A method for preparing low-temperature electrolyte for lithium iron phosphate power battery

By using a low-temperature electrolyte preparation method with additives with quaternary ammonium salt, imidazole and crown ether groups in lithium iron phosphate batteries, the problems of increasing viscosity and reducing ion mobility in low-temperature environments are solved, and the battery is improved Low temperature cycle performance and conductivity.

CN118448724BActive Publication Date: 2024-11-29JIANGSU FENGSHAN QUANNUO NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410517882.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-29
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

The electrolyte viscosity of lithium iron phosphate batteries increases in low temperature environments and reduces the ion mobility, resulting in a decrease in the electrochemical reaction rate, affecting the discharge capacity and rate performance.

Method used

Using a low-temperature electrolyte preparation method, by controlling the temperature in an inert atmosphere, dispersing the lithium salt and the organic solvent evenly, adding specific additives, an additive with a quaternary ammonium salt group, an imidazole group and a crown ether group is prepared. Reduce the freezing point of the electrolyte and improve the conductivity, improve the stability and interface wetting of the SEI film.

Benefits of technology

It significantly improves the low-temperature cycling performance of lithium-ion batteries, reduces polarization and SEI film impedance, and enhances the low-temperature conductivity of the electrolyte and the capacity retention rate of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery, and relates to the technical field of lithium ion batteries. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery of the present invention comprises the following steps: in an inert atmosphere, lithium salts, organic solvents, and additives are uniformly dispersed to obtain a low-temperature electrolyte for a lithium iron phosphate power battery. The preparation method of the additive comprises the following steps: synthesizing component one using 3-aminophenylacetylene and dichlorosilane; preparing component two using component one and 1-(4-bromophenyl)imidazole as raw materials; and reacting component two with a brominated crown ether to obtain component three; finally, ion exchange is performed on component three and lithium bistrifluoromethanesulfonyl imide to obtain an additive. The additive prepared in the present application is added to the electrolyte to give the electrolyte excellent low-temperature performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery. Background Art

[0002] Lithium iron phosphate battery is an important lithium-ion battery with the characteristics of high energy density, long cycle life, safety and stability. With these advantages, lithium iron phosphate battery is widely used in electronic equipment and new energy vehicles. However, the poor low-temperature performance of lithium iron phosphate battery hinders its application in special military and civilian sites such as high-cold and high-altitude areas. The charge and discharge capacity of commercial lithium iron phosphate battery at -20℃ is only about 12% of that at room temperature. At low temperatures, the viscosity of the electrolyte increases and the ion mobility of the electrolyte decreases. When the battery is discharged at low temperatures, there is no time to replenish Li from the electrolyte. + , voltage drop occurs, the internal resistance of the battery increases, the electrochemical polarization increases, the electrochemical reaction rate decreases, and the discharge capacity and rate performance of the battery are greatly affected. In addition, the internal resistance of the lithium iron phosphate battery increases at low temperatures, further reducing the performance of the battery. When the working temperature is stable below -20°C, the electrochemical performance of the battery is significantly reduced. The electrochemical impedance spectroscopy (EIS) test shows that the main factors for the reduction in battery performance are the increase in charge transfer resistance and the decrease in lithium ion diffusion capacity. Therefore, the low-temperature performance of lithium iron phosphate batteries can be effectively improved by increasing the reaction activity of the electrolyte-electrode interface.

[0003] As an important component of lithium-ion batteries, electrolyte not only determines the + The migration rate in the liquid phase also participates in the formation of the SEI film, which plays a key role in the performance of the SEI film. Because the composition of the electrolyte is easier to operate and modify in practical applications, research in this area is a breakthrough in improving the low-temperature performance of lithium-ion batteries. At present, there are several ways to improve the low-temperature performance of electrolytes: (1) optimizing the solvent composition; (2) new electrolyte salts; (3) additives. Among them, the SEI film has an important influence on the low-temperature performance of the battery. It is an ion conductor and an electronic insulator. It is Li + The channel from the liquid phase to the electrode surface. At low temperatures, the SEI film impedance becomes larger, and Li + The diffusion rate in the SEI film decreases sharply, which makes the charge accumulation on the electrode surface deepen, resulting in a decrease in the lithium insertion ability of graphite and enhanced polarization. Optimizing the composition and film-forming conditions of the SEI film with the same specifications and improving the ionic conductivity of the SEI film at low temperatures are beneficial to improving the low-temperature performance of the battery. Therefore, the development of film-forming additives with excellent low-temperature performance is the current research focus. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery, and to solve the following technical problems:

[0005] When existing electrolytes are used in low-temperature environments, the viscosity of the electrolyte increases, the ion mobility in the electrolyte decreases, the electrochemical reaction rate decreases, and the discharge capacity and rate performance of the battery are adversely affected.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery comprises the following steps: in an inert atmosphere, controlling the temperature, evenly dispersing a lithium salt and an organic solvent, adding an additive, and evenly dispersing the additive to obtain a low-temperature electrolyte for a lithium iron phosphate power battery;

[0008] The preparation method of the additive comprises the following steps:

[0009] S1: In a nitrogen atmosphere, 3-aminophenylacetylene and toluene were added to a reaction bottle, the temperature was controlled at 200-220°C, dichlorosilane was added, the temperature was kept for 3-6 hours, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1;

[0010] S2: Add component 1, 1-(4-bromophenyl)imidazole, bis(triphenylphosphine)palladium dichloride, cuprous iodide, tetrahydrofuran and triethylamine into a reaction tube, seal the tube tightly after nitrogen protection, control the temperature at 60-80°C, react for 18-24h, rotary evaporate, purify, concentrate and dry to obtain component 2;

[0011] S3: Add crown ether bromide and acetone to a reaction bottle, control the temperature at 40-50°C, add component 2, keep warm for 36-48 hours under stirring, and purify to obtain component 3;

[0012] S4: Add component three, lithium bis(trifluoromethanesulfonyl imide) and ultrapure water into a reaction kettle, control the temperature to 70-80°C, keep the temperature under stirring for 9-12 hours, extract with dichloromethane, and remove dichloromethane by rotary evaporation to obtain an additive.

[0013] As a further embodiment of the present invention: the mass ratio of 3-aminophenylacetylene, toluene and dichlorosilane in S1 is 2.3-2.5:30-300:1.

[0014] As a further embodiment of the present invention, the addition ratio of component 1, 1-(4-bromophenyl)imidazole, bis(triphenylphosphine)palladium dichloride, cuprous iodide, tetrahydrofuran and triethylamine in S2 is 50 g: 45-50 g: 2.5-3.2 mg: 1.8-2.1 mg: 1.5-1.8 mL: 0.4-0.5 mL.

[0015] As a further solution of the present invention: the addition ratio of the brominated crown ether, acetone and component 2 in S3 is 0.9-1.5 g: 10-50 mL: 1 g.

[0016] As a further solution of the present invention: The specific steps of purification in S3 are: adding dichloromethane to dissolve, adding activated carbon to adsorb impurities, and then adding acetone to wash to obtain component three.

[0017] As a further solution of the present invention: the addition ratio of component three, lithium bis(trifluoromethanesulfonyl imide) and ultrapure water in S4 is 1 g: 0.4-0.6 g: 50-100 mL.

[0018] As a further solution of the present invention: the additive accounts for 1-10% of the total mass of the electrolyte.

[0019] As a further solution of the present invention: the inert atmosphere is an argon atmosphere, wherein the water content in the argon atmosphere is less than 1 ppm and the oxygen content in the argon atmosphere is less than 1 ppm.

[0020] As a further scheme of the present invention: the preparation method of brominated crown ether comprises the following steps: adding 165g of polyphosphoric acid (PPA) into a reaction bottle, controlling the temperature at 60-65°C, adding 5.3g of benzo-15-crown-5 ether and 3.9g of 6-bromohexanoic acid, controlling the temperature at 70-80°C, keeping warm for 6-9h under stirring conditions, adding water to stop the reaction, stirring evenly, adding chloroform to extract, collecting the extract, and rotary evaporating to obtain brominated crown ether.

[0021] As a further embodiment of the present invention: the organic solvent is obtained by mixing fluoroethylene carbonate (FEC), cyclic carbonate and linear carbonate in a volume ratio of 1:1:1-2; the cyclic carbonate is obtained by mixing one or more of ethylene carbonate (EC) and propylene carbonate (PC) in any ratio; the linear carbonate is obtained by mixing one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) in any ratio.

[0022] As a further embodiment of the present invention: the lithium salt is lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium hexafluorophosphate (LiPF 6 ), lithium trifluoromethanesulfonate (CF 3 SO 3 Any one or more of the above-mentioned electrolytes are mixed in any ratio; the concentration of the lithium salt in the electrolyte is 0.5-2 mol / L.

[0023] Beneficial effects of the present invention:

[0024] The present application first uses 3-aminophenylacetylene and dichlorosilane as raw materials to carry out aminolysis reaction in toluene solution to obtain component one; and uses component one and 1-(4-bromophenyl)imidazole as raw materials, bis(triphenylphosphine)palladium dichloride as a catalyst, and cuprous iodide as a co-catalyst, and uses the terminal alkyne group of component one and the bromide group of 1-(4-bromophenyl)imidazole to undergo a cross-coupling reaction to prepare component two; the present application uses the imidazole group of component two to react with the brominated crown ether to obtain component three having a crown ether group; finally, the present application uses component three to carry out ion exchange with lithium bistrifluoromethanesulfonyl imide to obtain an additive; wherein the brominated crown ether is prepared by Friedel-Crafts acylation reaction of benzo-15-crown-5 ether and 6-bromohexanoic acid as raw materials. The present application obtains an electrolyte with a low freezing point and high ionic conductivity by adding the additive prepared in the present application to the electrolyte, thereby improving the low temperature performance of the battery.

[0025] The additive structure prepared in the present application contains quaternary ammonium salt groups, imidazole groups, crown ether groups and silicon-nitrogen bonds, wherein the unprotonated N in the imidazole can serve as a proton donor and acceptor, and the protons move directionally on the imidazole groups along the hydrogen bond chain, which can reduce the transmission resistance of the protons, reduce the activation energy of ion transport, promote the migration of lithium ions, form micro-regions with lower freezing points inside the electrolyte, and Li+ has better mobility. The overall conductivity of the electrolyte is improved, which is beneficial to the battery capacity at low temperatures; the quaternary ammonium salt group can modify the cations and improve the redox stability of the ionic liquid; the crown ether group contained in the additive of the present application can not only + Coordination promotes ionization, is conducive to the formation of a smooth and dense solid electrolyte phase interface film, can effectively improve the solubility and ionization of lithium salts at low temperatures; reduce the solidification temperature of the electrolyte; thereby reducing the viscosity of the electrolyte and improving the conductivity; and giving the additive water-oil amphiphilic properties, showing a certain surface activity, with a fuzzy phase interface, can solve the interface wettability between the electrode material and the electrolyte, and reduce the interface contact resistance; it can also improve compatibility, improve the solubility effect, make the electrolyte show a certain coordination inclusion ability, generate a stable complex, and have a good effect of inhibiting lithium dendrites. The additive prepared in this application increases the charge transfer rate of lithium-ion batteries, greatly reduces polarization at low temperatures, reduces the SEI membrane impedance, and improves the stability of the SEI membrane; it is conducive to the formation of an SEI membrane with lower interface impedance, promotes the diffusion of ions and the movement of charges, thereby improving the low-temperature cycle performance of lithium iron phosphate batteries. The formed SEI membrane has a lower low-temperature impedance characteristic.

[0026] (2) The present application uses a blend of fluoroethylene carbonate, cyclic carbonate and linear carbonate as the organic solvent of the electrolyte; among them, fluoroethylene carbonate can not only reduce the viscosity of the electrolyte and improve the low-temperature conductivity of the electrolyte; but also, due to the presence of hydrogen bonds in the fluoroethylene carbonate molecule, it can reduce the melting point of the compound, and it can be reduced at a potential higher than that of the cyclic carbonate, introduce CF groups, reduce the activation energy of the membrane, and is beneficial to Li + Diffusion in the membrane. The present application simultaneously adds cyclic carbonate and linear carbonate as organic solvent components, and the use of carbonate organic solvents has good electrochemical stability and a wider electrochemical window, effectively widening the liquid phase temperature range of the electrolyte. DETAILED DESCRIPTION

[0027] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1 The preparation method of the additive comprises the following steps:

[0029] S1: In a nitrogen atmosphere, 2.3 g of 3-aminophenylacetylene and 30 g of toluene were added to a reaction bottle, the temperature was controlled at 200°C, 1 g of dichlorosilane was added, the temperature was kept for 3 h, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1;

[0030] S2: Add 50g of component 1, 45g of 1-(4-bromophenyl)imidazole, 2.5mg of bis(triphenylphosphine)palladium dichloride, 1.8mg of cuprous iodide, 1.5mL of tetrahydrofuran, and 0.4mL of triethylamine into a reaction tube, seal the tube tightly with nitrogen protection, control the temperature at 60°C, react for 18h, rotary evaporate, purify, concentrate, and dry to obtain component 2;

[0031] S3: The preparation method of brominated crown ether comprises the following steps: adding 165 g of polyphosphoric acid (PPA) into a reaction bottle, controlling the temperature at 60° C., adding 5.3 g of benzo-15-crown-5 ether and 3.9 g of 6-bromohexanoic acid, controlling the temperature at 70° C., keeping the temperature under stirring for 6 hours, adding water to stop the reaction, stirring evenly, adding chloroform to extract, collecting the extract, and rotary evaporating to obtain brominated crown ether;

[0032] S4: Add 0.9 g of brominated crown ether and 10 mL of acetone to a reaction bottle, control the temperature at 40°C, add 1 g of component 2, keep the temperature under stirring for 36 hours, add dichloromethane to dissolve, add activated carbon to adsorb impurities, and then add acetone to wash to obtain component 3;

[0033] S5: Add 1 g of component three, 0.5 g of lithium bis(trifluoromethanesulfonyl)imide and 50 mL of ultrapure water into a reaction kettle, control the temperature to 75°C, keep the temperature under stirring for 9 hours, extract with dichloromethane, and remove dichloromethane by rotary evaporation to obtain an additive.

[0034] Example 2 The preparation method of the additive comprises the following steps:

[0035] S1: In a nitrogen atmosphere, 2.4 g of 3-aminophenylacetylene and 100 g of toluene were added to a reaction bottle, the temperature was controlled at 210°C, 1 g of dichlorosilane was added, the temperature was kept for 4 h, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1;

[0036] S2: Add 50g of component 1, 47g of 1-(4-bromophenyl)imidazole, 2.5mg of bis(triphenylphosphine)palladium dichloride, 1.8mg of cuprous iodide, 1.5mL of tetrahydrofuran, and 0.4mL of triethylamine into a reaction tube, seal the tube tightly with nitrogen protection, control the temperature at 60°C, react for 24h, rotary evaporate, purify, concentrate, and dry to obtain component 2;

[0037] S3: The preparation method of brominated crown ether comprises the following steps: adding 165 g of polyphosphoric acid (PPA) into a reaction bottle, controlling the temperature at 60° C., adding 5.3 g of benzo-15-crown-5 ether and 3.9 g of 6-bromohexanoic acid, controlling the temperature at 70° C., keeping the temperature under stirring for 6 hours, adding water to stop the reaction, stirring evenly, adding chloroform to extract, collecting the extract, and rotary evaporating to obtain brominated crown ether;

[0038] S4: Add 1.2 g of brominated crown ether and 30 mL of acetone to a reaction bottle, control the temperature at 45°C, add 1 g of component 2, keep warm for 36 h under stirring, add dichloromethane to dissolve, add activated carbon to adsorb impurities, and then add acetone to wash to obtain component 3;

[0039] S5: Add 1 g of component three, 0.5 g of lithium bis(trifluoromethanesulfonyl)imide and 50 mL of ultrapure water into a reaction kettle, control the temperature to 75°C, keep the temperature under stirring for 9 hours, extract with dichloromethane, and remove dichloromethane by rotary evaporation to obtain an additive.

[0040] Example 3 The preparation method of the additive comprises the following steps:

[0041] S1: In a nitrogen atmosphere, 2.5 g of 3-aminophenylacetylene and 300 g of toluene were added to a reaction bottle, the temperature was controlled at 220°C, 1 g of dichlorosilane was added, the temperature was kept for 6 h, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1;

[0042] S2: Add 50g of component 1, 50g of 1-(4-bromophenyl)imidazole, 2.5mg of bis(triphenylphosphine)palladium dichloride, 1.8mg of cuprous iodide, 1.5mL of tetrahydrofuran, and 0.4mL of triethylamine into a reaction tube, seal the tube tightly with nitrogen protection, control the temperature at 80°C, react for 24h, rotary evaporate, purify, concentrate, and dry to obtain component 2;

[0043] S3: The preparation method of brominated crown ether comprises the following steps: adding 165 g of polyphosphoric acid (PPA) into a reaction bottle, controlling the temperature at 60° C., adding 5.3 g of benzo-15-crown-5 ether and 3.9 g of 6-bromohexanoic acid, controlling the temperature at 70° C., keeping the temperature under stirring for 6 hours, adding water to stop the reaction, stirring evenly, adding chloroform to extract, collecting the extract, and rotary evaporating to obtain brominated crown ether;

[0044] S4: Add 1.5 g of brominated crown ether and 50 mL of acetone to a reaction bottle, control the temperature to 50°C, add 1 g of component 2, keep the temperature under stirring for 48 h, add dichloromethane to dissolve, add activated carbon to adsorb impurities, and then add acetone to wash to obtain component 3;

[0045] S5: Add 1 g of component three, 0.5 g of lithium bis(trifluoromethanesulfonyl)imide and 50 mL of ultrapure water into a reaction kettle, control the temperature to 75°C, keep the temperature under stirring for 9 hours, extract with dichloromethane, and remove dichloromethane by rotary evaporation to obtain an additive.

[0046] Example 4 A method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery comprises the following steps:

[0047] A1: mixing fluoroethylene carbonate (FEC), ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1 to obtain an organic solvent;

[0048] A2: In an argon atmosphere (water content 0.4ppm, oxygen content less than 0.7ppm), control the temperature and mix lithium hexafluorophosphate (LiPF 6 ), after the organic solvent prepared in A1 is evenly dispersed, the additive prepared in Example 1 is added and evenly dispersed to obtain a low-temperature electrolyte for lithium iron phosphate power batteries; wherein the additive accounts for 1% of the total mass of the electrolyte; LiPF 6 The concentration in the electrolyte is 1 mol / L.

[0049] Example 5 A method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery comprises the following steps:

[0050] A1: mixing fluoroethylene carbonate (FEC), ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1 to obtain an organic solvent;

[0051] A2: In an argon atmosphere (water content 0.4ppm, oxygen content less than 0.7ppm), control the temperature and mix lithium hexafluorophosphate (LiPF 6 ), after the organic solvent prepared in A1 is evenly dispersed, the additive prepared in Example 2 is added and evenly dispersed to obtain a low-temperature electrolyte for lithium iron phosphate power batteries; wherein the additive accounts for 1% of the total mass of the electrolyte; LiPF 6 The concentration in the electrolyte is 1 mol / L.

[0052] Example 6 A method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery comprises the following steps:

[0053] A1: mixing fluoroethylene carbonate (FEC), ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1 to obtain an organic solvent;

[0054] A2: In an argon atmosphere (water content 0.4ppm, oxygen content less than 0.7ppm), control the temperature and mix lithium hexafluorophosphate (LiPF 6 ), after the organic solvent prepared in A1 is evenly dispersed, the additive prepared in Example 3 is added and evenly dispersed to obtain a low-temperature electrolyte for lithium iron phosphate power batteries; wherein the additive accounts for 1% of the total mass of the electrolyte; LiPF 6 The concentration in the electrolyte is 1 mol / L.

[0055] Comparative Example 1 The preparation method of the additive comprises the following steps:

[0056] S1: In a nitrogen atmosphere, 2.3 g of 3-aminophenylacetylene and 30 g of toluene were added to a reaction bottle, the temperature was controlled at 200°C, 1 g of dichlorosilane was added, the temperature was kept for 3 h, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1;

[0057] S2: Add 50g of component 1, 45g of 1-(4-bromophenyl)imidazole, 2.5mg of bis(triphenylphosphine)palladium dichloride, 1.8mg of cuprous iodide, 1.5mL of tetrahydrofuran, and 0.4mL of triethylamine into a reaction tube, seal the tube tightly with nitrogen protection, control the temperature at 60°C, react for 18h, rotary evaporate, purify, concentrate, and dry to obtain component 2;

[0058] S3: The preparation method of brominated crown ether comprises the following steps: adding 165 g of polyphosphoric acid (PPA) into a reaction bottle, controlling the temperature at 60° C., adding 5.3 g of benzo-15-crown-5 ether and 3.9 g of 6-bromohexanoic acid, controlling the temperature at 70° C., keeping the temperature under stirring for 6 hours, adding water to stop the reaction, stirring evenly, adding chloroform to extract, collecting the extract, and rotary evaporating to obtain brominated crown ether;

[0059] S4: Add 0.9 g of brominated crown ether and 10 mL of acetone into a reaction bottle, control the temperature at 40°C, add 1 g of component 2, keep warm for 36 h under stirring, add dichloromethane to dissolve, add activated carbon to adsorb impurities, and then add acetone to wash to obtain the additive.

[0060] Comparative Example 2 The preparation method of the additive comprises the following steps:

[0061] S1: Add 50 g of 3-aminophenylacetylene, 45 g of 1-(4-bromophenyl)imidazole, 2.5 mg of bis(triphenylphosphine)palladium dichloride, 1.8 mg of cuprous iodide, 1.5 mL of tetrahydrofuran, and 0.4 mL of triethylamine into a reaction tube, seal the tube under nitrogen protection, control the temperature at 60°C, react for 18 h, rotary evaporate, purify, concentrate, and dry to obtain component 2;

[0062] S2: The preparation method of brominated crown ether comprises the following steps: adding 165 g of polyphosphoric acid (PPA) into a reaction bottle, controlling the temperature at 60° C., adding 5.3 g of benzo-15-crown-5 ether and 3.9 g of 6-bromohexanoic acid, controlling the temperature at 70° C., keeping the temperature under stirring for 6 hours, adding water to stop the reaction, stirring evenly, adding chloroform to extract, collecting the extract, and rotary evaporating to obtain brominated crown ether;

[0063] S3: Add 0.9 g of brominated crown ether and 10 mL of acetone to a reaction bottle, control the temperature at 40°C, add 1 g of component 2, keep the temperature under stirring for 36 hours, add dichloromethane to dissolve, add activated carbon to adsorb impurities, and then add acetone to wash to obtain component 3;

[0064] S4: Add 1 g of component three, 0.5 g of lithium bis(trifluoromethanesulfonyl)imide and 50 mL of ultrapure water into a reaction kettle, control the temperature to 75°C, keep the temperature under stirring for 9 hours, extract with dichloromethane, and remove dichloromethane by rotary evaporation to obtain an additive.

[0065] Comparative Example 3 The preparation method of the additive comprises the following steps:

[0066] S1: In a nitrogen atmosphere, 2.3 g of 3-aminophenylacetylene and 30 g of toluene were added to a reaction bottle, the temperature was controlled at 200°C, 1 g of dichlorosilane was added, the temperature was kept for 3 h, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1;

[0067] S2: Add 50 g of component 1, 45 g of 1-(4-bromophenyl)imidazole, 2.5 mg of bis(triphenylphosphine)palladium dichloride, 1.8 mg of cuprous iodide, 1.5 mL of tetrahydrofuran, and 0.4 mL of triethylamine into a reaction tube, seal the tube under nitrogen protection, control the temperature at 60°C, react for 18 h, and rotary evaporate, purify, concentrate, and dry to obtain the additive.

[0068] Comparative Example 4 The preparation method of the additive comprises the following steps:

[0069] S1: In a nitrogen atmosphere, 2.3 g of 3-aminophenylacetylene and 30 g of toluene were added to a reaction bottle, the temperature was controlled at 200°C, 1 g of dichlorosilane was added, the temperature was kept for 3 h, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1;

[0070] S2: Add 50g of component 1, 45g of 1-(4-bromophenyl)imidazole, 2.5mg of bis(triphenylphosphine)palladium dichloride, 1.8mg of cuprous iodide, 1.5mL of tetrahydrofuran, and 0.4mL of triethylamine into a reaction tube, seal the tube tightly with nitrogen protection, control the temperature at 60°C, react for 18h, rotary evaporate, purify, concentrate, and dry to obtain component 2;

[0071] S5: Add 1 g of component 2, 0.5 g of lithium bis(trifluoromethanesulfonyl)imide and 50 mL of ultrapure water into a reaction kettle, control the temperature to 75°C, keep the temperature under stirring for 9 hours, extract with dichloromethane, and remove dichloromethane by rotary evaporation to obtain an additive.

[0072] Comparative Example 5 Compared with Example 4, in Comparative Example 5, only the additive prepared in Example 1 added in Example 4 is replaced by the additive prepared in Comparative Example 1 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0073] Comparative Example 6 Compared with Example 4, in Comparative Example 6, only the additive prepared in Example 1 added in Example 4 is replaced by the additive prepared in Comparative Example 2 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0074] Comparative Example 7 Compared with Example 4, in Comparative Example 7, only the additive prepared in Example 1 added in Example 4 is replaced by the additive prepared in Comparative Example 3 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0075] Comparative Example 8 Compared with Example 4, in Comparative Example 8, only the additive prepared in Example 1 added in Example 4 is replaced by the additive prepared in Comparative Example 4 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0076] Performance Testing

[0077] Prepare the battery:

[0078] ①Pole sheet preparation: The positive electrode active material is LiFePO 4, the conductive agent is acetylene black, and the binder is polytetrafluoroethylene (PTFE). The active material, acetylene black, and PTFE with a mass ratio of 75:20:5 are fully ground, mixed evenly, and anhydrous ethanol is added as a dispersant, pressed into a positive electrode sheet with a thickness of 100um, and then punched into a disc with a diameter of 8mm at 10MPa, and dried in a constant temperature drying oven at 100℃ for 24h, and an aluminum sheet is used as a positive electrode current collector to obtain a positive electrode sheet;

[0079] ② Preparation of electrolyte: electrolytes prepared in Examples 4-6 and Comparative Examples 5-8;

[0080] ③Battery assembly: It was carried out in a glove box filled with argon (moisture content <1ppm), with metal lithium sheets as auxiliary electrodes and reference electrodes (copper sheet current collector), Celgard2400 porous polypropylene diaphragm, and electrolytes of different components. After assembly in the mold, it was sealed and allowed to stand at room temperature for 10 hours to obtain a battery sample.

[0081] (1) Ionic conductivity: The conductivity was tested in a water bath using a digital conductivity meter model DDS-307A produced by Shanghai Leici Instrument Factory. The measurement stability range was -40-25°C. The test results are shown in Table 1.

[0082] Table 1: Statistical table of conductivity performance test data of Examples 4-6 and Comparative Examples 5-8

[0083]

[0084] As can be seen from Table 1, when the additives prepared in the present application are added to the electrolyte, it can be seen that the temperature dependence of the electrolytes prepared in Examples 4 to 6 of the present application is low, which gives the electrolytes excellent low-temperature resistance.

[0085] (2) Charge and discharge test: At room temperature, the battery was cycled using the LAND CT-2001A battery test system; low-temperature cycled at -40°C using the NEWARE CT-3008 battery test system; the charge and discharge voltage range was 3.0-5.1V, and the charge and discharge current density was 0.4mA / cm 2 ;

[0086] Cycle steps:

[0087] a: Pre-cycle step: first, constant current charge (CC) at a current density of 0.05C to 3.3V, then constant current charge to the cut-off voltage at 0.2C, constant voltage charge (CV) at the cut-off voltage until the current drops to 1 / 10 of the constant current charge current value, and then 0.2C constant current discharge (CC) to 3V;

[0088] b: The battery was pre-cycled for 1 cycle at room temperature. After the pre-cycle, it was cycled again at -40°C at a rate of 5.5C in the voltage range of 3-5.1V (CC / CV charge-CC discharge, the cut-off current of constant voltage charge is 1 / 10 of the constant current charge current value), and cycled for 300 cycles (1C=372mA˙g-1). The test results are shown in Table 2;

[0089] Table 2: Statistical table of conductivity performance test data of Examples 4-6 and Comparative Examples 5-8

[0090]

[0091] As can be seen from Table 2, the additives prepared in Examples 1-3 of the present application are added as components to the electrolyte. After 300 cycles, the lithium battery maintains an excellent capacity retention rate, so that the prepared lithium-ion battery still maintains low-temperature high cycle stability in a low-temperature environment.

[0092] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery, characterized in that: The method comprises the following steps: in an inert atmosphere, controlling the temperature, evenly dispersing the lithium salt and the organic solvent, adding an additive, and evenly dispersing the additive to obtain a low-temperature electrolyte for a lithium iron phosphate power battery; The preparation method of the additive comprises the following steps: S1: In a nitrogen atmosphere, 3-aminophenylacetylene and toluene were added to a reaction bottle, the temperature was controlled at 200-220°C, dichlorosilane was added, the temperature was kept for 3-6 hours, rotary evaporation was performed, filtration was performed, and the filtrate was distilled under reduced pressure to obtain component 1; S2: Add component 1, 1-(4-bromophenyl)imidazole, bis(triphenylphosphine)palladium dichloride, cuprous iodide, tetrahydrofuran and triethylamine into a reaction tube, seal the tube tightly after nitrogen protection, control the temperature at 60-80°C, react for 18-24h, rotary evaporate, purify, concentrate and dry to obtain component 2; S3: Add crown ether bromide and acetone to a reaction bottle, control the temperature at 40-50°C, add component 2, keep warm for 36-48 hours under stirring, and purify to obtain component 3; S4: Add component three, lithium bis(trifluoromethanesulfonyl)imide and ultrapure water into a reaction kettle, control the temperature to 70-80°C, keep the temperature for 9-12 hours under stirring, extract with dichloromethane, and remove dichloromethane by rotary evaporation to obtain an additive; The brominated crown ether is prepared by using benzo-15-crown-5 ether and 6-bromohexanoic acid as raw materials through a Friedel-Crafts acylation reaction.

2. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The mass ratio of 3-aminophenylacetylene, toluene and dichlorosilane in S1 is 2.3-2.5:30-300:

1.

3. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The addition ratio of component 1, 1-(4-bromophenyl)imidazole, bis(triphenylphosphine)palladium dichloride, cuprous iodide, tetrahydrofuran, and triethylamine in S2 is 50 g: 45-50 g: 2.5-3.2 mg: 1.8-2.1 mg: 1.5-1.8 mL: 0.4-0.5 mL.

4. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The addition ratio of brominated crown ether, acetone and component 2 in S3 is 0.9-1.5 g:10-50 mL:1 g.

5. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The addition ratio of component three, lithium bis(trifluoromethanesulfonyl imide) and ultrapure water in S4 is 1 g: 0.4-0.6 g: 50-100 mL.

6. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The lithium salt is any one of lithium perchlorate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium hexafluorophosphate, and lithium trifluoromethanesulfonate, or a mixture of any of the above. The concentration of the lithium salt in the electrolyte is 0.5-2 mol / L.

7. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The organic solvent is obtained by mixing fluoroethylene carbonate, cyclic carbonate and linear carbonate in a volume ratio of 1:1:1-2; the cyclic carbonate is obtained by mixing one or more of ethylene carbonate and propylene carbonate in any ratio; the linear carbonate is obtained by mixing one or more of dimethyl carbonate, diethyl carbonate and methyl ethyl carbonate in any ratio.

8. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The additive accounts for 1-10% of the total mass of the electrolyte.

9. The method for preparing a low-temperature electrolyte for a lithium iron phosphate power battery according to claim 1, characterized in that: The inert atmosphere is an argon atmosphere, in which the water content is less than 1 ppm and the oxygen content is less than 1 ppm.

Citation Information

Patent Citations

  • Low-temperature electrolyte for lithium iron phosphate battery

    CN106129472A

  • High-low-temperature electrolyte suitable for lithium iron phosphate power battery and preparation method for electrolyte

    CN107069087A