-state electrolytes have been widely studied in recent years. Among various solid-state electrolytes, the sodium superion conductor (NASICON) structured solid electrolyte with high ionic conductivity and low cost has a wide electrochemical window, high ionic conductivity and good structural stability. In the case of most ceramic electrolytes that react with water and air, NASICON-type solid electrolytes show extremely high stability, making them very attractive solid-state electrolyte materials. The more mature materials studied in the NASICON system are Li 1+x Al x Ti 2-x (PO4)3 (LATP) and Li 1+x Al x Ge 2-x (PO4)3 (LAGP). The Ge element contained in LAGP is too expensive and has not yet been put into practical application. LATP has low raw material cost, high ion conductivity, simple preparation process, and is stable to water and air. It is considered to be one of the most promising solid electrolyte materials for industrial application. Despite the above advantages, the instability of lithium metal anodes widely present in NASICONON electrolytes has limited its development.
[0003] There are two main obstacles in the practical application of LATP. The first is the interface contact problem between the rigid ceramic material and the electrode. The poor physical contact between the solid electrolyte and the two solid surfaces of lithium metal causes a large interface impedance, which hinders the Li + The high-valent Ti element in LATP is easily reduced at low potentials, and the interface between LATP and the lithium metal anode is unstable, which triggers the Ti reaction when in physical contact. 4+ To Ti 3+ The irreversible reduction reaction forms a large amount of interfacial compounds, which leads to a sharp decrease in ionic conductivity and structural collapse. The mixed ion conductive layer formed will conduct electrons, causing the battery to short-circuit and deteriorate in performance. All of these will eventually lead to battery failure. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the poor or unstable interface contact between the LATP solid electrolyte and the lithium metal anode in the prior art, which leads to side reactions between the LATP solid electrolyte and the lithium metal, such as the growth of lithium dendrites or the high-valent Ti element in the LATP being converted from Ti to 4+ To Ti 3+ The irreversible reduction reaction of the LATP solid electrolyte reduces the defect of the interface impedance between the LATP solid electrolyte and the electrode interface, and provides a modified solid electrolyte and its preparation method and application. The modified solid electrolyte of the present invention avoids direct contact between Li and LATP by coating a modified layer on the surface of the LATP solid electrolyte, while achieving the effect of good contact between the modified solid electrolyte and the electrode, and the interface impedance between the modified solid electrolyte and the electrode interface is also reduced.
[0005] The present invention solves the above technical problems through the following technical solutions.
[0006] The present invention provides a modified solid electrolyte, which comprises a solid electrolyte and a modified layer;
[0007] Wherein, the modified layer includes polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) and molybdenum disulfide (MoS2); the mass ratio of the polyvinylidene fluoride-hexafluoropropylene and the lithium bis(trifluoromethanesulfonyl imide) is 1: (1-3.5); and the modified layer is coated on the surface of the solid electrolyte.
[0008] In the present invention, the solid electrolyte is, for example, a LATP solid electrolyte, wherein the LATP is Li 1+x Al x Ti 2-x (PO4)3, wherein x satisfies 0≤x≤0.5, for example, x is 0.3.
[0009] In the present invention, the solid electrolyte is in the shape of a disc, for example.
[0010] In the present invention, preferably, the thickness of the solid electrolyte is 0.5-2 mm, for example, 1.1 mm.
[0011] In the present invention, preferably, the mass ratio of the solid electrolyte to the polyvinylidene fluoride-hexafluoropropylene is (0.2-2):1, for example, 0.75:1.
[0012] In the present invention, preferably, the thickness of the modified layer is 10-30 μm, more preferably 20-30 μm, for example 26.4 μm, 26.7 μm, 27.3 μm, 27.4 μm, 28.8 μm, 29.6 μm or 30.0 μm.
[0013] In the present invention, preferably, in the modified layer, the polyvinylidene fluoride-hexafluoropropylene is in a spherical connected structure, and the lithium bis(trifluoromethanesulfonyl)imide and the molybdenum disulfide are dispersed on the surface of the polyvinylidene fluoride-hexafluoropropylene.
[0014] In the present invention, preferably, the mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the lithium bis(trifluoromethanesulfonyl)imide is 1:(2-3), such as 1:2, 1:2.5 or 1:3.
[0015] In the present invention, preferably, the mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the molybdenum disulfide is 1:(0.02-0.2), more preferably 1:(0.05-0.15), for example 1:0.02, 1:0.05, 1:0.1, 1:0.15 or 1:0.2.
[0016] In a specific embodiment of the present invention, the solid electrolyte is a LATP solid electrolyte, and the LATP solid electrolyte has a mass of 0.24 g, a diameter of 10 mm, and a thickness of 1.1 mm.
[0017] In a specific embodiment of the present invention, the modified solid electrolyte is a modified solid electrolyte of any of the following schemes:
[0018] Scheme 1: The modified solid electrolyte comprises a LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.8:0.032;
[0019] Scheme 2: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.8:0.016;
[0020] Scheme 3: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.8:0.048;
[0021] Scheme 4: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bistrifluoromethanesulfonyl imide and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bistrifluoromethanesulfonyl imide and the molybdenum disulfide is 0.24:0.32:0.64:0.032;
[0022] Scheme 5: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bistrifluoromethanesulfonyl imide and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bistrifluoromethanesulfonyl imide and the molybdenum disulfide is 0.24:0.32:0.96:0.032;
[0023] Scheme 6: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.96:0.0064;
[0024] Scheme 7: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.96:0.064.
[0025] The present invention provides a method for preparing a modified solid electrolyte, which comprises the following steps:
[0026] The modified layer solution is coated on the solid electrolyte and the solvent is removed;
[0027] Wherein, the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), molybdenum disulfide (MoS2) and solvent;
[0028] The mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the lithium bis(trifluoromethanesulfonyl)imide is 1:(1-3.5).
[0029] In the present invention, preferably, the preparation process of the modified solid electrolyte is carried out in a glove box.
[0030] Preferably, in the glove box, H2O<0.1ppm and O2<0.1ppm.
[0031] In the present invention, preferably, the coating amount of the modified layer liquid per unit area on the solid electrolyte is 0.25-0.64 μL / mm 2 , for example 0.38 μL / mm 2 .
[0032] In the present invention, preferably, the mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the lithium bis(trifluoromethanesulfonyl)imide is 1:(2-3), such as 1:2, 1:2.5 or 1:3.
[0033] In the present invention, preferably, the mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the molybdenum disulfide is 1:(0.02-0.2), more preferably 1:(0.05-0.15), for example 1:0.02, 1:0.05, 1:0.1, 1:0.15 or 1:0.2.
[0034] In the present invention, preferably, the solvent is selected from N,N-dimethylformamide (DMF) and / or N-methylpyrrolidone (NMP).
[0035] In the present invention, preferably, the usage ratio of the polyvinylidene fluoride-hexafluoropropylene and the solvent is (0.16-0.48) g: (2-5) mL, for example, 0.32 g: 3 mL.
[0036] In the present invention, preferably, the modified layer liquid is prepared by the following method, which specifically comprises the following steps:
[0037] S1, dissolving the polyvinylidene fluoride-hexafluoropropylene and the lithium bis(trifluoromethanesulfonyl)imide in the solvent, stirring to obtain a viscous solution;
[0038] S2, adding the molybdenum disulfide to the viscous solution obtained in step S1, and stirring.
[0039] Preferably, in step S1, the stirring temperature is 25-70°C, for example, 60°C.
[0040] Preferably, in step S1, the stirring time is 10-20 hours, for example, 12 hours.
[0041] Preferably, in step S2, the stirring temperature is 25-70°C, for example 60°C.
[0042] Preferably, in step S2, the stirring time is 2-8 hours, such as 3 hours or 4 hours.
[0043] In the present invention, preferably, the solvent is removed by heating, and the heating temperature is 60-120°C, such as 100°C.
[0044] In the present invention, the modified layer liquid is coated on the solid electrolyte, and after heating to completely volatilize the solvent, the modified solid electrolyte coated with the modified layer is obtained.
[0045] Preferably, the thickness of the modified layer is 10-30 μm, more preferably 20-30 μm, for example, 26.4 μm, 26.7 μm, 27.3 μm, 27.4 μm, 28.8 μm, 29.6 μm or 30.0 μm.
[0046] In the present invention, the solid electrolyte is in the shape of a disc, for example.
[0047] In the present invention, preferably, the thickness of the solid electrolyte is 0.5-2 mm, for example, 1.1 mm.
[0048] In the present invention, the solid electrolyte is, for example, a LATP solid electrolyte, wherein the LATP is Li 1+x Al x Ti 2-x (PO4)3, wherein x satisfies 0≤x≤0.5, for example, x is 0.3.
[0049] Preferably, the LATP solid electrolyte is prepared by the following method, which specifically comprises the following steps:
[0050] a. Add a lithium source, an aluminum source, and a titanium source to ethanol and stir to dissolve to obtain a solution A; add a phosphorus source to water and stir to dissolve to obtain a solution B; add the solution B dropwise to the solution A and stir to obtain a mixed solution C;
[0051] Wherein, the volume ratio of the ethanol to the water is (1-10): (1-10);
[0052] The molar ratio of the lithium source, the aluminum source, the titanium source, and the phosphorus source is (1+x):x:(2-x):3; x is the molar number of the aluminum source;
[0053] b. Using ammonia water to adjust the pH of the mixed solution C obtained in step a to neutral or alkaline, stirring, and obtaining a LATP precursor solution;
[0054] c. Drying, calcining, ball-milling and sieving the LATP precursor solution obtained in step b to obtain LATP solid electrolyte powder;
[0055] d. The LATP solid electrolyte powder obtained in step c is tableted, calcined, and polished to obtain a LATP solid electrolyte.
[0056] In step a, preferably, the water is deionized water, and the ethanol is anhydrous ethanol.
[0057] In step a, preferably, the stirring is carried out in a magnetic stirring manner, and the purpose of the stirring is to mix the solution evenly.
[0058] In step a, preferably, the lithium source is selected from one or more of lithium nitrate, lithium carbonate and lithium hydroxide.
[0059] In step a, preferably, the aluminum source is selected from one or more of aluminum hydroxide, aluminum nitrate, aluminum chloride and aluminum oxide.
[0060] In step a, preferably, the titanium source is selected from tetrabutyl titanate and / or isopropyl titanate.
[0061] In step a, preferably, the phosphorus source is selected from one or more of diammonium phosphate, phosphoric acid, and diammonium hydrogen phosphate.
[0062] In a specific embodiment of the present invention, the lithium source, the aluminum source, the titanium source, the phosphorus source, the anhydrous ethanol and the water are used in a ratio of 1.3 mmol: 0.3 mmol: 1.7 mmol: 3 mmol: 10 mL: 10 mL.
[0063] In step b, preferably, the pH of the mixed solution C is 7-10, for example 9.
[0064] In step b, the purpose of the stirring is to make the mixed solution mixed evenly.
[0065] In step b, preferably, the stirring time is 1-10 hours, for example 1 hour.
[0066] In step c, preferably, the drying temperature is 50-100°C, such as 80°C.
[0067] In step c, preferably, the drying time is 2-24 hours, for example 12 hours.
[0068] In step c, preferably, the calcination temperature is 600-900°C, for example 800°C.
[0069] In step c, preferably, the calcination time is 4-10 hours, such as 6 hours.
[0070] In step d, the obtained LATP solid electrolyte is generally in the form of a ceramic sheet.
[0071] In step d, the obtained LATP solid electrolyte generally has good density and no obvious pores.
[0072] In some preferred embodiments of the present invention, the solid electrolyte is a LATP solid electrolyte, the mass of the LATP solid electrolyte is 0.24 g, the diameter is 10 mm, and the thickness is 1.1 mm; the coating volume of the modified layer solution is 20-50 μL, for example, 30 μL.
[0073] In a specific embodiment of the present invention, the preparation method of the modified solid electrolyte is any of the following schemes:
[0074] Scheme 1: coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.8 g: 3 mL: 0.032 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ;
[0075] Scheme 2: Coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.8 g: 3 mL: 0.016 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ;
[0076] Scheme 3: Apply the modified layer solution on the LATP solid electrolyte and remove the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer solution includes polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.8 g: 3 mL: 0.048 g; the coating amount of the modified layer solution per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ;
[0077] Scheme 4: coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.64 g: 3 mL: 0.032 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ;
[0078] Scheme 5: Coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.96 g: 3 mL: 0.032 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ;
[0079] Scheme 6: Apply the modified layer solution on the LATP solid electrolyte and remove the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer solution includes polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.96 g: 3 mL: 0.0064 g; the coating amount of the modified layer solution per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ;
[0080] Scheme 7: Coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.96 g: 3 mL: 0.064 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 .
[0081] The present invention provides a modified solid electrolyte prepared by the modified solid electrolyte preparation method as described above.
[0082] The present invention also provides a use of the modified solid electrolyte as described above in preparing a lithium ion battery, wherein the lithium ion battery is, for example, a lithium ion symmetrical battery.
[0083] In the present invention, preferably, the method for preparing the lithium-ion symmetrical battery comprises the following steps: assembling lithium sheets on both sides of the modified solid electrolyte respectively.
[0084] The size of the lithium sheet is generally smaller than that of the modified solid electrolyte.
[0085] Preferably, the assembly process is carried out in a glove box, and more preferably, in the glove box, H2O<0.1ppm and O2<0.1ppm.
[0086] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0087] The reagents and raw materials used in the present invention are commercially available.
[0088] The positive and progressive effects of the present invention are:
[0089] The modified solid electrolyte obtained by the present invention can replace the electrolyte and the diaphragm. The modified layer obtained by the present invention on the modified solid electrolyte avoids the direct contact between Li and LATP, so that the modified solid electrolyte has higher ion conductivity and lithium ion migration number, wider electrochemical window, good mechanical properties, and good compatibility with lithium negative electrode; in addition, the modified layer on the modified solid electrolyte can inhibit the growth of lithium dendrites, so that the lithium ion battery made of the modified solid electrolyte can obtain higher discharge specific capacity and long cycle stability, and achieve the effect of good contact between the modified solid electrolyte and the electrode.
[0090] In the modified layer of the modified solid electrolyte of the present invention, polyvinylidene fluoride-hexafluoropropylene has higher ionic conductivity and lower crystallinity than other polymers, and is helpful to form a stable interface; the addition of lithium bis(trifluoromethanesulfonyl)imide can interact with the polymer electrolyte matrix to form a fast carrier conduction channel; the addition of molybdenum disulfide can react with Li metal to form a lithium sulfide interface, promote the uniform deposition of metallic lithium, and thus hinder the growth of lithium dendrites. The modified layer of the present invention reduces the interface impedance between the LATP solid electrolyte and lithium metal, and increases the critical current density of the lithium symmetric battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] Figure 1 This is the X-ray diffraction pattern of the LATP solid electrolyte prepared in step 1 of Example 1.
[0092] Figure 2 This is a scanning electron microscope image of the cross section of the modified solid electrolyte prepared in Example 1.
[0093] Figure 3 This is a scanning electron microscope image of the modified layer on the surface of the modified solid electrolyte prepared in Example 1.
[0094] Figure 4 This is a comparison chart of the electrochemical impedance of the modified solid electrolytes prepared in Examples 1-3, Examples 6-7 and Comparative Examples 1-2.
[0095] Figure 5 This is a comparison diagram of the electrochemical impedance of the modified solid electrolytes prepared in Example 1, Examples 4-5 and Comparative Examples 3-4.
[0096] Figure 6 This is a comparison chart of the critical current density of the modified solid electrolytes prepared in Example 1, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0097] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0098] The reagents or instruments used are not marked with the manufacturer, and are all conventional products that can be purchased through regular channels. The reagent and instrument information involved in the examples and comparative examples of the present invention are shown in Table 1:
[0099] Table 1
[0100]
[0101] Example 1
[0102] This embodiment provides a modified solid electrolyte, and the preparation method thereof adopts the following steps:
[0103] Step 1 Place 98.67mg LiNO3 and 112.5mg Al(NO3)3·9H2O in a beaker containing 10 mL of anhydrous ethanol, stir magnetically to fully dissolve them, and add 578μL Ti(OC4H9)4 and stir thoroughly after complete dissolution, record as solution A, and set aside. Then use deionized water to dissolve 345mg NH4H2PO4 in another beaker, stir magnetically to fully dissolve them, record as solution B. Slowly add solution B to solution A and stir continuously to mix them evenly. After the addition is completed, adjust the pH value to 9 with ammonia water, continue stirring for 1h to age it, and obtain a white LATP precursor solution. Dry the LATP precursor solution at 80℃ for 12h to obtain the LATP precursor. Put the LATP precursor into an agate mortar and grind it into a fine powder, put it into an alumina magnetic boat and vibrate it, place it in a tube furnace and calcine it at 800℃ for 6h, and after cooling, ball mill and sieve it to obtain the LATP solid electrolyte powder. Finally, the obtained powder was placed in a mold and pressed into a 13 mm disc, loaded into an alumina magnetic boat, and placed in a tube furnace and calcined at 800 ° C for 6 h. After cooling, it was polished with sandpaper to obtain a LATP solid electrolyte ceramic disc with a mass of 0.24 g, a diameter of 10 mm, and a thickness of 1.1 mm.
[0104] Step 2: Dissolve 0.32 g PVDF-HFP and 0.8 g LiTFSI in 3 mL DMF, stir at 60 °C for 12 h to obtain a viscous solution, add 32 mg MoS2 powder to the obtained viscous solution, continue stirring at 60 °C for 3 h, take 30 μL of the stirred solution and coat it on the surface of the LATP solid electrolyte prepared in step 1, heat at 100 °C to completely evaporate the solvent, and obtain a modified solid electrolyte.
[0105] The above steps were all completed in a glove box, where H2O<0.1ppm and O2<0.1ppm.
[0106] Example 2
[0107] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Example 1 only in that the mass of MoS2 powder added in step 2 is different. The mass of MoS2 powder added in this embodiment is 16 mg, and the other conditions and operations are the same as those in Example 1.
[0108] Example 3
[0109] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Example 1 only in that the mass of MoS2 powder added in step 2 is different. The mass of MoS2 powder added in this embodiment is 48 mg, and the other conditions and operations are the same as those in Example 1.
[0110] Example 4
[0111] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Embodiment 1 only in that the mass of LiTFSI added in step 2 is different. The mass of LiTFSI powder added in this embodiment is 0.64 g, and the other conditions and operations are the same as those in Embodiment 1.
[0112] Example 5
[0113] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Embodiment 1 only in that the mass of LiTFSI added in step 2 is different. The mass of LiTFSI powder added in this embodiment is 0.96 g, and the other conditions and operations are the same as those in Embodiment 1.
[0114] Example 6
[0115] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Example 1 only in that the mass of MoS2 powder added in step 2 is different. The mass of MoS2 powder added in this embodiment is 6.4 mg, and the other conditions and operations are the same as those in Example 1.
[0116] Example 7
[0117] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Example 1 only in that the mass of MoS2 powder added in step 2 is different. The mass of MoS2 powder added in this embodiment is 64 mg, and the other conditions and operations are the same as those in Example 1.
[0118] Comparative Example 1
[0119] This comparative example provides a modified solid electrolyte, and the preparation method thereof is different from that of Example 1 only in that MoS2 is not added in step 2, and the other conditions and operations are the same as those of Example 1.
[0120] Comparative Example 2
[0121] In this comparative example, LATP solid electrolyte was prepared according to the following steps.
[0122] This comparative example is the same as step 1 in Example 1, but no interface modification is performed.
[0123] Comparative Example 3
[0124] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Embodiment 1 only in that the mass of LiTFSI added in step 2 is different. The mass of LiTFSI powder added in this embodiment is 0.16 g, and the other conditions and operations are the same as those in Embodiment 1.
[0125] Comparative Example 4
[0126] This embodiment provides a modified solid electrolyte, and the preparation method thereof is different from that of Example 1 only in that the mass of LiTFSI added in step 2 is different. The mass of LiTFSI powder added in this embodiment is 1.28 g, and the other conditions and operations are the same as those in Example 1.
[0127] Comparative Example 5
[0128] This comparative example provides a modified solid electrolyte, and the preparation method thereof is different from that of Example 1 only in that the MoS2 powder in step 2 is replaced with bismuth sulfide Bi2S3, and the other conditions and operations are the same as those of Example 1.
[0129] Effect Example
[0130] 1. Structural characterization
[0131] (1) X-ray diffraction analysis
[0132] Figure 1 This is the X-ray diffraction pattern of the LATP solid electrolyte prepared in step 1 of Example 1 obtained by an X-ray diffraction analyzer. From the figure, it can be observed that the diffraction peak position of the X-ray diffraction spectrum of the LATP synthesized in the present invention is consistent with the standard PDF card of LiTi2(PO4)3 (JCPDS 35-0754), which proves that the LATP particles synthesized in the present invention have high crystallinity. Compared with the standard PDF card of LiTi2(PO4)3, the diffraction peak shifts to the right, which is because Al 3+ The doping of Al reduces the lattice constant and d value, which also proves that Al 3+ Successfully doped into the crystal lattice.
[0133] (2) Morphological and structural characterization
[0134] Figure 2 The cross-sectional scanning electron microscope image of the solid electrolyte obtained by scanning electron microscope of the modified solid electrolyte prepared in Example 1 shows that the LATP has a closely bound and uniform grain shape, and there are basically no microcracks and voids, indicating that the ceramic has a high density, which is conducive to Li + Conductivity inside the electrolyte results in high ionic conductivity. The thickness of the modified layer is 30.0 μm and it fits tightly to the surface of the LATP solid electrolyte.
[0135] The thickness of the modified layers of Examples 2-7 and Comparative Examples 1-4 were measured using the same method. The results are shown in Table 2.
[0136] Table 2
[0137]
[0138] The LATP solid electrolyte is modified through a modified layer. By adding an appropriate amount of lithium salt and MoS2, the modified layer plays the role of forming a fast carrier conduction channel and forming a lithium sulfide interface, promoting the uniform deposition of metallic lithium and thus hindering the growth of lithium dendrites, thereby improving the electrochemical performance. Figure 3 This is a scanning electron microscope image of the modified layer on the surface of the modified solid electrolyte prepared in Example 1. From the image, it can be observed that the surface of the modified layer is smooth and is composed of PVDF-HFP spherical particles with a diameter of several microns. The spheres are interconnected to form a three-dimensional conductive network, and MoS2 particles are evenly distributed on the surface of the PVDF-HFP polymer.
[0139] 2. Electrochemical test
[0140] Electrochemical tests were performed by assembling lithium symmetric batteries using an electrochemical workstation and a blue battery working system. The positive and negative electrodes of lithium symmetric batteries are both lithium metals, and are mainly used to evaluate whether solid electrolyte materials will react with lithium metal during the charge and discharge process. A constant current is applied to both sides of the lithium symmetric battery, and the direction changes at a certain time. + The solid electrolyte is continuously dissolved and deposited on the surface of lithium metal, which generates polarization voltage to drive Li + The back-and-forth movement is used to evaluate the stability of the solid electrolyte to lithium and the Li + transmission performance.
[0141] (1) Electrochemical impedance spectroscopy
[0142] Electrochemical impedance spectroscopy test method: Electrochemical impedance spectroscopy is a transient electrochemical technique that uses a small-amplitude sinusoidal voltage or current as a disturbance signal to obtain the impedance response of the electrode system at different frequencies with the help of an impedance spectrum meter. The frequency range of the electrochemical impedance spectroscopy test in this experiment is 10 6 -10 -1 HZ, the amplitude perturbation parameter is 10mV.
[0143] The modified solid electrolytes of Examples 1-7 and Comparative Examples 1-4 were assembled to obtain lithium symmetric batteries. The interface impedance values of LATP and Li were shown in Table 3 through electrochemical impedance spectroscopy testing.
[0144] Table 3
[0145]
[0146] Figure 4 The electrochemical impedance comparison diagram of the modified solid electrolyte prepared for Example 1-3, Example 6-7 and Comparative Example 1-2. Example 1-3 and Example 6-7 control the growth of lithium dendrites by adjusting the addition of MoS2, and the addition amount is 10%, 5%, 15%, 2% and 20% of PVDF-HFP respectively. The difference between Example 1-3, Example 6-7 and Comparative Example 1 is that the addition amount of MoS2 is different, and the addition amount of MoS2 is 10%, 5%, 15%, 2%, 20% and 0% of PVDF-HFP respectively, while Comparative Example 2 does not use modified layer modification. Figure 4 The semicircle in the medium and high frequency region represents the grain boundary impedance of the LATP solid electrolyte after the modified layer is coated, and the semicircle in the low frequency region represents the interface resistance between LATP and Li. Figure 4 It can be seen that, compared with Examples 1-3, Examples 6-7 and Comparative Examples 1-2, when the addition amount of MoS2 is 10% of the addition amount of PVDF-HFP, the interface impedance value is lower, that is, the interface impedance value of Example 1 is the lowest in comparison.
[0147] Figure 5 The electrochemical impedance comparison diagram of the modified solid electrolyte prepared in Example 1, Examples 4-5 and Comparative Examples 3-4 is that the amount of LiTFSI added is different. The addition of LiTFSI does not change the crystal structure of PVDF-HFP, but it will reduce the crystallinity of PVDF-HFP, which is beneficial to improve the migration rate of lithium ions and the ionic conductivity of the solid electrolyte; but when the lithium salt content is too high, agglomeration will occur, thereby hindering the conduction of lithium ions and reducing the mechanical properties of the polymer electrolyte. Therefore, the content of LiTFSI added to PVDF-HFP is crucial. Figure 5 It can be seen that, compared with Example 1, Examples 4-5 and Comparative Examples 3-4, when the addition amount of LiTFSI is 2.5 times the addition amount of PVDF-HFP, the interface impedance value is lower, that is, the interface impedance value of Example 1 is the lowest in comparison.
[0148] (2) Critical current density test
[0149] Critical current density (CCD) is used to evaluate the ability of solid electrolytes to inhibit lithium dendrites. The critical current density is defined as the current density that enables lithium dendrites to grow through the solid electrolyte interface (ESI) and solid electrolyte (SSE) and short-circuit the battery. The critical current density depends not only on the properties of SEI, but also on the SSE thickness, applied stacking pressure, and lithium plating / stripping ability / number of times, etc. For example, the critical current density value increases with the increase of SSE thickness, but decreases with the increase of lithium plating / stripping time / capacity.
[0150] Critical current density test method: The present invention uses a blue electric test system to test the critical current density of a symmetrical battery with metal lithium as an electrode at room temperature. The test is time-controlled, with each charge / discharge controlled for 30 min and each current density increased by 0.1 mA cm -2 .
[0151] The modified solid electrolytes of Examples 1-7 and Comparative Examples 1-4 were assembled to obtain lithium symmetric batteries. Through testing, the values of their critical current densities are shown in Table 4.
[0152] Table 4
[0153]
[0154] The higher the critical current density, the stronger the ability to suppress lithium dendrites and the better the electrochemical stability. Figure 6 It can be seen that the critical current density of Example 1 can reach 1.6 mA·cm −2 , and at the critical current density, the polarization voltage is lower than 1V, and the charge and discharge platform is also very stable, which shows that the modified solid electrolyte obtained in Example 1 has good lithium dendrite inhibition ability and excellent electrochemical stability. The difference between Comparative Example 1 and Example 1 is that MoS2 is not added in Comparative Example 1. Figure 6 It can be seen that the result leads to that in comparative example 1, the current density is 0.5 mA·cm −2 When the current density is 0.5 mA·cm −2 When the current is 1.2 mA·cm −2 The difference between Comparative Example 2 and Example 1 is that the modified layer is not applied in Comparative Example 2. Figure 6 As a result, when the current density rises to 0.4 mA cm −2 The voltage polarization of the symmetrical battery obtained in Comparative Example 2 is serious, indicating that lithium dendrites are formed and LATP is locally short-circuited. The difference between Comparative Example 5 and Example 1 is that MoS2 is replaced by Bi2S3, resulting in a critical current density of only 0.6 mA·cm −2 .
Claims
1. A modified solid electrolyte, characterized in that: The modified solid electrolyte comprises a solid electrolyte and a modified layer; Wherein, the modified layer includes polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the lithium bis(trifluoromethanesulfonylimide) is 1:(1-3.5); and the modified layer is coated on the surface of the solid electrolyte.
2. The modified solid electrolyte according to claim 1, characterized in that It meets one or more of the following conditions: (1) The solid electrolyte is a LATP solid electrolyte, wherein the LATP is Li 1+x Al x Ti 2-x (PO4)3, wherein x satisfies 0≤x≤0.5, for example, x is 0.3; (2) The thickness of the solid electrolyte is 0.5-2 mm, for example, 1.1 mm; (3) The mass ratio of the solid electrolyte to the polyvinylidene fluoride-hexafluoropropylene is (0.2-2):1, for example, 0.75:1; (4) The thickness of the modified layer is 10-30 μm, more preferably 20-30 μm, for example, 26.4 μm, 26.7 μm, 27.3 μm, 27.4 μm, 28.8 μm, 29.6 μm or 30.0 μm; (5) In the modified layer, the polyvinylidene fluoride-hexafluoropropylene is in a spherical connected structure, and the lithium bis(trifluoromethanesulfonyl)imide and the molybdenum disulfide are dispersed on the surface of the polyvinylidene fluoride-hexafluoropropylene; (6) The mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the lithium bis(trifluoromethanesulfonyl)imide is 1:(2-3), for example, 1:2, 1:2.5 or 1:3; (7) The mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the molybdenum disulfide is 1:(0.02-0.2), preferably 1:(0.05-0.15), for example 1:0.02, 1:0.05, 1:0.1, 1:0.15 or 1:0.
2.
3. The modified solid electrolyte according to claim 1, characterized in that The solid electrolyte is a LATP solid electrolyte, which has a mass of 0.24 g, a diameter of 10 mm, and a thickness of 1.1 mm.
4. The modified solid electrolyte according to claim 1, characterized in that The modified solid electrolyte is a modified solid electrolyte of any of the following schemes: Scheme 1: The modified solid electrolyte comprises a LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.8:0.032; Scheme 2: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.8:0.016; Scheme 3: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.8:0.048; Scheme 4: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bistrifluoromethanesulfonyl imide and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bistrifluoromethanesulfonyl imide and the molybdenum disulfide is 0.24:0.32:0.64:0.032; Scheme 5: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bistrifluoromethanesulfonyl imide and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bistrifluoromethanesulfonyl imide and the molybdenum disulfide is 0.24:0.32:0.96:0.032; Scheme 6: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.96:0.0064; Scheme 7: The modified solid electrolyte includes LATP solid electrolyte and a modified layer; the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer is composed of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide) and molybdenum disulfide; the modified layer is coated on the surface of the solid electrolyte; the mass ratio of the LATP solid electrolyte, the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide) and the molybdenum disulfide is 0.24:0.32:0.96:0.
064.
5. A method for preparing a modified solid electrolyte, characterized in that: It includes the following steps: The modified layer solution is coated on the solid electrolyte and the solvent is removed; Wherein, the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonyl)imide, molybdenum disulfide and solvent; The mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the lithium bis(trifluoromethanesulfonyl)imide is 1:(1-3.5).
6. The method for preparing the modified solid electrolyte according to claim 5, characterized in that: It meets one or more of the following conditions: (1) The preparation process of the modified solid electrolyte is carried out in a glove box; Preferably, in the glove box, H2O<0.1ppm, O2<0.1ppm; (2) The coating amount of the modified layer liquid per unit area on the solid electrolyte is 0.25-0.64 μL / mm 2 , for example 0.38 μL / mm 2 ; (3) The mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the lithium bis(trifluoromethanesulfonyl)imide is 1:(2-3), for example, 1:2, 1:2.5 or 1:3; (4) The mass ratio of the polyvinylidene fluoride-hexafluoropropylene to the molybdenum disulfide is 1:(0.02-0.2), preferably 1:(0.05-0.15), for example 1:0.02, 1:0.05, 1:0.1, 1:0.15 or 1:0.2; (5) The solvent is selected from N,N-dimethylformamide (DMF) and / or N-methylpyrrolidone (NMP); (6) The usage ratio of the polyvinylidene fluoride-hexafluoropropylene and the solvent is (0.16-0.48) g: (2-5) mL, for example, 0.32 g: 3 mL; (7) The modified layer liquid is prepared by the following method, which specifically comprises the following steps: S1, dissolving the polyvinylidene fluoride-hexafluoropropylene and the lithium bis(trifluoromethanesulfonyl)imide in the solvent, stirring to obtain a viscous solution; S2, adding the molybdenum disulfide to the viscous solution obtained in step S1, and stirring; Preferably, in step S1, the stirring temperature is 25-70°C, for example, 60°C; Preferably, in step S1, the stirring time is 10-20 hours, for example, 12 hours; Preferably, in step S2, the stirring temperature is 25-70°C, for example, 60°C; Preferably, in step S2, the stirring time is 2-8 hours, for example, 3 hours or 4 hours; (8) The solvent is removed by heating, and the heating temperature is 60-120°C, for example, 100°C; (9) The thickness of the solid electrolyte is 0.5-2 mm, for example, 1.1 mm; (10) The solid electrolyte is a LATP solid electrolyte, wherein the LATP is Li 1+x Al x Ti 2-x (PO4)3, wherein x satisfies 0≤x≤0.5, for example, x is 0.
3.
7. The method for preparing the modified solid electrolyte according to claim 5, characterized in that: The solid electrolyte is a LATP solid electrolyte, and the mass of the LATP solid electrolyte is 0.24 g, the diameter is 10 mm, and the thickness is 1.1 mm; the coating volume of the modified layer solution is 20-50 μL, for example, 30 μL.
8. The method for preparing the modified solid electrolyte according to claim 5, characterized in that: The preparation method of the modified solid electrolyte is any of the following schemes: Scheme 1: coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.8 g: 3 mL: 0.032 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ; Scheme 2: Coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.8 g: 3 mL: 0.016 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ; Scheme 3: Apply the modified layer solution on the LATP solid electrolyte and remove the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer solution includes polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.8 g: 3 mL: 0.048 g; the coating amount of the modified layer solution per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ; Scheme 4: coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.64 g: 3 mL: 0.032 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ; Scheme 5: Coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.96 g: 3 mL: 0.032 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ; Scheme 6: Apply the modified layer solution on the LATP solid electrolyte and remove the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer solution includes polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.96 g: 3 mL: 0.0064 g; the coating amount of the modified layer solution per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 ; Scheme 7: Coating the modified layer liquid on the LATP solid electrolyte and removing the solvent; wherein the thickness of the LATP solid electrolyte is 1.1 mm; the modified layer liquid comprises polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonylimide), molybdenum disulfide and DMF; the amount ratio of the polyvinylidene fluoride-hexafluoropropylene, the lithium bis(trifluoromethanesulfonylimide), the solvent and the molybdenum disulfide is 0.32 g: 0.96 g: 3 mL: 0.064 g; the coating amount of the modified layer liquid per unit area on the LATP solid electrolyte is 0.38 μL / mm 2 .
9. A modified solid electrolyte prepared by the method for preparing a modified solid electrolyte according to any one of claims 5 to 8.
10. Use of the modified solid electrolyte according to any one of claims 1 to 4 or the modified solid electrolyte according to claim 9 in preparing a lithium ion battery.