Electrode for lithium rechargeable battery and lithium rechargeable battery
By using a porous layer on the electrode of the lithium rechargeable battery, combined with the binder resin derived from urethane acrylate and inorganic fine particles, the problem of short circuit and insufficient interface bonding strength of lithium batteries at high temperatures is solved, and the problem of short circuit and insufficient interface bonding strength is achieved. Higher battery stability and capacity.
Patent Information
- Application Number
- CN202380033858.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-21
- Filing Date
- 2023-08-22
- Publication Date
- 2024-11-22
AI Technical Summary
The lithium rechargeable battery at high temperatures caused by the short circuit between the positive electrode and the negative electrode, which reduces the battery life and performance. The interface bonding strength of the existing polymer separators is insufficient, which affects the stability of the battery and capacity.
A porous layer consisting of a binder resin containing repeating units derived from urethane (meth)acrylate monomer or oligomer and inorganic fine particles is formed on the electrode substrate, providing high temperature stability and strong structure. Stability and crosslinked structures are formed by photopolymerization to improve interface bonding strength.
It improves the high temperature stability, structural stability and interface bonding strength of lithium rechargeable batteries, extends the battery life, improves charging and discharge capacity, and provides high bending resistance.
Smart Images

Figure CN119013798A_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0105065 filed in the Korean Intellectual Property Office on August 22, 2022, and Korean Patent Application No. 10-2023-0109223 filed in the Korean Intellectual Property Office on August 21, 2023, the disclosures of which are incorporated herein by reference in their entirety.
[0003] The present invention relates to an electrode for a lithium rechargeable battery and a lithium rechargeable battery including the same, wherein the electrode for a lithium rechargeable battery not only has high high temperature stability, strong structural stability and high interface bonding strength with a counter electrode, but also can improve the life characteristics, charging capacity and discharging capacity of the lithium rechargeable battery and has high bending resistance. Background Art
[0004] Recently, with the development of technology and the demand for mobile devices, the demand for rechargeable batteries as energy sources has increased rapidly, and therefore, a large number of studies have been conducted on rechargeable batteries that can meet various needs. In addition, rechargeable batteries have attracted considerable attention as power sources for electric vehicles (EV), hybrid electric vehicles (HEV), and plug-in hybrid electric vehicles (HEV), which are developed to solve problems such as air pollution caused by existing gasoline and diesel vehicles using fossil fuels.
[0005] When a short circuit occurs due to contact between the positive electrode and the negative electrode, the lithium rechargeable battery generates extreme heat and causes an explosion. Due to material properties and manufacturing process properties including stretching, the porous separator of the rechargeable battery exhibits extreme thermal shrinkage behavior at temperatures of about 100°C or higher, which causes a problem of causing a short circuit between the positive electrode and the negative electrode.
[0006] Therefore, various studies are being conducted on methods that can ensure shape stability and high-temperature stability of lithium rechargeable batteries. Summary of the invention
[0007] Technical issues
[0008] An object of the present invention is to provide an electrode for a lithium rechargeable battery, which not only has high high-temperature stability, strong structural stability, and high interfacial bonding strength with a counter electrode, but also can improve the life characteristics, charging capacity, and discharging capacity of the lithium rechargeable battery, and has high bending resistance.
[0009] Another object of the present invention is to provide a lithium rechargeable battery including the electrode for a lithium rechargeable battery.
[0010] Technical Solution
[0011] Provided herein is an electrode for a lithium rechargeable battery, comprising an electrode substrate and a porous layer formed on the electrode substrate, the porous layer comprising a binder resin and inorganic fine particles, the binder resin comprising a (co)polymer containing repeating units derived from a urethane (meth)acrylate-based monomer or oligomer.
[0012] Also provided herein is a lithium rechargeable battery including the electrode for a lithium rechargeable battery.
[0013] Now, a lithium rechargeable battery electrode, a lithium rechargeable battery, and the like according to an embodiment of the present invention will be described in more detail.
[0014] As used herein, photopolymerizable compounds generally refer to compounds that cause a polymerization reaction when irradiated with light, for example, when irradiated with visible light or ultraviolet light.
[0015] Furthermore, the (meth)acryloyl group is meant to include both an acryloyl group and a methacryloyl group.
[0016] Furthermore, a (co)polymer is meant to include both a copolymer and a homopolymer.
[0017] Furthermore, the electrode substrate means a current collector.
[0018] In addition, the electrode means an electrode layer coated on an electrode substrate, and the electrode layer coated on a single side or a double side is referred to as a single side electrode and a double side electrode, respectively.
[0019] According to one embodiment of the present invention, there is provided an electrode for a lithium rechargeable battery, comprising an electrode substrate and a porous layer formed on the electrode substrate, the porous layer comprising a binder resin and inorganic fine particles, the binder resin comprising a (co)polymer containing repeating units derived from a urethane (meth)acrylate-based monomer or oligomer.
[0020] The inventors have developed an electrode for a lithium rechargeable battery including a porous layer, and have determined through experiments that such an electrode for a lithium rechargeable battery not only has high high temperature stability, strong structural stability, and high interfacial bonding strength with a counter electrode, but can also improve the life characteristics, charging capacity, and discharging capacity of the lithium rechargeable battery, thereby completing the present invention.
[0021] In particular, in the porous layer, the inorganic fine particles can be connected, linked or fixed by the above-mentioned binder resin. Since the binder resin includes a (co)polymer containing a repeating unit derived from a monomer or oligomer based on urethane (meth) acrylate, it can have flexibility or bending resistance that is difficult to achieve in a rechargeable battery including a known electrode coating or a separator having a coating formed thereon.
[0022] Specifically, the porous layer or the electrode for a lithium rechargeable battery including the porous layer may have bending resistance that does not cause cracks when wound on a cylindrical mandrel having a diameter of 2 mm or more according to an ISO 1519:2011 standard method.
[0023] According to the ISO 1519:2011 standard method, the porous layer or the electrode for lithium rechargeable battery including the porous layer is subjected to a cylindrical mandrel test from large diameter to small diameter to determine the bending resistance. The measurement sample can be an electrode for lithium rechargeable battery including a porous layer, and the electrode can be a single-sided electrode or a double-sided electrode. In the case of a single-sided electrode, the porous layer is formed on the surface opposite to the current collector while in contact with the electrode layer, and in the case of a double-sided electrode, the porous layer is formed on the surface opposite to the current collector while in contact with only one side of the electrode layer.
[0024] In a state where the porous layer is formed on the electrode substrate, the above-mentioned bending resistance can be evaluated in a state where the porous layer is in close contact with the cylindrical mandrel so that it faces outward without contacting the cylindrical mandrel.
[0025] The bending resistance value can be determined by the diameter of the largest first mandrel at which cracks appear in the coating when the electrode coated with the porous layer is brought into close contact with the cylindrical mandrel, or the coating is separated from the electrode layer, or the coating and the electrode layer are separated from the current collector together. When such a method is applied, the porous layer or the lithium rechargeable battery electrode including the porous layer can have a bending resistance that does not cause cracks when wound on a cylindrical mandrel having a diameter of 2 mm or more, 3 mm or more, or 4 mm or more, 2 mm to 40 mm, 3 mm to 30 mm, or 4 mm to 20 mm according to the ISO 1519:2011 standard method.
[0026] Meanwhile, conventional lithium rechargeable batteries have problems such as weak interfacial bonding strength between a polymer separator disposed between a positive electrode and a negative electrode and a counter electrode, thereby reducing the efficiency of a battery assembly process, and interfacial peeling occurs due to insufficient bonding strength when the electrodes expand and contract, thereby reducing battery life characteristics. In particular, there is a problem that it exhibits a large thermal shrinkage behavior at a temperature of 100° C. or higher, which causes a short circuit between the positive electrode and the negative electrode.
[0027] On the contrary, the lithium rechargeable battery electrode of the above embodiment can have high interfacial bonding strength with the counter electrode and strong internal structure while the porous layer formed on the electrode substrate replaces the function of the existing polymer separator. Even at a temperature of 100° C. or higher, the electrode can prevent the degradation of structural stability and the degradation of battery performance.
[0028] More specifically, a binder resin comprising a (co)polymer containing repeating units derived from a monomer or oligomer based on urethane (meth)acrylate contains a flexible functional group inside that can absorb external impact, and it combines with adjacent binder resins through a photopolymerization reaction to form a cross-linked structure, thereby playing a role in fixing the position of aluminum oxide particles distributed between the binder resins.
[0029] The inorganic fine particles are a main component for forming the porous layer, and serve to form pores through empty spaces existing between the inorganic fine particles, and also serve as a spacer that can maintain the physical shape of the porous layer.
[0030] Furthermore, the cross-linked structure of the porous layer has higher thermal stability and higher dimensional stability than existing polyolefin separators, thereby making it possible to improve life characteristics, charge capacity, and discharge capacity of a lithium rechargeable battery.
[0031] The porous layer can form micro-unit pores by adjusting the size of inorganic fine particles, the content of inorganic fine particles and the content of binder resin, and the pore size and porosity can also be adjusted. For example, the porosity of the porous layer can be 40% to 80%, 45% to 75% or 50% to 70%.
[0032] The porosity of the porous layer can be achieved according to the composition of the porous layer. When the porous layer satisfies the above-mentioned contents of inorganic fine particles and binder resin, the porosity of the porous layer can be achieved. Since the porous layer has a porosity within the above-mentioned range, the technical effect of improving battery performance can be achieved due to electrochemical reasons that allow electrolyte lithium ions to move smoothly through the pores.
[0033] If the porosity of the porous layer is less than 40%, the movement of lithium ions is restricted and the resistance increases, which may cause a technical problem of deterioration of the charging and discharging characteristics of the battery. If the porosity of the porous layer is greater than 80%, the mechanical properties of the porous layer may be weakened, which may cause a technical problem of deterioration of the durability of the battery device.
[0034] The porosity may be calculated according to the following Mathematical Equation 1 by using the ratio of the density obtained by measuring the volume and mass of the porous layer of the sample coated with the above composition on a fixed area of the electrode substrate to the theoretical density of the solid content of the coating composition.
[0035] [Mathematical equation 1]
[0036] Porosity (%)={1-(actual density) / (theoretical density)}×100.
[0037] By adjusting the size of the inorganic fine particles, the content of the inorganic fine particles and the content of the binder resin, the size of the pores formed in the porous layer can be adjusted. Specifically, the porous layer can be formed with pores having a cross-sectional diameter of 20nm to 2000nm, 30nm to 1000nm, 100nm to 1000nm or 100nm to 500nm.
[0038] In particular, since the porous layer contains inorganic fine particles, pores having a cross-sectional diameter within the above range can be formed, whereby the electrode for the lithium rechargeable battery not only has high high temperature stability, strong structural stability and high interface adhesion strength with the counter electrode, but also can improve the life characteristics, charging capacity and discharging capacity of the lithium rechargeable battery.
[0039] Meanwhile, the porous layer may contain 1 to 50 parts by weight, or 3 to 45 parts by weight, or 5 to 40 parts by weight, or 20 to 38 parts by weight of a binder resin relative to 100 parts by weight of the inorganic fine particles. As described above, the porous layer may form micro-unit pores by adjusting the size of the inorganic fine particles, the content of the inorganic fine particles, and the content of the binder resin, and the pore size and porosity may also be adjusted.
[0040] That is, since the porous layer contains 1 to 50 parts by weight, or 3 to 45 parts by weight, or 5 to 40 parts by weight, or 20 to 38 parts by weight of a binder resin relative to 100 parts by weight of inorganic fine particles, the porosity of the porous layer can be 40% to 80%, 45% to 75% and 50% to 70%, and the porous layer can be formed with pores having a cross-sectional diameter of 20nm to 2000nm, 30nm to 1000nm or 30nm to 500nm.
[0041] In addition, since the porous layer contains 1 to 50 parts by weight, or 3 to 45 parts by weight, or 5 to 40 parts by weight, or 20 to 38 parts by weight of the binder resin relative to 100 parts by weight of the inorganic fine particles, the effect of maintaining stable adhesion between the porous layer and the electrode substrate can be achieved without hindering ionic conductivity.
[0042] When the porous layer contains an excessive or too small amount of binder resin relative to the inorganic fine particles, the pore size and porosity decrease due to the reduction of empty spaces formed between the inorganic fine particles, which leads to deterioration of the final battery performance, or the bonding strength between the inorganic fine particles weakens and the peeling resistance weakens, which leads to deterioration of the mechanical properties of the porous layer.
[0043] The diameter of each particle of the inorganic fine particles may be in nanometer units or micrometer units, and the inorganic fine particles may include, for example, inorganic fine particles in which the diameter of each particle is in the range of 1 nm to 500 μm. In addition, the inorganic fine particles may be formed into one particle (secondary particle) by agglomerating each particle (primary particle), and the formed secondary particle may behave like an independent particle.
[0044] More specifically, the inorganic fine particles may include boehmite including primary particles having average particle diameters of 10 nm to 500 nm, 20 nm to 400 nm, and 30 nm to 300 nm.
[0045] The average particle size can be measured using known methods and equipment. For example, a method can be used in which a scanning electron microscope (SEM) photograph is taken at 50,000x magnification using a Jeol JSM-7400F, and then the diameter is calculated using an image analysis program (Image Pro Plus ver 4.5).
[0046] Meanwhile, the inorganic fine particles may include secondary particles having D50 of 10 nm to 2000 nm, 20 nm to 1000 nm, and 50 nm to 800 nm.
[0047] In addition, the inorganic fine particles may include boehmite including primary particles having an average particle diameter of 10nm to 500nm, 20nm to 400nm, and 30nm to 300nm, wherein the boehmite may include secondary particles having a D50 of 10nm to 2000nm, 20nm to 1000nm, and 50nm to 800nm.
[0048] D 50It means the particle size of particles corresponding to 50% of the total number of particles when the measured particles are arranged in order from the smallest particle diameter to the largest particle diameter. D50 can be measured using known methods and equipment. For example, D50 can be measured using PSA (Particle size analyzer) or DLS (Dynamic light scattering). For example, for D50 measurement using PSA, the particle size distribution of a solution in which particles are dispersed can be measured using a Malvern Mastersizer 3000, and for D50 measurement using DLS, the particle size distribution of a solution in which particles are dispersed can be measured using an ELSZ-2000DLS (Otsuka Electronics).
[0049] If the diameter of the inorganic fine particles is too small, the dispersibility decreases, which makes it difficult to adjust the physical properties of the porous layer, and if the diameter of the inorganic fine particles is too large, the thickness of the porous layer may increase and the mechanical properties may deteriorate, and due to the excessively large pore size, the possibility of internal short circuits occurring when charging and discharging the battery becomes higher.
[0050] If the inorganic fine particles are electrically stable and chemically stable, they are not particularly limited. Specifically, if no oxidation or reduction reaction occurs within the operating voltage range of the applied battery, the inorganic fine particles are not particularly limited. In particular, in the case of using inorganic fine particles having ion transfer ability, performance can be enhanced by improving the ionic conductivity in lithium rechargeable batteries. In addition, in the case of using inorganic fine particles with a high dielectric constant, it helps to improve the dissociation of electrolyte salts such as lithium salts in liquid electrolytes, thereby improving the ionic conductivity of the electrolyte.
[0051] For example, the inorganic fine particles may include one or more types of inorganic fine particles selected from the following: alumina (Al2O3), boehmite (AlOOH), aluminum hydroxide (Al(OH)3), silicon dioxide (SiO2), titanium dioxide (TiO2) and magnesium hydroxide (Mg(OH)2).
[0052] The inorganic fine particles may not be substituted by a separate functional group or a separate compound on the surface, and the inorganic fine particles may include inorganic fine particles surface-modified by one or more compounds selected from (meth)acrylates, thiol groups, and organosilane compounds. The functional groups or compounds substituted on the inorganic particle surfaces may be selected in consideration of the physical properties, type, etc. of the binder resin of the porous layer.
[0053] Meanwhile, as described above, in one embodiment, the binder resin may play a role in connecting or binding or fixing the inorganic fine particles, and the binder resin may include a (co)polymer containing repeating units derived from a urethane (meth)acrylate-based monomer or oligomer.
[0054] Examples of the urethane (meth)acrylate-based monomer or oligomer include at least one selected from polyester (meth)urethane acrylate, polyester urethane di(meth)acrylate, polyether (meth)urethane acrylate, and polyether urethane di(meth)acrylate.
[0055] The specific molecular weight of the urethane (meth)acrylate-based oligomer is not limited, but for example, the weight average molecular weight thereof (weight average molecular weight measured by GPC method using polystyrene calibration) may be 50,000 g / mol or less, 40,000 g / mol or less, 30,000 g / mol or less, or 300 g / mol or more, 1,000 g / mol or more, 3,000 g / mol or more, and 300 g / mol to 50,000 g / mol, 1,000 g / mol to 50,000 g / mol, 3,000 g / mol to 50,000 g / mol, or 3,000 g / mol to 30,000 g / mol.
[0056] Meanwhile, the (co)polymer may contain a repeating unit derived from a multifunctional acrylate in addition to the repeating unit derived from the urethane (meth)acrylate-based monomer or oligomer.
[0057] The multifunctional acrylate may be a multifunctional (meth)acrylate monomer or oligomer, wherein the number of functional groups based on (meth)acrylate may be 2 to 10, preferably 2 to 8, and more preferably 2 to 7.
[0058] Examples of the multifunctional acrylate may be at least one selected from the following: pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol hepta(meth)acrylate, tripentaerythritol hepta(meth)acrylate, toluene diisocyanate, xylene diisocyanate, hexamethylene diisocyanate, trimethylolpropane tri(meth)acrylate and trimethylolpropane polyethoxy tri(meth)acrylate, and specific examples are not limited thereto.
[0059] The (co)polymer may contain a repeating unit derived from a urethane (meth)acrylate-based monomer or oligomer and a repeating unit derived from a multifunctional acrylate in appropriate amounts in consideration of specific physical properties of the porous layer and the like.
[0060] Meanwhile, the porous layer is formed by curing (thermal curing or photocuring) the binder resin and the inorganic particles together. The components contained in the binder resin and the inorganic particles form crosslinking bonds or covalent bonds, thereby improving the heat resistance, mechanical strength, etc. of the porous layer and the electrode for lithium rechargeable batteries.
[0061] The content of the repeating units derived from the urethane (meth)acrylate-based monomer or oligomer in the (co)polymer is not particularly limited, for example, the (co)polymer may contain 1 wt % to 99 wt % or 10 wt % to 90 wt % of the repeating units derived from the urethane (meth)acrylate-based monomer or oligomer.
[0062] Meanwhile, in one embodiment, the thickness of the porous layer is not particularly limited, and may be adjusted to, for example, 0.01 μm to 100 μm in consideration of battery performance.
[0063] For example, the thickness of the porous layer may be 0.1 μm or more and 30 μm or less.
[0064] More specifically, the thickness of the porous layer may be 0.1 μm or more, 1 μm or more, 5 μm or more, 10 μm or more, or 30 μm or less, or it may be 0.1 μm or more and 30 μm or less, 1 μm or more and 30 μm or less, 5 μm or more and 30 μm or less, and 10 μm or more and 30 μm or less.
[0065] If the thickness of the porous layer is less than 0.1 μm, a short circuit may occur in the lithium rechargeable battery due to deterioration of coating uniformity. If the thickness exceeds 30 μm, the ion conductivity of lithium ions may decrease, which may reduce battery performance, and the energy density of the lithium rechargeable battery may deteriorate due to an increase in volume when a plurality of unit cells are stacked.
[0066] Meanwhile, the lithium rechargeable battery electrode may be a negative electrode for a lithium rechargeable battery, or may be a positive electrode for a lithium rechargeable battery. As described above, when the provided lithium rechargeable battery electrode is applied, a separate porous polymer separator may not be provided, sufficient interfacial bonding strength with the positive electrode may be ensured, and battery life may also be relatively increased.
[0067] Meanwhile, an electrode for a lithium rechargeable battery can be obtained by applying a composition for forming a porous layer including a binder including a urethane (meth)acrylate-based monomer or oligomer and inorganic fine particles onto an electrode substrate, and thermally or photocuring the applied resultant.
[0068] In the step of coating the composition for forming the porous layer, conventional coating methods known in the art can be used, for example, various methods such as spin coating, dip coating, die coating, roller coating, comma coating, gravure coating, rod coating, curtain coating, extrusion coating, casting, screen printing, inkjet printing, blade coating, or a combination of these can be used.
[0069] In the step of photocuring the composition for forming the porous layer, ultraviolet light or visible light having a wavelength of 200 nm to 400 nm may be irradiated, and the exposure amount during the irradiation is preferably 100 mJ / cm 2 Up to 4,000mJ / cm 2 The exposure time is also not particularly limited and may be appropriately changed depending on the exposure device used, the wavelength of the irradiated light, or the exposure amount.
[0070] Furthermore, in the step of photocuring the photocurable coating composition, nitrogen purge or the like may be performed to apply a nitrogen atmosphere condition.
[0071] The composition for forming the porous layer can be applied and dried after curing. In the drying step, the drying method is not particularly limited, and any known method can be used. Examples include drying using warm air, hot air or low humidity air, vacuum drying, and drying using infrared or electron beam irradiation. For example, drying can be carried out in a drying chamber under normal pressure or pressurized conditions, optionally by applying heat or hot air to the substrate.
[0072] The temperature applied during drying is not particularly limited, but can be determined according to the type of components, solvents or non-solvents used. For example, drying can be performed at temperatures of 60°C or higher, 80°C or higher, 90°C or higher, and 150°C or lower, 120°C or lower, 110°C or lower, 80°C or higher and 140°C or lower, 90°C or higher and 120°C or lower, 80°C or higher and 110°C or lower, 90°C or higher and 110°C or lower.
[0073] When the composition for forming the porous layer is photocured, a photopolymerization initiator may be included. The photopolymerization initiator may be used without particular limitation, as long as it is a compound known to be used in a photocurable resin composition. Specifically, a benzophenone-based compound, an acetophenone-based compound, a biimidazole-based compound, a triazine-based compound, an oxime-based compound, or a mixture of two or more thereof may be used.
[0074] The composition for forming the porous layer may further comprise an organic solvent. Non-limiting examples of organic solvents include ketones, alcohols, acetates and ethers, or mixtures of two or more thereof. Specific examples of such organic solvents include ketones, such as methyl ethyl ketone, methyl isobutyl ketone, acetylacetone or isobutyl ketone; alcohols, such as methanol, ethanol, diacetone alcohol, n-propanol, isopropanol, n-butanol, isobutanol or tert-butanol; acetates, such as ethyl acetate, isopropyl acetate or polyethylene glycol monomethyl ether acetate; ethers, such as tetrahydrofuran or propylene glycol monomethyl ether; or mixtures of two or more thereof.
[0075] Meanwhile, the composition for forming the porous layer may further optionally contain a dispersant.
[0076] The dispersant can improve the dispersibility of the inorganic fine particles or prevent the particles from agglomerating during the formation of the porous layer, and can improve the surface characteristics of the produced porous layer, thereby improving the mechanical characteristics, resistance characteristics, and the like of the porous layer.
[0077] After separately forming a particle dispersion containing inorganic fine particles, a dispersant and an organic solvent, the particle dispersion can also be mixed with a photocurable composition containing a binder and a photopolymerization initiator to form a composition for forming a porous layer, wherein the binder contains a monomer or oligomer based on urethane (meth) acrylate. The porous layer can be formed by thermally curing or photocuring the resultant thus applied.
[0078] The type and the like of the dispersant are not particularly limited, but specific examples of the dispersant include monoesters or diesters of phosphoric acid having an acid value of 90 KOH / g to 110 KOH / g or acidic dicarboxylic acid monoesters.
[0079] More specifically, the following groups of dispersants may be used: (a) monoesters or diesters of phosphoric acid, for example monoesters or diesters of phosphoric acid containing alkyl, aryl, aralkyl or alkylaryl alkoxylates (for example nonylphenol ethoxylates, isotridecanol ethoxylates, alkylene oxide polyethers prepared starting from butanol), monoesters or diesters of phosphoric acid containing polyesters (for example lactone polyesters, such as caprolactone polyesters or mixed caprolactone / valerolactone polyesters), or
[0080] (b) Acidic dicarboxylic acid monoesters, examples being acidic dicarboxylic acid monoesters (more particularly monoesters of succinic acid, maleic acid or phthalic acid) comprising alkyl, aryl, aralkyl or alkylaryl alkoxylates (for example nonylphenol ethoxylate, isotridecanol ethoxylate or alkylene oxide polyethers prepared starting from butanol), and the like.
[0081] The content or amount of the dispersant is not particularly limited, but for example, 0.01 to 30 parts by weight, 0.1 to 20 parts by weight, 0.5 to 15 parts by weight, or 1 to 10 parts by weight of the dispersant can be used relative to 100 parts by weight of the inorganic fine particles.
[0082] Meanwhile, according to another embodiment of the present invention, a lithium rechargeable battery including the lithium rechargeable battery electrode may be provided. Specifically, the lithium rechargeable battery may include the lithium rechargeable battery electrode of one embodiment, a counter electrode, and an electrolyte interposed therebetween.
[0083] The electrode for a lithium rechargeable battery may be a positive electrode for a lithium rechargeable battery, or may be a negative electrode for a lithium rechargeable battery.
[0084] Electrodes for lithium rechargeable batteries include all of the above.
[0085] As described above, a lithium rechargeable battery of one embodiment includes a lithium rechargeable battery electrode, wherein the lithium rechargeable battery electrode includes a porous layer as a separator instead of a porous polymer separator including a porous substrate and a coating formed on the porous substrate, and even if the electrode expands and contracts, the adhesion is maintained, thereby making it possible to achieve excellent battery life characteristics.
[0086] The negative electrode may include: a negative electrode material including a negative electrode active material, a conductive material, and a binder; and a current collector supporting the negative electrode material.
[0087] The negative electrode active material may include a material capable of reversibly intercalating and deintercalating lithium ions, lithium metal, a lithium metal alloy, a material capable of doping and dedoping lithium, and a transition metal oxide.
[0088] As materials capable of reversibly embedding and de-embedding lithium ions, crystalline carbon, amorphous carbon, or mixtures thereof as carbonaceous materials can be cited. Specifically, the carbonaceous material can be natural graphite, artificial graphite, crystalline graphite, pyrolytic carbon, mesophase pitch, carbon fiber based on mesophase pitch, mesophase carbon microbeads, petroleum or coal tar pitch derived coke, soft carbon, hard carbon, etc.
[0089] The lithium metal alloy may include an alloy of lithium and a metal selected from the following: Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, Sn, Bi, Ga, and Cd.
[0090] Materials capable of doping and de-doping lithium may include Si, Si-C composite materials, SiO x (0 < x < 2), Si-Q alloys (where Q is an element selected from the following: alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, but not Si), Sn, SnO2, Sn-R alloys (where R is an element selected from the following: alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, but not Sn), etc.
[0091] In addition, as materials capable of doping and de-doping lithium, at least one of the above examples may be mixed with SiO2 and then used. Q and R may be Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, etc.
[0092] In addition, transition metal oxides may include vanadium oxides, lithium vanadium oxides, lithium titanium oxides, etc.
[0093] The negative electrode current collector is generally manufactured to have a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the corresponding battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc., aluminum cadmium alloy, etc. may be used.
[0094] In addition, similar to the positive electrode current collector, the negative electrode current collector may also be processed to form fine irregularities on its surface to enhance the adhesion to the negative electrode active material, and the current collector may be used in various forms, such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabric structures.
[0095] Preferably, the negative electrode may include a negative electrode active material, which includes at least one selected from carbonaceous materials and silicon compounds.
[0096] Here, the carbonaceous material is a material containing at least one selected from the following: natural graphite, artificial graphite, crystalline graphite, pyrolytic carbon, mesophase pitch, mesophase pitch-based carbon fiber, mesophase carbon microbeads, petroleum or coal tar pitch-derived coke, soft carbon, and hard carbon, as exemplified above. In addition, the silicon compound may be the Si-containing compound exemplified above, i.e., Si, Si-C composite material, SiOx (where 0 < x < 2), Si-Q alloy, a mixture thereof, or a mixture of at least one of them and SiO2.
[0097] In addition, the negative electrode may contain microsilicon. When the negative electrode contains microsilicon, a more excellent capacity can be achieved compared with the case of using a carbonaceous material as the negative electrode active material. Specifically, when using a specific microsilicon as the silicon compound, even after charging and discharging 500 times or more, a remaining capacity of 80% or more can be maintained, and an energy density significantly more excellent than that of a conventional lithium rechargeable battery can be achieved. In addition, when the negative electrode contains microsilicon, the charge / discharge life of a solid battery using a solid electrolyte can be greatly increased, and the charging speed at room temperature can also be greatly improved.
[0098] Although the size of the microsilicon is not particularly limited, for example, the microsilicon may have a diameter of 100 μm or less, or a diameter of 1 μm to 100 μm, or a diameter of 1 μm to 20 μm.
[0099] Meanwhile, the negative electrode active material may be included in an amount of 85% by weight to 98% by weight relative to the total weight of the negative electrode material.
[0100] Specifically, the content of the negative electrode active material may be 85% by weight or more, or 87% by weight or more, or 90% by weight or more; and 98% by weight or less, or 97% by weight or less, or 96% by weight or less relative to the total weight of the negative electrode material. Preferably, the content of the negative electrode active material may be 85% by weight or more and 98% by weight or less, 85% by weight or more and 97% by weight or less, 85% by weight or more and 96% by weight or less, 87% by weight or more and 98% by weight or less, 87% by weight or more and 97% by weight or less, 87% by weight or more and 96% by weight or less, 90% by weight or more and 98% by weight or less, 90% by weight or more and 97% by weight or less, 90% by weight or more and 96% by weight or less.
[0101] The conductive material is used to impart conductivity to the electrode.
[0102] The conductive material can be used without particular limitation, as long as it has electronic conductivity without causing chemical changes in the battery. As non-limiting examples, the conductive material may include carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon graphene, and carbon fiber; graphite such as natural graphite and artificial graphite; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. As the conductive material, any one of the above examples alone or a mixture of two or more thereof may be used.
[0103] The content of the conductive material can be adjusted within a range that does not cause a decrease in the capacity of the battery while exhibiting an appropriate level of conductivity. Preferably, the content of the conductive material can be 0.5 wt % to 10 wt %, or 1 wt % to 10 wt %, or 1 wt % to 5 wt %, relative to the total weight of the negative electrode material.
[0104] The binder is used to properly attach the negative electrode material to the current collector. As a non-limiting example, the binder may include polyvinylidene fluoride (PVdF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene copolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, etc. As a binder, any one of the above examples alone or a mixture of two or more thereof may be used.
[0105] The content of the binder can be adjusted within the range of not causing a decrease in battery capacity while showing an appropriate level of adhesion. Preferably, the content of the binder can be 0.5 wt % to 10 wt %, 1 wt % to 10 wt %, or 1 wt % to 5 wt % relative to the total weight of the negative electrode material.
[0106] The lithium rechargeable battery may also optionally include a porous polymer substrate.
[0107] The type of the porous polymer substrate is not particularly limited, but for example, a polymer substrate formed of one or more polymers selected from the group consisting of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene ether, cyclic olefin copolymer, polyphenylene sulfide and polyethylene naphthalate, or a mixture of two or more thereof, or a multilayer film, woven fabric or nonwoven fabric thereof can be used.
[0108] The porous polymer substrate can adjust the type and thickness of the substrate, the diameter and number of pores, and especially the thickness of ultrafine filaments in the case of nonwoven fabrics, taking into account melting temperature, manufacturing convenience, porosity, ion movement, insulating properties, etc.
[0109] The thickness of the porous polymer substrate is not particularly limited, and can be adjusted to, for example, 0.01 μm to 100 μm in consideration of battery performance.
[0110] The positive electrode for a lithium rechargeable battery may include a positive electrode active material, a binder, a conductive material, and a positive electrode additive.
[0111] The positive electrode additive for lithium rechargeable batteries has the property of irreversibly releasing lithium during charging and discharging of the lithium rechargeable batteries. Therefore, the positive electrode additive for lithium rechargeable batteries can be included in the positive electrode for lithium rechargeable batteries and used as a sacrificial positive electrode material for pre-lithiation.
[0112] Specifically, the positive electrode may be manufactured by coating the positive electrode mixture on a positive electrode current collector and then drying it, and if necessary, a filler may also be added to the mixture.
[0113] A positive electrode for a lithium rechargeable battery includes a positive electrode material including a positive electrode active material, a conductive material, a sacrificial positive electrode material, and a binder; and a current collector supporting the positive electrode material.
[0114] As the development towards higher capacity batteries progresses, in order to increase the capacity of the battery, the proportion of negative electrode active material in the negative electrode must be higher, which also increases the amount of lithium consumed in the SEI layer. Therefore, the design capacity of the battery can be determined by calculating the amount of lithium consumed in the SEI layer of the negative electrode and then back-calculating the amount of sacrificial positive electrode material to be applied to the positive electrode side.
[0115] According to one embodiment, the sacrificial positive electrode material may be included in an amount greater than 0 wt % and 15 wt % or less relative to the total weight of the positive electrode material. In order to compensate for the irreversible lithium consumed in the formation of the SEI layer, the content of the sacrificial positive electrode material is preferably greater than 0 wt % relative to the total weight of the positive electrode material. However, when the sacrificial positive electrode material is excessively included, the content of the positive electrode active material exhibiting a reversible charge / discharge capacity decreases, and the capacity of the battery decreases, and the residual lithium in the battery is plated on the negative electrode, causing the battery to short-circuit or compromise safety. Therefore, the content of the sacrificial positive electrode material is preferably 15 wt % or less relative to the total weight of the positive electrode material.
[0116] Specifically, relative to the total weight of the positive electrode material, the content of the sacrificial positive electrode material can be greater than 0% by weight, or 0.5% by weight or more, or 1% by weight or more, or 2% by weight or more, or 3% by weight or more; and 15% by weight or less, or 12% by weight or less, or 10% by weight or less.
[0117] As the positive electrode active material, compounds known in the technical field to which the present invention pertains and applicable to lithium rechargeable batteries can be used without particular limitation.
[0118] As non-limiting examples, the positive electrode active material can include NCM (Li[Ni,Co,Mn]O2), NCMA (Li[Ni,Co,Mn,Al]O2), LiCoO2, LiNiO2, LiMnO2, LiMn2O2, LiNi 1-d Co d O2, LiCo 1-d Mn d O2, LiNi 1-d Mn d O2 (where 0 ≤ d < 1), Li(Ni a Co b Mn c )O4 (0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-e Ni e O4, LiMn 2- e Co e O4 (where 0 < e < 2), LiCoPO4, LiFePO4, etc. As the positive electrode active material, one or a mixture of two or more of the above examples can be used.
[0119] According to one embodiment of the present invention, relative to the total weight of the positive electrode material, the positive electrode active material can be included in an amount of 80% to 98% by weight. Specifically, relative to the total weight of the positive electrode material, the content of the positive electrode active material can be 80% by weight or more, or 82% by weight or more, or 85% by weight or more, and 98% by weight or less.
[0120] The positive electrode for lithium rechargeable battery can be formed by stacking a positive electrode material including a positive electrode active material, a conductive material, a sacrificial positive electrode material and a binder on a current collector. The filler is selectively used as a component to suppress the expansion of the positive electrode, and is not particularly limited as long as it is a fiber material that does not cause chemical changes in the battery. For example, olefin polymers such as polyethylene and polypropylene are used; and fiber materials such as glass fiber and carbon fiber. The details of the conductive material, binder and current collector contained in the positive electrode material include all of the above.
[0121] Meanwhile, the electrolyte can be used without particular limitation as long as it is known to be applicable to lithium rechargeable batteries in the technical field to which the present invention belongs. For example, the electrolyte can include an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, a solid inorganic electrolyte, a melt inorganic electrolyte, an aqueous electrolyte, etc.
[0122] An aqueous electrolyte is an electrolyte obtained by dissolving a salt in an aqueous solvent such as water or alcohol, and a lithium rechargeable battery using such an aqueous electrolyte has advantages in terms of high ion conductivity and safety of the aqueous electrolyte, and low process and manufacturing costs. In addition, batteries using an aqueous electrolyte rather than a non-aqueous organic electrolyte have advantages in terms of the environment.
[0123] Specifically, the aqueous electrolyte may include an aqueous solvent and a lithium salt. The aqueous solvent is a solvent containing water, and is not particularly limited, but may contain 1 wt % or more of water relative to the total weight of the aqueous solvent constituting the electrolyte. As the aqueous solvent, water may be used alone, or a solvent miscible with water may be used in combination.
[0124] The water-miscible solvent may be a polar solvent, and may include, for example, at least one selected from C1 to C5 alcohols and C1 to C10 glycol ethers.
[0125] For example, the C1 to C5 alcohol may be at least one selected from methanol, ethanol, n-propanol, isopropanol, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, glycerol, and 1,2,4-butanetriol, but is not limited thereto.
[0126] In addition, the C1 to C10 glycol ether may be at least one selected from the following: ethylene glycol monomethyl ether (MG), diethylene glycol monomethyl ether (MDG), triethylene glycol monomethyl ether (MTG), polyethylene glycol monomethyl ether (MPG), ethylene glycol monoethyl ether (EG), diethylene glycol monoethyl ether (EDG), ethylene glycol monobutyl ether (BG), diethylene glycol monobutyl ether (BDG), triethylene glycol monobutyl ether (BTG), propylene glycol monomethyl ether (MFG) and dipropylene glycol monomethyl ether (MFDG), but are not limited thereto.
[0127] The lithium salt contained in the electrolyte is dissolved in the aqueous solvent and serves as a source of lithium ions in the battery, which enables the basic operation of the lithium rechargeable battery and facilitates the movement of lithium ions between the positive electrode and the negative electrode.
[0128] Specifically, the lithium salt includes LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiN(SO2F)2 (LiFSI, lithium bis(fluorosulfonyl)imide), LiCl, LiI, LiB(C2O4)2, etc. Preferably, the lithium salt may be LiPF6, LiFSI, and a mixture thereof.
[0129] The lithium salt may be included in the electrolyte at a concentration of 0.1 M to 2.0 M. The lithium salt included in this concentration range imparts appropriate conductivity and viscosity to the electrolyte, thereby exhibiting excellent electrolyte performance.
[0130] Alternatively, the electrolyte may include a non-aqueous organic solvent and a lithium salt.
[0131] The nonaqueous organic solvent may be used without particular limitation as long as it can serve as a medium through which ions involved in an electrochemical reaction of a battery can move.
[0132] Specifically, the non-aqueous organic solvent includes ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol-based solvents such as ethanol and isopropanol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched or cyclic hydrocarbon group, which may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; cyclopentane; and the like.
[0133] In the above examples, as non-aqueous organic solvent, it is preferred to use a carbonate-based solvent. In particular, considering the charge and discharge performance of the battery and the compatibility with the sacrificial positive electrode material, the non-aqueous organic solvent may preferably be a mixture of cyclic carbonates (such as ethylene carbonate and propylene carbonate) with high ionic conductivity and high dielectric constant and linear carbonates (such as ethyl methyl carbonate, dimethyl carbonate and diethyl carbonate) with low viscosity. In this case, mixing and using cyclic carbonates and linear carbonates in a volume ratio of 1:1 to 1:9 can be beneficial to achieving the above performance.
[0134] In addition, as the non-aqueous organic solvent, a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 1:2 to 1:10; or a solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) are mixed in a volume ratio of 1 to 3:1 to 9:1 can be preferably used.
[0135] The lithium salt contained in the electrolyte is dissolved in the non-aqueous organic solvent and serves as a source of lithium ions in the battery, which enables the basic operation of the lithium rechargeable battery and facilitates the movement of lithium ions between the positive electrode and the negative electrode.
[0136] Specifically, the lithium salt may include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiN(SO2F)2 (LiFSI, lithium bis(fluorosulfonyl)imide), LiCl, LiI, LiB(C2O4)2, etc. Preferably, the lithium salt may be LiPF6, LiFSI, and a mixture thereof.
[0137] The lithium salt may be included in the electrolyte at a concentration of 0.1 M to 2.0 M. The lithium salt included in this concentration range imparts appropriate conductivity and viscosity to the electrolyte, thereby exhibiting excellent electrolyte performance.
[0138] Optionally, the electrolyte may contain an additive for the purpose of improving battery life characteristics, suppressing battery capacity reduction, improving battery discharge capacity, and the like.
[0139] For example, the additive may include compounds based on haloalkylene carbonates, such as difluoroethylene carbonate; or pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride; etc. The additive may be included in an amount of 0.1 wt % to 5 wt % relative to the total weight of the electrolyte.
[0140] The lithium rechargeable battery of one embodiment may be a lithium ion battery, a lithium ion polymer battery, or a lithium polymer battery according to the type of electrolyte.
[0141] The liquid electrolyte may be a non-aqueous electrolyte containing a lithium salt. The non-aqueous electrolyte containing a lithium salt is composed of a non-aqueous electrolyte and lithium, and the non-aqueous electrolyte includes a non-aqueous organic solvent, an organic solid electrolyte, an inorganic solid electrolyte, etc., but is not limited thereto.
[0142] The organic solid electrolyte may include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociative groups.
[0143] As inorganic solid electrolytes, Li nitrides, halides and sulfates such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH and Li3PO4-Li2S-SiS2 can be used.
[0144] Additionally, in order to improve the charge / discharge characteristics and flame retardancy, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N, N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum chloride, etc. If necessary, in order to impart non-flammability, the non-aqueous electrolyte may also include a halogen-containing solvent such as carbon tetrachloride and ethylene trifluoride. In addition, in order to improve high temperature storage characteristics, the non-aqueous electrolyte may also include carbon dioxide gas, etc., and may also include fluoroethylene carbonate (FEC), propylene sulfone (PRS), etc.
[0145] In one specific example, a lithium salt-containing non-aqueous electrolyte can be prepared by adding a lithium salt (e.g., LiPF6, LiClO4, LiBF4, and LiN(SO2CF3)2) to a mixed solvent of a cyclic carbonate (e.g., EC or PC) as a high dielectric solvent and a linear carbonate (e.g., DEC, DMC, or EMC) as a low viscosity solvent.
[0146] Lithium rechargeable batteries can be used as energy sources with improved performance and safety in the fields of portable electronic devices such as mobile phones, laptops, tablets, mobile batteries, and digital cameras, and in the fields of transportation vehicles such as electric vehicles, electric motorcycles, and personal mobile devices.
[0147] The lithium rechargeable battery may have various shapes, such as a prismatic shape, a cylindrical shape, and a pouch shape.
[0148] The lithium rechargeable battery of another embodiment described above may be implemented as a battery module including the same as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source.
[0149] At this time, specific examples of the device may be an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and a system for power storage, but are not limited thereto.
[0150] In the above embodiment, the porous layer is coated and then assembled through a process such as winding or stacking (lamination), and then an electrolyte is injected therein, thereby manufacturing a lithium rechargeable battery.
[0151] On the other hand, when the lithium rechargeable battery electrode is peeled at 90 degrees relative to the counter electrode, the lithium rechargeable battery of one embodiment may have a peel strength of 10 gf / 20 mm or more. The peel strength may be achieved according to the composition of the porous layer.
[0152] Specifically, when the electrode for a lithium rechargeable battery is peeled at 90 degrees relative to the counter electrode, the peel strength of the lithium rechargeable battery of one embodiment may be 10 gf / 20 mm or more, 20 gf / 20 mm or more, 30 gf / 20 mm or more, 200 gf / 20 mm or less, 180 gf / 20 mm or less, 150 gf / 20 mm or less, and 10 gf / 20 mm or more and 200 gf / 20 mm or less, 20 gf / 20 mm or more and 200 gf / 20 mm or less, 30 gf / 20 mm or more and 180 gf / 20 mm or less, 30 gf / 20 mm or more and 150 gf / 20 mm or less.
[0153] When the electrode for a lithium rechargeable battery is peeled at 90 degrees with respect to the counter electrode, the peel strength may be 10 gf / 20 mm or more. The peel strength may be measured using a texture analyzer according to the ASTM D6862 measuring method.
[0154] In addition, the coulombic efficiency of the lithium rechargeable battery of the above embodiment may be 75% or more and 99% or less, 75% or more and 90% or less, and 75% or more and 83% or less. The coulombic efficiency may be calculated as the ratio of the discharge capacity to the charge capacity.
[0155] Beneficial Effects
[0156] An electrode for a lithium rechargeable battery and a lithium rechargeable battery including the same can be provided, wherein the electrode for a lithium rechargeable battery not only has high high temperature stability, strong structural stability, and high interface bonding strength with a counter electrode, but also can improve the life characteristics, charging capacity, and discharging capacity of the lithium rechargeable battery and has high bending resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0157] Figure 1 The method for measuring the bending resistance in Experimental Example 1 is schematically shown. DETAILED DESCRIPTION
[0158] Hereinafter, the action and effect of the present invention will be described in more detail with reference to specific embodiments of the present invention. However, this is given as an embodiment to help understand the present invention. The following examples are not intended to limit the scope of the present invention in any way.
[0159] <Preparation Examples 1 to 6: Preparation of Particle Dispersion Liquid and Coating Composition for Forming Porous Layer>
[0160] (1) Preparation of particle dispersion
[0161] The components of the particle dispersion listed in Table 1 below were mixed and then shaken at 200 rpm for 24 hours in an orbital shaker using 1 mm beads to form a particle dispersion.
[0162] (2) Preparation of coating composition for forming porous layer
[0163] After the components of the photocurable composition shown in Table 1 below were mixed, they were mixed with the obtained particle dispersion to prepare a coating composition for forming a porous layer.
[0164] [Table 1]
[0165]
[0166] MIBK: Methyl isobutyl ketone
[0167] CyH: Cyclohexanone
[0168] Boehmite: Aluminum hydroxide particles having an average particle size of primary particles of about 50 nm to 60 nm and a D50 of secondary particles of about 130 nm.
[0169] Dispersant (BYK-102): Poly(oxy-1,2-ethanediyl) α-isotridecyl-w-hydroxy-phosphate copolymer with acidic groups (acid value: 101 mg KOH / g)
[0170] UA5216 (manufactured by Miwon Specialty): Contains about 40% of polyester urethane diacrylate (weight average molecular weight: 30,000 g / mol) (diluted with isobornyl acrylate)
[0171] BR-345: Bifunctional polyether urethane acrylate (trade name, Bomar product, solid content: about 100% by weight)
[0172] Linc-3A: Fluorine-based (meth)acrylate compound (manufacturer: KYOEISHA, solid content: about 100% by weight)
[0173] DPHA: Dipentaerythritol hexaacrylate
[0174] PETA: Pentaerythritol triacrylate
[0175] IBOA: Isobornyl acrylate
[0176] HEA: 2-Hydroxyethyl Acrylate
[0177] <Examples and Comparative Examples: Production of Lithium Rechargeable Battery Electrode and Lithium Rechargeable Battery>
[0178] Examples 1 to 4
[0179] (1) Fabrication of single-side negative electrode
[0180] Carbon-based powder and silicon-based powder as negative electrode active materials, carbon black as conductive material, and styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) as binders were added to distilled water (deionized water) as a solvent in an amount of 91.5 wt %, 4 wt %, 1.5 wt %, 2 wt % and 1 wt %, respectively, to prepare a slurry for an electrode layer. The slurry for an electrode layer was applied to one surface of a copper (Cu) film having a thickness of 10 μm as a current collector, dried, and then rolled to manufacture an electrode.
[0181] (2) Production of half-cell (single-side)
[0182] The composition for forming a porous layer obtained above was applied to the single-sided electrode manufactured above to a constant thickness of 15 to 20 μm using a #30 Mayer rod and dried at 110° C. for 2 minutes to manufacture a negative electrode having a porous layer formed thereon.
[0183] A lithium metal with a thickness of 0.3 mm was assembled on a negative electrode on which a porous layer was formed using a stacking method, and an electrolyte solution (ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (volume ratio), 1 mol lithium hexafluorophosphate (LiPF6)) was injected into the assembled battery to produce a lithium rechargeable battery.
[0184] Comparative Examples 1 and 2
[0185] A lithium rechargeable battery electrode and a lithium rechargeable battery were manufactured in the same manner as in Example 1, except that the particle dispersions and the coating compositions for forming a porous layer of Preparation Examples 5 and 7 were used, respectively.
[0186] <Experimental example>
[0187] Experimental Example 1: Measurement of bending resistance
[0188] like Figure 1 As shown, the negative electrode single-side electrode including the porous layer manufactured in the examples and comparative examples was subjected to a cylindrical mandrel test from a large diameter to a small diameter according to the ISO1519:2011 standard method to determine the bending resistance.
[0189] The sample was prepared by cutting it into a size of 12 cm long and 2.5 cm wide. The copper current collector surface of the negative electrode single-side electrode was brought into contact with a portion of the cylindrical mandrel, and the negative electrode single-side sample was slowly rolled on the cylindrical mandrel so that the coating could be bent 180 degrees.
[0190] The bending resistance value is determined by the diameter of the largest first mandrel at which cracks appear in the coating or the coating and the electrode layer together separate from the current collector.
[0191] Experimental Example 2: Analysis of Porous Layer
[0192] The thickness and porosity of the porous layer of the lithium rechargeable battery produced in each of Examples and Comparative Examples were analyzed and shown in Table 1 below.
[0193] The porosity of the porous layer was calculated as follows. The thickness of the porous layer was measured to calculate the volume of a certain area of the porous layer. Only the weight of the porous layer was calculated, excluding the weight of the electrode substrate and the current collector in the sample weight, and the actual density of the porous layer was calculated by dividing the weight by the volume. The theoretical density when the solid components of the porous layer were 100% dense was calculated, and the porosity was calculated according to the following mathematical equation 1.
[0194] [Mathematical equation 1]
[0195] Porosity (%)={1-(actual density) / (theoretical density)}×100.
[0196] Experimental Example 3: Adhesion Strength
[0197] The negative electrode single-sided electrode including the porous layer manufactured in the embodiment and the comparative example is cut into a size of 2 cm wide and 10 cm long to prepare a sample. The sample is fixed on a 0.1T glass plate using 3M double-sided tape so that the porous layer is in contact with the double-sided tape. At this time, the sample is positioned so that the short side of the sample overlaps the short side of the slide. The other end that is not fixed to the double-sided tape is peeled off at 90 degrees, and the peel strength value is measured using a texture analyzer (model name: TA.XT plus100, Stable micro systems) according to the ASTM D6862 measurement method, and is shown in Table 2 below.
[0198] Experimental Example 4: Electrochemical Characteristics
[0199] The negative electrodes having the porous layer prepared in the examples and comparative examples were vacuum dried at 80° C. for 10 hours and then fabricated into coin cells, and the ion conduction resistance was measured.
[0200] To produce a coin cell, the negative electrode with a porous layer is punched into a circle with a diameter of 16 mm, placed in a coin cell can so that the porous layer is visible, and then 0.1 ml of an electrolyte solution (EC / EMC=3 / 7 volume %, VC 2%) is injected. A spacer is placed on the porous layer, lithium metal for the positive electrode punched into a diameter of 15 mm is added, the can is closed, and then a coin cell is produced. After waiting for 2 hours at room temperature and 10 hours at 45 degrees so that the electrolyte solution can penetrate well, 3 charge / discharge cycles are performed under the conditions of 0.1C discharge and 0.1C charge, and the first discharge capacity is determined. The first coulomb efficiency is calculated according to the following equation:
[0201] First coulombic efficiency = (first cycle discharge capacity) / (first cycle discharge capacity) * 100 (%)
[0202] The charge capacity retention rate and discharge capacity retention rate were measured by C-rate analysis using coin cells subjected to 3 charge / discharge cycles. Specifically, 3 charge / discharge cycles were performed in the order of 0.33C, 1C, 2C, 3C and 0.33C, and then the ratio of the average value of the final charge capacity at 0.33C to the average value of the initial charge capacity at 0.33C was calculated to determine the charge capacity retention rate. The discharge capacity retention rate was also obtained by calculating the ratio of the average value of the final discharge capacity at 0.33C to the average value of the initial discharge capacity at 0.33C.
[0203] [Table 2]
[0204]
[0205] As shown in Table 2, it was determined that the lithium rechargeable battery of the example exhibited a peel strength of 49 gf / 20 mm or more between the porous layer and the counter electrode, and thus could achieve excellent electrode adhesive strength.
[0206] In addition, it was determined that the lithium rechargeable batteries of Examples 1 to 4 exhibited a discharge capacity of 8000 mAh / g or greater, a coulombic efficiency of 85% or greater, an ion conduction resistance of 0.37 kV / minch or greater and 0.4 kV / minch or less, a discharge capacity retention rate of 85% or greater, and a charge capacity retention rate of 75% or greater, and that sufficient battery efficiency and operating performance could be ensured.
[0207] On the other hand, the lithium rechargeable batteries of Comparative Examples 1 and 2 remain at low levels in terms of discharge capacity, coulombic efficiency, discharge capacity retention rate, and charge capacity retention rate. In particular, the lithium ion battery of Comparative Example 2 is expected to undergo interface peeling due to insufficient bonding strength when the electrodes expand and contract, which causes a decrease in battery life characteristics.
Claims
1. An electrode for a lithium rechargeable battery, comprising: an electrode substrate, and A porous layer is formed on the electrode substrate, the porous layer comprising a binder resin and inorganic fine particles, the binder resin comprising a (co)polymer containing a repeating unit derived from a urethane (meth)acrylate-based monomer or oligomer.
2. The lithium rechargeable battery electrode according to claim 1, wherein: The porous layer has a porosity of 40% or more and 80% or less.
3. The electrode for a lithium rechargeable battery according to claim 1, wherein: The porous layer includes pores having a cross-sectional diameter of 20 nm to 2000 nm.
4. The electrode for a lithium rechargeable battery according to claim 1, wherein: The porous layer includes 1 to 50 parts by weight of the binder resin relative to 100 parts by weight of the inorganic fine particles.
5. The electrode for a lithium rechargeable battery according to claim 1, wherein: The urethane (meth)acrylate-based oligomer has a weight average molecular weight of 3,000 g / mol to 50,000 g / mol.
6. The electrode for a lithium rechargeable battery according to claim 1, wherein: The urethane (meth)acrylate-based monomer or oligomer includes at least one selected from the group consisting of polyester (meth)urethane acrylate, polyester urethane di(meth)acrylate, polyether (meth)urethane acrylate, and polyether urethane di(meth)acrylate.
7. The electrode for a lithium rechargeable battery according to claim 1, wherein: The (co)polymers also contain repeating units derived from multifunctional acrylates.
8. The electrode for a lithium rechargeable battery according to claim 1, wherein: The inorganic fine particles include at least one selected from the group consisting of alumina (Al2O3), boehmite (AlOOH), aluminum hydroxide (Al(OH)3), silicon dioxide (SiO2), titanium dioxide (TiO2), and magnesium hydroxide (Mg(OH)2).
9. The electrode for a lithium rechargeable battery according to claim 1, wherein: The inorganic fine particles include boehmite including primary particles having an average particle diameter of 10 nm to 500 nm.
10. The electrode for a lithium rechargeable battery according to claim 1, wherein: The inorganic fine particles include inorganic fine particles surface-modified with at least one compound selected from the group consisting of (meth)acrylates, thiols, and organic silane compounds.
11. The electrode for a lithium rechargeable battery according to claim 1, wherein: The thickness of the porous layer is 0.1 μm or more and 30 μm or less.
12. The electrode for a lithium rechargeable battery according to claim 1, wherein: The electrode substrate is a negative electrode substrate, and The electrode for a lithium rechargeable battery is a negative electrode for a lithium rechargeable battery.
13. The electrode for a lithium rechargeable battery according to claim 1, wherein: When the electrode for a lithium rechargeable battery is wound on a cylindrical mandrel having a diameter of 2 mm or more according to the ISO 1519:2011 standard method, cracks do not occur.
14. A lithium rechargeable battery comprising the electrode for a lithium rechargeable battery according to claim 1.
15. The lithium rechargeable battery according to claim 14, comprising: The lithium rechargeable battery electrode; and A counter electrode is in contact with the porous layer included in the electrode for a lithium rechargeable battery.