Production of lithium hydroxide and lithium carbonate
The generation of lithium hydroxide and lithium carbonate through electrolysis and reaction steps is solved, and the problems of low efficiency and high cost in the prior art are achieved, and efficient and low waste lithium compound production is achieved.
Patent Information
- Application Number
- CN202410646534.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The existing lithium hydroxide and lithium carbonate production processes are inefficient and require high-cost reagents and generate large amounts of waste, resulting in insufficient in reducing waste and material reuse.
By electrolyzing the potassium chloride solution, a potassium hydroxide solution is generated and reacted with the lithium chloride solution to form a reciprocal salt system, precipitating potassium chloride and lithium hydroxide, and then producing lithium hydroxide and lithium carbonate. This method can reduce the use of Reliance on lime, soda ash, hydrochloric acid and sodium hydroxide and improves the purity and efficiency of the product by repeating electrolysis, reaction and precipitation steps.
It realizes efficient production of lithium hydroxide and lithium carbonate, reduces production costs, reduces waste generation, improves resource reuse rate, and improves production efficiency.
Smart Images

Figure CN119018913A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application is a partial continuation (CIP) application of U.S. patent application No. 17 / 658,647 filed on April 8, 2022. U.S. patent application No. 17 / 658,647 is a continuation application of U.S. patent application No. 17 / 395,457 filed on August 6, 2021. U.S. patent application No. 17 / 395,457 was published and authorized on May 24, 2022 as U.S. Patent No. 11,339,481.
[0003] Incorporated by Reference
[0004] All documents cited in this application, including but not limited to any published applications and / or patents in the sequential chain of this application, are hereby incorporated by reference in their respective entireties. Technical Field
[0005] The field of the present disclosure relates generally to lithium production, and more particularly to the production of lithium hydroxide and lithium carbonate. Background Art
[0006] Although lithium is widely distributed on Earth, there are few commercial sources of concentrated lithium suitable for producing lithium compounds (such as lithium carbonate and lithium hydroxide). These lithium compounds are needed by a variety of industries, including but not limited to the pharmaceutical and energy industries. One source of lithium is minerals, such as spodumene. Another source is naturally occurring brines, such as those found in salt marshes, salt lakes, salt mines, and geothermal resources.
[0007] An emerging source of lithium is used batteries collected from scrapped electronics and e-waste, electric bicycles, power tools and electric vehicles. After discharge, these batteries are shredded, separating plastic, aluminum and copper foil in the process. The remaining material is a "black mass" containing lithium and other valuable metals such as nickel, cobalt and manganese. Once the lithium is extracted and concentrated, conventional methods react the resulting lithium solution with one or more reagents to produce lithium hydroxide or lithium carbonate. However, these reagents (which may include lime, soda ash, hydrochloric acid and sodium hydroxide, etc.) are expensive to obtain, may contain harmful impurities and produce additional waste streams such as calcium carbonate, sodium chloride and sodium sulfate.
[0008] In addition, existing lithium hydroxide and lithium carbonate production processes may be inefficient and need to be improved in terms of waste reduction and material reuse. Therefore, a more cost-effective and efficient method and system for producing lithium hydroxide and lithium carbonate is needed. Summary of the invention
[0009] An exemplary method for producing lithium hydroxide is described.
[0010] One or more embodiments of the method include: electrolyzing a potassium chloride solution to obtain a potassium hydroxide solution, a depleted potassium chloride solution, chlorine gas, and hydrogen gas; reacting the potassium hydroxide solution with a lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide, and water; and precipitating potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals.
[0011] Another exemplary method for producing lithium hydroxide is described. One or more embodiments of the method include: electrolyzing a potassium chloride solution to obtain a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas; reacting the potassium hydroxide solution with a lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide, and water; precipitating potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals; dissolving the potassium chloride crystals in water or a lean potassium chloride solution and filtering the resulting mixture to obtain a potassium chloride solution; and repeating the electrolysis, reaction, precipitation, and dissolution steps.
[0012] Other exemplary methods for producing lithium hydroxide are described. One or more embodiments of the method include: electrolyzing a potassium chloride solution to obtain a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas; reacting the potassium hydroxide solution with a lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide, and water; precipitating potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals; and purifying the lithium hydroxide crystals.
[0013] An exemplary system for producing lithium hydroxide is described. One or more embodiments of the system include: at least one electrolytic cell, wherein the at least one electrolytic cell is configured to electrolyze a potassium chloride solution to obtain a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas; at least one reactor, wherein the at least one reactor is configured to react the potassium hydroxide solution with the lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide, and water; and at least one crystallizer, wherein the at least one crystallizer is configured to precipitate potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals.
[0014] Another exemplary system for producing lithium hydroxide is described. One or more embodiments of the system include: at least one electrolytic cell, wherein the at least one electrolytic cell is configured to electrolyze a potassium chloride solution to obtain a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas; and at least one reactor, wherein the at least one reactor is configured to react the potassium hydroxide solution with the lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide, and water, and precipitate potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals.
[0015] An exemplary method for producing lithium carbonate is described. One or more embodiments of the method include: electrolyzing a potassium chloride solution to produce a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas; reacting the potassium hydroxide solution with a carbon dioxide source to form a potassium carbonate solution; and reacting the potassium carbonate solution with a lithium chloride solution to produce a product mixture including potassium chloride and lithium carbonate solids.
[0016] Other exemplary methods for producing lithium carbonate are described. One or more embodiments of the method include: electrolyzing potassium chloride solution to obtain potassium hydroxide solution, lean potassium chloride solution, chlorine gas, and hydrogen gas; reacting the potassium hydroxide solution with a carbon dioxide source to form a potassium carbonate solution; reacting the potassium carbonate solution with a lithium chloride solution to obtain a product mixture including potassium chloride and lithium carbonate solids; removing the lithium carbonate solids from the mixture to form a regenerated potassium chloride solution; combining the regenerated potassium chloride solution with the lean potassium chloride solution to replenish the potassium chloride solution; and repeating the electrolysis, reaction, removal, and combining steps.
[0017] Another exemplary method for producing lithium carbonate is described. One or more embodiments of the method include: electrolyzing a sodium chloride solution to produce a sodium hydroxide solution, a lean sodium chloride solution, chlorine gas, and hydrogen gas; reacting the sodium hydroxide solution with a carbon dioxide source to form a sodium carbonate solution; and reacting the sodium carbonate solution with a sodium chloride solution to produce a product mixture including sodium chloride and lithium carbonate solids.
[0018] Other exemplary methods for producing lithium carbonate are described. One or more embodiments of the method include: electrolyzing a sodium chloride solution to obtain a sodium hydroxide solution, a lean sodium chloride solution, chlorine gas, and hydrogen gas; reacting the sodium hydroxide solution with a carbon dioxide source to form a sodium carbonate solution; reacting the sodium carbonate solution with the sodium chloride solution to obtain a product mixture including sodium chloride and lithium carbonate solids; removing the lithium carbonate solids from the mixture to form a regenerated sodium chloride solution; combining the regenerated sodium chloride solution with the lean sodium chloride solution to replenish the sodium chloride solution; and repeating the electrolysis, reaction, removal, and combining steps.
[0019] An exemplary system for producing lithium carbonate is described. One or more embodiments of the system include: at least one electrolytic cell, wherein the at least one electrolytic cell is configured to electrolyze a potassium chloride solution to obtain a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas; and at least one reactor, wherein the at least one reactor is configured to react the potassium hydroxide solution with a carbon dioxide source to form a potassium carbonate solution; and react the potassium carbonate solution with a lithium chloride solution to obtain a product mixture including potassium chloride and lithium carbonate solids.
[0020] Other exemplary systems for producing lithium carbonate are described. One or more embodiments of the system include: at least one electrolytic cell, wherein the at least one electrolytic cell is configured to electrolyze a sodium chloride solution to obtain a sodium hydroxide solution, a lean sodium chloride solution, chlorine gas, and hydrogen gas; and at least one reactor, wherein the at least one reactor is configured to react the sodium hydroxide solution with a carbon dioxide source to form a sodium carbonate solution; and react the sodium carbonate solution with a lithium chloride solution to obtain a product mixture including sodium chloride and lithium carbonate solids.
[0021] Other embodiments of the method and system may include reacting a potassium hydroxide solution with a lithium chloride solution, a lithium nitrate solution, or any combination thereof to form a reciprocal salt system. In some embodiments, the reciprocal salt system may include multiple components, including but not limited to potassium hydroxide, lithium chloride, lithium nitrate, potassium chloride, potassium nitrate, lithium hydroxide, water, impurities, or any combination thereof. In some aspects, the system may allow precipitation of potassium chloride, potassium nitrate, or a combination thereof, and lithium hydroxide, thereby forming lithium hydroxide crystals and potassium chloride crystals, potassium nitrate crystals, or a combination thereof.
[0022] In some embodiments, the lithium chloride or lithium nitrate solution can be obtained by reacting calcium chloride, calcium nitrate, or a combination thereof with a lithium sulfate solution. In other embodiments, the lithium sulfate solution can be obtained from different sources, such as reacting spodumene with sulfur compounds, lithium-containing waste, or brine. In some embodiments, the lithium nitrate solution can be obtained by leaching black matter or spodumene with nitric acid.
[0023] The methods and systems of the present disclosure may also include methods such as purifying lithium hydroxide crystals and separating lithium hydroxide crystals and potassium chloride crystals, potassium nitrate crystals, or a combination thereof from a reciprocal salt system. In some embodiments, lithium hydroxide crystals may be reacted with carbon dioxide as an additional or alternative route to forming the lithium carbonate solids described throughout the present disclosure.
[0024] The embodiments covered are defined by the claims rather than the Summary. The Summary is a high-level overview of various aspects and introduces some of the concepts that are further described in the Detailed Description section below. The Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to determine the scope of the claimed subject matter. The subject matter should be understood by reference to appropriate portions of the entire specification, any or all of the drawings, and each claim. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A first example of a lithium hydroxide or lithium carbonate production system according to aspects of the present disclosure is shown.
[0026] Figure 2 A second example of a lithium production system according to aspects of the present disclosure is shown.
[0027] Figure 3 A third example of a lithium hydroxide or lithium carbonate production system according to aspects of the present disclosure is shown.
[0028] Figure 4 An example of at least one electrolytic cell according to aspects of the present disclosure is shown.
[0029] Figure 5 Exemplary current efficiencies of example membranes according to aspects of the present disclosure are shown.
[0030] Figure 6 Exemplary voltages for example membranes according to aspects of the present disclosure are shown.
[0031] Figure 7 An exemplary crystallization reactor according to aspects of the present disclosure is shown.
[0032] Figures 8 to 14 An example of a lithium production method according to aspects of the present disclosure is shown.
[0033] Fig.15 Example temperature and weight percent data are shown for exemplary reciprocal salt systems according to aspects of the present disclosure.
[0034] Fig.16 A Yeneck of an exemplary reciprocal salt system according to aspects of the present disclosure picture.
[0035] Fig.17 An example of a second exemplary crystallization reactor for conducting relative solubility tests of lithium hydroxide and potassium chloride at different temperatures in accordance with aspects of the present disclosure is shown.
[0036] Fig.18 Exemplary results of relative solubility testing of lithium hydroxide and potassium chloride at different temperatures according to aspects of the present disclosure are shown.
[0037] Fig.19 Results based on thermodynamic values from simulations of relative solubility tests of lithium hydroxide and potassium nitrate at different temperatures in accordance with various aspects of the present disclosure are shown.
[0038] Some embodiments of the present disclosure are described herein by way of example only with reference to the accompanying drawings. With specific reference now to the accompanying drawings in detail, it should be emphasized that the embodiments shown are by way of example and for the purpose of illustrative discussion of the embodiments of the present disclosure. In this regard, the description in conjunction with the accompanying drawings makes it clear to those skilled in the art how the embodiments of the present disclosure can be implemented. DETAILED DESCRIPTION
[0039] Some embodiments of the present disclosure describe methods for producing lithium hydroxide. In some examples, lithium hydroxide can be produced using lithium chloride, lithium nitrate, potassium chloride, and water as reagents. In some aspects, lithium hydroxide can be produced without using lime, soda ash, hydrochloric acid, sodium hydroxide, or a combination thereof as reagents.
[0040] In some examples, the lithium hydroxide is lithium hydroxide monohydrate. In some examples, the lithium hydroxide monohydrate is "battery grade", which is defined herein as conforming to applicable technical standards, such as, but not limited to, technical standards set by the International Organization for Standardization (ISO) or the American Society for Testing and Materials (ASTM). One such non-limiting example of a standard for determining whether lithium hydroxide monohydrate is "battery grade" is GB / T 8766-2013, which is incorporated herein by reference in its entirety. In some examples, the lithium hydroxide is a mixture of lithium hydroxide (i.e., anhydrous lithium hydroxide) and lithium hydroxide monohydrate. In this article, it is believed that the anhydrous lithium hydroxide present in the lithium hydroxide monohydrate will not adversely affect the purity of the anhydrous lithium hydroxide or lithium hydroxide monohydrate, and vice versa.
[0041] In some examples, the method of producing lithium hydroxide does not include direct electrolysis of lithium chloride. As used herein, "direct electrolysis of lithium chloride" is electrolysis in which lithium chloride is used as an electrolyte in electrolysis. Therefore, one or more embodiments of the method include: electrolysis of potassium chloride solution.
[0042] In some examples, the potassium chloride solution includes 10 wt% to 40 wt% potassium chloride based on the total weight of the potassium chloride solution. In other examples, the potassium chloride can be present in the following exemplary amounts based on the total weight of the potassium chloride solution: 20 wt% to 40 wt%, 30 wt% to 40 wt%, 10 wt% to 30 wt%, 10 wt% to 20 wt%, 20 wt% to 30 wt%, or any combination thereof.
[0043] In some instances, the potassium chloride solution is formed by obtaining potassium chloride (e.g., commercially available) and dissolving potassium chloride in water, brine, or a lean potassium chloride solution. In some instances, potassium chloride is obtained by reacting potassium hydroxide with lithium chloride (as described in more detail below). In some applications, the potassium chloride generated by reacting potassium hydroxide with lithium chloride can be reintroduced into the electrolyzer, for example, via a recycled stream.
[0044] In some embodiments, the electrolysis is performed using an electrolytic cell, as discussed in further detail below. In some examples, the electrolytic cell is a chlor-alkali electrolytic cell. As used herein, a "chlor-alkali electrolytic cell" is an electrolytic cell configured to perform the following half-cell reaction:
[0045] Anode: 2Cl - →Cl2+2e - .
[0046] Cathode: H2O+2e - →H2+2OH - .
[0047] In some examples, electrolysis is performed using at least one mercury cell that can utilize the Castner-Kellner process. A non-limiting example of at least one mercury cell is described in U.S. Pat. No. 528,322, which is incorporated herein by reference in its entirety for all purposes.
[0048] In some embodiments, the temperature at which the electrolysis is performed can be 20°C or higher, 30°C or higher, 40°C or higher, 50°C or higher, 60°C or higher, 70°C or higher, 80°C or higher, 90°C or higher, or 100°C or higher. In some examples, the temperature or operating temperature at which the electrolysis is performed is 70°C to 120°C, 90°C to 120°C, 100°C to 120°C, 110°C to 120°C, 70°C to 110°C, 70°C to 100°C, 70°C to 90°C, or any combination thereof.
[0049] In some examples, the electrolysis temperature can be the temperature of at least one electrolyte (e.g., an anolyte, a catholyte, or both) used in the electrolysis. Thus, in some examples, the temperature is measured by inserting a temperature sensor into at least one electrolyte during electrolysis. In some examples, the electrolysis can be conducted at a lower temperature during startup, during termination, or both than the operating temperature at which the electrolysis is in a "steady state." Exemplary differences between the temperatures at termination and startup and the operating temperature are described in " "Perfluorinated Membranes for KOHProduction", Product Bulletin, EI duPont de Nemours & Co., Inc., Wilmington (1988), revised edition 2001 (hereinafter referred to as “The Product Bulletin”), which is incorporated herein by reference in its entirety for all purposes.
[0050] In some instances, the electrolysis is membrane electrolysis. In some embodiments, the membrane used for membrane electrolysis is selective for positive ions. In some instances, the membrane includes at least one of the following: polyolefins, polyurethanes, polyesters, polyamides, polyketones, polysulfones, or polycarbonates. In some embodiments, the membrane may include a fluoropolymer. In some implementations, the membrane includes one or more of the following: PVDF, polyvinylidene fluoride, polytetrafluoroethylene-hexafluoropropylene (FEP), poly(ethylene-tetrafluoroethylene) (ETFE), polychlorotrifluoroethylene (PCTFE), polytetrafluoroethylene-perfluoropropyl vinyl ether (PFA), polyvinylidene fluoride-hexafluoropropylene (PVDF-co-HFP), polyvinyl fluoride (PVF) or any combination thereof. In some instances, the membrane is a sulfonated perfluorinated membrane, such as, but not limited to, a sulfonated perfluorinated membrane from DuPont TM Commercially available Nafion TM membrane.
[0051] In some examples, electrolysis of potassium chloride solution produces potassium hydroxide solution, lean potassium chloride solution, chlorine gas, and hydrogen gas.
[0052] In some examples, hydrogen and chlorine can react to form hydrochloric acid, for example, by the following reaction:
[0053] H2(g)+Cl2(g)→2HCl(aq)
[0054] In some cases, the generated hydrochloric acid can be used to adjust the pH of any solution described herein.
[0055] One or more embodiments of the method include reacting a potassium hydroxide solution with a lithium chloride solution.
[0056] In some examples, the lithium chloride solution includes 10 wt% to 50 wt% lithium chloride based on the total weight of the lithium chloride solution. In other examples, the lithium chloride can be present in the following exemplary amounts based on the total weight of the lithium chloride solution: 20 wt% to 50 wt%, 30 wt% to 50 wt%, 40 wt% to 50 wt%, 10 wt% to 40 wt%, 10 wt% to 30 wt%, 10 wt% to 20 wt%, 20 wt% to 40 wt%, or any combination thereof.
[0057] In some instances, the lithium chloride solution is obtained from naturally occurring salt water, such as, but not limited to, geothermal salt water. Other examples of naturally occurring salt water that may include lithium chloride include, but are not limited to, salt water from salt marshes, salt water from salt lakes, and salt water from salt mines, or any combination thereof. Some specific examples of naturally occurring salt water that may be suitable include, but are not limited to, salt water from Atacama Salt Marsh (Salar deAtacama), salt water from Umbre Muerto Salt Marsh (Salar de Hombre Muerto), Salar Olaroz, Salar de Cauchari, salt water from Salar de Rincon, Salar Pastos Grandes, Salar el Centenario, salt water from Salar de Maricunga (Salar deMaricunga), salt water from Tres Quebradas (Tres Quebradas), or a combination thereof. In some examples, the naturally occurring brine includes sodium, potassium, magnesium, calcium, strontium, sulfate ions, chloride ions, or any combination thereof. In some examples, the naturally occurring brine can include boron.
[0058] In some instances, the lithium chloride solution is formed by concentrating and purifying a naturally occurring brine. In some instances, the lithium chloride solution is formed by applying a direct lithium extraction method to a naturally occurring brine. In some instances, the brine may be concentrated and purified by any mechanism known in the art, such as, but not limited to, subjecting the brine to at least one of solar evaporation, mechanical evaporation, membrane filtration, chemical precipitation, solvent extraction, ion exchange, or any combination thereof. In some instances, membrane filtration includes nanofiltration, reverse osmosis, or any combination thereof. Other examples of non-limiting methods of concentration are described in: Bukowsky et al., The recovery of pure lithium chloride from "brines" containing higher contents of calcium chloride and magnesium chloride, Hydrometallurgy, Vol. 27, No. 3, 1991, pp. 317-325; and Schultze et al., Recovering Lithium Chloride from a Geothermal Brine, January 1984, US Department of the Interior, Bureau of Mines, and Garrett, D. 2004; Handbook of lithium and natural calcium chloride: their deposits, processing, uses and properties; each of the above documents is incorporated herein by reference in its entirety for all purposes.
[0059] In some instances, the lithium chloride solution is produced from a mineral source. In some instances, the mineral source is spodumene. Non-limiting examples of methods for producing lithium chloride solutions from spodumene include: U.S. Patent Nos. 2,533,246 and 3,024,083; WIPO patent application No. 2021 / 138345; and Barbosa et al., Extraction of lithium from β-spodumene using chlorination roasting with calcium chloride, Thermochimica Acta, Vol. 605, 2015, pp. 63-67; for all purposes, each of the above documents is incorporated herein by reference in its entirety. In some embodiments, the mineral source may include: petalite, lepidolite, hectorite, or any combination thereof.
[0060] In some embodiments, the lithium chloride solution can be obtained from lithium carbonate. In some examples, the lithium carbonate can be produced by the lithium carbonate production method described herein.
[0061] In some examples, lithium carbonate (Li2CO3) reacts to form lithium chloride (LiCl) as follows:
[0062] Li2CO3(s)+2HCl(aq)→2LiCl(aq)+CO2(g)+H2O(l)
[0063] In some embodiments utilizing the above reaction, hydrochloric acid (HCl) can be obtained from the electrolysis described herein. In some embodiments of the above reaction, carbon dioxide (CO2) can be captured (e.g., using a scrubber) to be reused as a carbon dioxide source (i.e., a carbon dioxide source for producing lithium carbonate) as described herein. The captured CO2 can also be used for other purposes, such as, but not limited to, the production of potassium carbonate or the production of sodium carbonate or other applications.
[0064] In some examples, lithium carbonate (Li2CO3) reacts to form lithium chloride (LiCl) as follows:
[0065] 2Li2CO3(s)+2Cl2(g)→4LiCl(aq)+2CO2(g)+O2(g).
[0066] In some embodiments utilizing the above reaction, chlorine (Cl2) can be obtained from the electrolysis described herein. In some embodiments of the above reaction, the hydrogen produced by electrolysis can be used as an energy source. In some embodiments of the above reaction, carbon dioxide (CO2) can be collected as described above. In some examples, the above reaction can be carried out using the catalyst described below, such as Kim et al., "Manufacture characteristics of metal oxide-hydroxidesfor the catalytic decomposition of a sodium hypochlorite solution", Chemical Engineering Journal, Vol. 200-202, 2012, described in pp. 52-58, which is incorporated herein by reference in its entirety for all purposes.
[0067] In some examples, the reaction of lithium chloride with potassium hydroxide (KOH) may include performing the following reaction:
[0068]
[0069] In some embodiments, lithium chloride and potassium hydroxide are reacted in a stoichiometric manner. As used herein, "stoichiometric" means that lithium chloride and potassium hydroxide are combined in a molar ratio of 1:1. In some examples, non-stoichiometric molar ratios of lithium chloride to potassium hydroxide may also be used, such as but not limited to 1:2, 2:1, 1:3, 3:1, 4:1, 1:4... However, as discussed in more detail below, in some embodiments, the use of non-stoichiometric molar ratios may affect the reaction yield.
[0070] In some examples, a potassium hydroxide solution is reacted with a lithium chloride solution to produce a reciprocal salt system. In some examples, the reciprocal salt system comprises, consists of, or consists essentially of potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide, and water. As used herein, a "reciprocal salt system" is a salt system according to et al., “Glossary of terms related to solubility (IUPAC Recommendations 2008)” Pure and Applied Chemistry, Vol. 80, No. 2, 2008, pp. 233-276, which is incorporated herein by reference in its entirety for all purposes.
[0071] use et al., an exemplary reciprocal salt system of the present disclosure can be defined as follows:
[0072] K + ,Li + ||Cl – ,OH – +H2O
[0073] Another exemplary reciprocal salt system of the present disclosure can be defined as follows:
[0074] K + ,Li + ||NO3 – ,OH – +H2O
[0075] Another exemplary reciprocal salt system of the present disclosure can be defined as follows:
[0076] K + ,Li + ||NO 3– ,Cl – ,OH – +H2O
[0077] A more comprehensive definition of "reciprocal salt system" is provided in "AQUEOUS SOLUTION AND THE PHASE DIAGRAM" by Frederick Field Purdon and Victor Wallace Slater (1946), which is hereby incorporated by reference in its entirety for all purposes. According to this definition, a reciprocal salt system consists of two salts and water, wherein the two salts do not share the same ion. These salts produce two new salts, which are called double decomposition interactions, thereby forming a reciprocal salt pair. A reciprocal salt system can be illustrated by a square-bottomed pyramid, with water at the top and four salts at the four corners. This layout emphasizes the reciprocal relationship between salt pairs. The reaction in a reciprocal salt system must reach a state of equilibrium, where the rates of the forward and reverse reactions are equal. Therefore, a reciprocal salt system cannot exist without an irreversible reaction that reaches equilibrium. Irreversible non-equilibrium reactions are incompatible with the reciprocal behavior of salts, which, according to the definition of double decomposition reactions, must be stable in an equilibrium state, with all ions in a soluble state--unreacted or precipitated--to make the system exist as defined.
[0078] Some embodiments include: precipitating potassium chloride and lithium hydroxide from a reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals. In some instances, the reaction and precipitation are performed simultaneously, sequentially, or in combination. In some instances, the reaction and precipitation steps are performed in a single device, a crystallization reactor. In some instances, precipitation is performed when the reciprocal salt system is in equilibrium. In some instances, the equilibrium can be a chemical equilibrium, a phase equilibrium, or any combination thereof. In some instances, the reaction and precipitation steps are performed in separate devices. For example, the reaction can be performed in at least one reactor (described below), and the precipitation can be performed using at least one crystallizer (described below).
[0079] In some examples, the reaction, precipitation, or any combination thereof can be performed at ambient pressure at a temperature range of -50°C to 150°C, -25°C to 150°C, 0°C to 150°C, 25°C to 150°C, 50°C to 150°C, 75°C to 150°C, 100°C to 150°C, 125°C to 150°C, -50°C to 125°C, -50°C to 100°C, -50°C to 75°C, -50°C to 50°C, -50°C to 50°C, -50°C to 25°C, -50°C to 0°C, -50°C to -25°C, -25°C to 125°C, 0°C to 100°C, 25°C to 75°C, or any combination thereof. The reaction, precipitation, or any combination thereof can also be performed at ambient pressure, below ambient pressure (e.g., by using at least one vacuum source), or at a pressure above ambient pressure (e.g., using a pressurized reactor). Therefore, some embodiments of the present disclosure may contemplate varying operating temperatures at pressures other than ambient pressure.
[0080] In some embodiments, the reciprocal salt system includes potassium chloride in an amount of 5 wt% to 30 wt%, 10 wt% to 30 wt%, 15 wt% to 30 wt%, 20 wt% to 30 wt%, 25 wt% to 30 wt%, 5 wt% to 25 wt%, 5 wt% to 20 wt%, 5 wt% to 15 wt%, 5 wt% to 10 wt%, 10 wt% to 25 wt%, 15 wt% to 20 wt%, or any combination thereof, based on the total weight of the reciprocal salt system. In some embodiments, the reciprocal salt system includes lithium hydroxide in an amount of 1 wt% to 10 wt%, 2 wt% to 10 wt%, 5 wt% to 10 wt%, 7 wt% to 10 wt%, 9 wt% to 10 wt%, 1 wt% to 9 wt%, 1 wt% to 7 wt%, 1 wt% to 5 wt%, 1 wt% to 2 wt%, 2 wt% to 9 wt%, 5 wt% to 7 wt%, or any combination thereof, based on the total weight of the reciprocal salt system. In some embodiments, the reciprocal salt system includes water in an amount of 60 wt% to 90 wt%, 70 wt% to 90 wt%, 80 wt% to 90 wt%, 60 wt% to 80 wt%, 60 wt% to 70 wt%, 70 wt% to 80 wt%, or any combination thereof, based on the total weight of the reciprocal salt system.
[0081] In some examples, precipitating potassium chloride and lithium hydroxide from the reciprocal salt system includes: a cooling stage. In some examples, the cooling stage can be carried out at ambient pressure at a temperature range of -50°C to 50°C, -50°C to 25°C, -50°C to 0°C, -50°C to -25°C, -25°C to 50°C, 0°C to 50°C, 25°C to 50°C, -25°C to 25°C, or any combination thereof. It should be understood that the temperature can be varied at other pressures mentioned above.
[0082] In some examples, the cooling stage selectively crystallizes potassium chloride crystals. As used herein, "selectivity" means that the amount of one component in a solution increases while the amount of another component decreases or remains unchanged. For example, in the case of "selective crystallization" of potassium chloride crystals, the amount of lithium hydroxide crystals may decrease or remain unchanged.
[0083] In some examples, during the cooling stage, the proportion of potassium chloride in the crystalline phase increases. In some embodiments, during the cooling stage, the weight fraction (g / g) of potassium chloride in the crystalline phase relative to the total weight of the reciprocal salt system is: 0.1 to 0.4, 0.2 to 0.4, 0.3 to 0.4, 0.1 to 0.3, 0.1 to 0.2, 0.2 to 0.3 or any combination thereof.
[0084] In some examples, precipitating potassium chloride and lithium hydroxide includes: an evaporation heating stage. In some examples, the temperature of the evaporation heating stage at ambient pressure can be: 25°C to 150°C, 50°C to 150°C, 75°C to 150°C, 100°C to 150°C, 125°C to 150°C, 25°C to 125°C, 25°C to 100°C, 25°C to 75°C, 25°C to 50°C, 50°C to 125°C, 75°C to 105°C, or any combination thereof, it being understood that the temperature can be varied at other pressures as mentioned above.
[0085] In some embodiments, the evaporation heating stage selectively precipitates lithium hydroxide crystals. During the "selective precipitation" of lithium hydroxide crystals, the amount of potassium chloride crystals decreases or remains unchanged.
[0086] In some examples, during the evaporation heating stage, the proportion of lithium hydroxide in the crystalline phase increases. In some embodiments, during the evaporation heating stage, the weight fraction (g / g) of lithium hydroxide in the crystalline phase relative to the total weight of the reciprocal salt system is: 0.03 to 0.09, 0.05 to 0.09, 0.07 to 0.09, 0.03 to 0.07, 0.03 to 0.05, 0.05 to 0.07, or any combination thereof.
[0087] Some examples also include: purifying lithium hydroxide crystals. Some examples of purifying lithium hydroxide crystals also include: separating lithium hydroxide crystals from a reciprocal salt system. Some examples of purifying lithium hydroxide crystals also include: dissolving lithium hydroxide crystals in water or brine to form a lithium hydroxide solution. Some examples of purifying lithium hydroxide crystals also include: separating insoluble solids from the lithium hydroxide solution. Some examples of purifying lithium hydroxide crystals also include: evaporating water from the lithium hydroxide solution to recrystallize the lithium hydroxide crystals. In some examples, dissolving, separating and evaporating are repeated until a target purity is reached. In some examples, the target purity is greater than 50 wt% lithium hydroxide, lithium hydroxide monohydrate, or a combination thereof based on the total weight of the lithium hydroxide crystals. In some examples, the target purity is greater than 90 wt% lithium hydroxide, lithium hydroxide monohydrate, or a combination thereof based on the total weight of the lithium hydroxide crystals. In some examples, the target purity is greater than 95 wt% lithium hydroxide, lithium hydroxide monohydrate, or a combination thereof based on the total weight of the lithium hydroxide crystals. In some examples, the target purity is greater than 99 wt% lithium hydroxide, lithium hydroxide monohydrate, or a combination thereof, based on the total weight of the lithium hydroxide crystals. In some examples, the target purity is greater than 99.5 wt% lithium hydroxide, lithium hydroxide monohydrate, or a combination thereof, based on the total weight of the lithium hydroxide crystals. In some examples, the target purity is greater than 99.9 wt% lithium hydroxide, lithium hydroxide monohydrate, or a combination thereof, based on the total weight of the lithium hydroxide crystals. In some examples, the target purity is greater than 99.9 wt% lithium hydroxide, lithium hydroxide monohydrate, or a combination thereof, based on the total weight of the lithium hydroxide crystals. In some examples, the target purity is 50 wt% to 99.9 wt%, 90 wt% to 99.9 wt%, 95 wt% to 99.9 wt%, 99 wt% to 99.9 wt%, 50 wt% to 99 wt%, 50 wt% to 95 wt%, 50 wt% to 90 wt%, or any combination thereof, based on the total weight of the lithium hydroxide crystals.
[0088] Some examples also include: separating lithium hydroxide crystals, potassium chloride crystals, or a combination thereof from a reciprocal salt system. Suitable separators may be used for separation, examples of which are described in further detail below. In some examples, separation is performed using filtration, centrifugation, or any combination thereof. Some embodiments may include: separating a majority (i.e., >50%) of lithium hydroxide crystals, potassium chloride crystals, or a combination thereof from a reciprocal salt system. Some embodiments may include: separating all or substantially all (i.e., ≥99%) of lithium hydroxide crystals, potassium chloride crystals, or a combination thereof from a reciprocal salt system.
[0089] Some examples of the method also include: dissolving the potassium chloride crystals removed from the reciprocal salt solution in water, brine or lean potassium chloride solution, and filtering the resulting mixture to recover the potassium chloride solution. In some instances, the pH of the potassium chloride solution can be adjusted using hydrochloric acid produced in the above manner. In addition, as described above, in some embodiments, the potassium chloride solution recovered can be recovered and reused in at least one electrolyzer. Therefore, in some instances, the dissolution, electrolysis, reaction and precipitation steps can be repeated once or any times. In addition, in some embodiments, the recovered potassium chloride solution can be connected to the electrolyzer fluid, for example, by at least one recovery stream. In other embodiments, the recovered potassium chloride solution can be added to the electrolyzer in batches or by any other fluid arrangement known in the art.
[0090] Some embodiments of the present disclosure describe methods for producing lithium carbonate. In some examples, lithium carbonate can be produced using lithium chloride, potassium chloride or sodium chloride, water and a carbon dioxide source as reagents. In some aspects, lithium carbonate can be produced without using lime, soda ash, hydrochloric acid, sodium hydroxide or a combination thereof as reagents.
[0091] As described above, one or more embodiments of the method for producing lithium carbonate include: electrolyzing potassium chloride or sodium chloride solution. In the example of using sodium chloride solution, sodium chloride can replace potassium chloride in a specific electrolysis step. In some examples, when sodium chloride is used, it can be based on the above Product Bulletin causes deviation in electrolysis conditions.
[0092] In some instances, the electrolysis produces potassium hydroxide or sodium hydroxide solution, waste potassium chloride or lean sodium chloride solution, chlorine and hydrogen. In some instances, as described above, chlorine and hydrogen can react to form hydrochloric acid. The hydrochloric acid can be used as a pH adjusting agent, as further described above and below.
[0093] One or more embodiments of the method include: reacting a potassium hydroxide or sodium hydroxide solution with a carbon dioxide source to form a potassium carbonate solution or a sodium carbonate solution. The reaction may include at least one of the following reactions:
[0094] (1)2KOH(aq)+2CO2(g)→K2CO3(aq)+H2O(aq).
[0095] (2)2NaOH(aq)+2CO2(g)→Na2CO3(aq)+H2O(aq).
[0096] In some cases, the carbon dioxide source can be carbon dioxide gas (CO2). In some embodiments, carbon dioxide gas can be obtained from air, power generation, or any other means known in the art. In some examples, carbon dioxide gas can be obtained from the above-mentioned reaction to form a lithium chloride solution.
[0097] In some embodiments, the carbon dioxide source can be a chemical element or compound that reacts to form CO2. For example, in a particular embodiment, the carbon dioxide source can include: alkali metal bicarbonate (hereinafter referred to as MHCO3) and acetic acid. In some embodiments, the alkali metal M can be sodium or potassium. Alkali metal bicarbonate (MHCO3) and acetic acid (CH3COOH) can react to form CO2 and alkali metal acetate (MCH3COO) according to the following reaction:
[0098] MHCO3(aq)+CH3COOH(l)→CO2(g)+H2O(l)+MCH3COO(aq).
[0099] In some embodiments, the method comprises: reacting a potassium carbonate solution or a sodium carbonate solution with a lithium chloride solution. In some embodiments, the reaction is carried out with a reaction mixture comprising potassium carbonate or sodium carbonate and lithium chloride.
[0100] In some examples, the reaction includes at least one of the following reactions:
[0101] (1)K2CO3(aq)+2LiCl(aq)→Li2CO3(s)+2KCl(aq).
[0102] (2)Na2CO3(aq)+2LiCl(aq)→Li2CO3(s)+2NaCl(aq).
[0103] In some examples, the reaction of potassium carbonate and lithium chloride is carried out by heating the reaction mixture to a temperature sufficient to react potassium carbonate or sodium carbonate with lithium chloride. In some examples, the temperature is increased to: 30°C to 120°C, 40°C to 120°C, 50°C to 120°C, 60°C to 120°C, 70°C to 120°C, 80°C to 120°C, 90°C to 120°C, 100°C to 120°C, 110°C to 120°C, 30°C to 110°C, 30°C to 100°C, 30°C to 90°C, 30°C to 80°C, 30°C to 70°C, 30°C to 60°C, 30°C to 50°C, 30°C to 40°C, 40°C to 110°C, 50°C to 100°C, 60°C to 90°C, 70°C to 80°C, or any combination thereof.
[0104] In some embodiments, the product mixture produced by the reaction includes: potassium chloride or sodium chloride, and lithium carbonate solids. Some embodiments include: removing lithium carbonate solids from the product mixture. In some embodiments, removing at least some lithium carbonate solids from the product mixture. In some embodiments, removing most (>50%) of the lithium carbonate solids from the product mixture. In some embodiments, removing all or substantially all (≥99%) of the lithium carbonate solids from the product mixture. Removal can be performed using at least one suitable separator described herein.
[0105] In some examples, removal of the lithium carbonate solids produces a regenerated potassium chloride solution or a regenerated sodium chloride solution.
[0106] Some embodiments include: combining the regenerated potassium chloride solution or the regenerated sodium chloride solution with the lean potassium chloride solution or the lean sodium chloride solution to replenish the potassium chloride solution or the sodium chloride solution. Thus, in some examples, the electrolysis, reaction, removal, and combining steps may be repeated once or any number of times. For example, the potassium chloride solution or the sodium chloride solution may be regenerated using at least one recycled stream as described herein.
[0107] Some examples also include: adjusting the pH of potassium chloride solution, regenerated potassium chloride solution, sodium chloride solution or regenerated sodium chloride solution. In some embodiments, the pH can be adjusted using hydrochloric acid as described above (e.g., hydrochloric acid obtained by reacting hydrogen and chlorine). In some examples, the pH of potassium chloride solution or sodium chloride solution is adjusted to: 2 to 8, 5 to 8, 6 to 8, 7 to 8, 4 to 7, 4 to 6, 4 to 5, 5 to 7 or any combination thereof.
[0108] Some embodiments relate to a method of making lithium hydroxide using lithium nitrate as a reagent to replace or supplement lithium chloride. In some embodiments, lithium nitrate can be used as a standalone reagent without lithium chloride. In some embodiments, a mixture of lithium chloride and lithium nitrate can be used.
[0109] In some embodiments, lithium nitrate, lithium chloride, or a combination thereof can be produced by reacting lithium sulfate with calcium chloride, calcium nitrate, or a combination thereof. The reaction produces a solution of lithium chloride, lithium nitrate, or a combination thereof, which can then be used in the manufacturing method described in the present disclosure. The reaction can further produce a calcium sulfate precipitate.
[0110] Thus, some embodiments may include the step of precipitating calcium sulfate crystals from a lithium nitrate solution, a lithium chloride solution, or a combination thereof. The method of precipitating calcium sulfate crystals may occur over a wide temperature range of -10°C to 110°C. This overall range may encompass a number of sub-ranges including, but not limited to -5°C to 105°C, 0°C to 100°C, 5°C to 95°C, 10°C to 90°C, 15°C to 85°C, 20°C to 80°C, 25°C to 75°C, 30°C to 70°C, 35°C to 65°C, 40°C to 60°C, 45°C to 55°C, or any combination thereof.
[0111] Lithium sulfate can be obtained from a variety of sources. In some cases, the lithium sulfate solution can be produced by a reaction involving spodumene and sulfuric acid, as detailed in U.S. Patent No. 11,083,978, which is incorporated herein by reference in its entirety. In other cases, the lithium sulfate solution can come from battery waste, black matter, or other lithium-rich waste, as outlined in U.S. Patent Application No. 2021 / 0079495 and U.S. Patent Application No. 2020 / 0331002, each of which is incorporated herein by reference in its entirety. In some embodiments, the lithium sulfate solution can be obtained from brine.
[0112] In some embodiments, lithium nitrate can also be obtained by leaching black matter, battery waste or other lithium-containing waste using nitric acid, as outlined in U.S. Patent Application No. 2021 / 0079495 and U.S. Patent Application No. 2020 / 0331002, each of which is incorporated herein by reference in its entirety. In other embodiments, spodumene can be leached to form lithium nitrate using the nitric acid leaching method described in U.S. Patent No. 10,131,968, which is incorporated herein by reference in its entirety.
[0113] In some embodiments, lithium chloride may be obtained by leaching spodumene with hydrochloric acid as described in U.S. Patent No. 10,167,531, which is incorporated herein by reference in its entirety.
[0114] In some cases, the above-mentioned reciprocal salt system is formed by reacting potassium hydroxide with lithium chloride, lithium nitrate or any combination thereof. In these embodiments, the reciprocal salt system may include potassium hydroxide, lithium chloride and / or lithium nitrate, potassium chloride and / or potassium nitrate, lithium hydroxide and water. From the reciprocal salt system, lithium hydroxide and potassium chloride and / or potassium nitrate may be precipitated to form respective crystals.
[0115] In some embodiments, lithium hydroxide crystals or lithium hydroxide solution can be reacted with carbon dioxide to produce lithium carbonate solids, as described in detail in U.S. Patent Application Publication No. 2018 / 0320247, which is incorporated herein by reference in its entirety. Carbon dioxide-induced conversion of lithium hydroxide to lithium carbonate solids can provide an alternative or additional step to supplement the methods for producing lithium carbonate discussed elsewhere in this disclosure.
[0116] For some embodiments, a method of precipitating potassium chloride, potassium nitrate, or a combination thereof, and lithium hydroxide from a reciprocal salt system to produce lithium hydroxide crystals and potassium chloride crystals, potassium nitrate crystals, or any combination thereof is outlined. Precipitation of these crystals can include a cooling stage to selectively form potassium chloride and / or potassium nitrate crystals, and an evaporative heating stage to selectively precipitate lithium hydroxide crystals.
[0117] Figure 1 A first example of a lithium production system 100 according to aspects of the present disclosure is shown.
[0118] In the present disclosure, the lithium production system 100 can be used to produce lithium hydroxide (including lithium hydroxide monohydrate), lithium carbonate, or any combination thereof. The example shown includes: at least one electrolytic cell 105 and at least one reactor 110. The system 100 can be reference Figure 2 and Figure 3 Examples of the corresponding elements are described, or various aspects of the corresponding elements may be included.
[0119] In some embodiments, electrolytic cell 105 electrolyzes potassium chloride solution or sodium chloride solution to obtain: potassium hydroxide or sodium hydroxide solution, waste potassium chloride or sodium chloride solution, chlorine gas and hydrogen gas. In some examples, electrolytic cell 105 performs chlor-alkali electrolysis. In some examples, electrolytic cell 105 utilizes mercury cell technology. Electrolytic cell 105 can be a reference Figures 2 to 4 Examples of the corresponding elements are described, or various aspects of the corresponding elements may be included.
[0120] In some embodiments, at least one reactor 110 reacts potassium hydroxide solution with lithium chloride. In some examples, reactor 110 reacts hydrogen with chlorine to produce hydrochloric acid. In some examples, at least one reactor 110 includes at least one crystallization reactor 110. In some examples, reactor 110 can take the form of multiple reactors ( Figure 1In some embodiments, at least one reactor 110 reacts a potassium hydroxide solution or a sodium hydroxide solution with a carbon dioxide source to form a potassium carbonate solution or a sodium carbonate solution. In some examples, at least one reactor 110 reacts a potassium carbonate solution or a sodium carbonate solution with a lithium chloride solution to obtain a product mixture including potassium chloride or sodium chloride and lithium carbonate solids. In some examples, at least one reactor 110 is configured to react a sodium hydroxide solution or a potassium hydroxide solution with a carbon dioxide source to form a sodium carbonate solution or a potassium carbonate solution; and react a sodium carbonate solution or a potassium carbonate solution with a lithium chloride solution to obtain a product mixture including sodium chloride or potassium chloride and lithium carbonate solids. At least one reactor 110 may be a reference Figure 2 and Figure 3 Examples of the corresponding elements are described, or various aspects of the corresponding elements may be included.
[0121] Figure 2 A second example of a lithium production system 200 according to aspects of the present disclosure is shown. The example shown includes: at least one electrolytic cell 205, at least one reactor 210, and at least one crystallizer 215.
[0122] System 200 can be used as a reference Figure 1 and Figure 3 Examples of the corresponding elements are described, or various aspects of the corresponding elements may be included.
[0123] At least one electrolytic cell 205 may be a reference Figure 1 , Figure 3 and Figure 4 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. At least one reactor 210 may be a reference Figure 1 and Figure 3 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. The electrolytic cell 205 may electrolyze a potassium chloride solution or a sodium chloride solution to obtain a potassium hydroxide solution or a sodium hydroxide solution. Figure 2 In an example, the electrolysis cell 205 may include at least one membrane, and the electrolysis may be performed using membrane electrolysis, such as, but not limited to, chlor-alkali electrolysis.
[0124] In some embodiments, at least one crystallizer 215 is configured to precipitate potassium chloride and lithium hydroxide from the reciprocal salt system 200 to form lithium hydroxide crystals and potassium chloride crystals. In some examples, at least one crystallizer 215 can be a reference Figure 3Examples of the corresponding elements described, or aspects of the corresponding elements may be included. In some instances, at least one reactor 210 and at least one crystallizer 215 may be a single device, such as but not limited to a crystallization reactor. In some instances, at least one crystallizer 215 may be separated from at least one reactor 210. In these instances, at least one crystallizer 215 may take the form of multiple crystallizers in series or in parallel, such as but not limited to a multi-effect crystallizer column. In some embodiments, at least one crystallizer 215 may include a mechanical steam compressor crystallizer. In some instances, at least one crystallizer 215 may be thermally connected to an induction or convection heat source. An exemplary convection heat source is steam. An exemplary induction heat source is a heating coil. Other non-limiting examples of at least one crystallizer 215 include: mixed suspension mixed product removal (MSMPR) crystallizer, circulating liquid crystallizer, scraped surface crystallizer, tank crystallizer, forced circulation crystallizer, draft tube baffle (DTB) crystallizer or any combination thereof.
[0125] Figure 3 A third example of a lithium production system 300 according to aspects of the present disclosure is shown. The example shown includes: at least one electrolytic cell 305, at least one reactor 310, at least one crystallizer 315, at least one mixer 320, and at least one separator 325. The system 300 may be referenced Figure 1 and Figure 2 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. The electrolytic cell 305 may be a reference Figure 1 , Figure 2 and Figure 4 The reactor 310 may be an example of the corresponding element described in the embodiment of the present invention, or may include various aspects of the corresponding element. Figure 1 and Figure 2 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. The crystallizer 315 may be a reference Figure 2 Examples of the corresponding elements are described, or various aspects of the corresponding elements may be included.
[0126] In some examples, mixer 320 dissolves potassium chloride crystals or sodium chloride crystals in water, brine, poor potassium chloride solution or poor sodium chloride solution to obtain potassium chloride solution or sodium chloride solution. In some examples, mixer 320 dissolves lithium hydroxide crystals in water or brine to form lithium hydroxide solution. In some embodiments, mixer 320 merges regenerated potassium chloride solution with poor potassium chloride solution or poor sodium chloride solution to supplement potassium chloride solution or sodium chloride solution. In some examples, mixer 320 adjusts the pH of potassium chloride solution or sodium chloride solution. In some examples, mixer 320 can take the form of multiple mixers in series or in parallel. Non-limiting examples of mixer 320 include: vertical or horizontal stirring tank, high or low shear tube mixer, horizontal paddle mixer, screw conveying mixer, continuous high shear mixer, progressive cavity mixing pump or any combination thereof.
[0127] In some embodiments, the separator 325 separates lithium hydroxide crystals from the reciprocal salt system 300. In some examples, the separator 325 separates insoluble solids from the lithium hydroxide solution. In some examples, the separator 325 separates lithium hydroxide crystals, potassium chloride crystals, or a combination thereof from the reciprocal salt system 300. In some examples, the separator 325 uses filtration, centrifugation, or any combination thereof to separate lithium hydroxide crystals, potassium chloride crystals, or a combination thereof from the reciprocal salt system 300. In some examples, at least one separator 325 includes: a centrifuge, a filter, or a combination thereof. In some embodiments, the separator 325 separates lithium carbonate solids from the product mixture to obtain a regenerated potassium chloride solution or a regenerated sodium chloride solution. In some embodiments, the separator 325 includes: at least one separator 325, wherein the at least one separator 325 is configured to remove lithium carbonate solids from a product mixture of lithium carbonate and sodium chloride or potassium chloride. In some examples, the separator 325 includes a filter press, a belt filter, a plate filter, a sedimentation centrifuge, a filter centrifuge, or any combination thereof.
[0128] The lithium production system 300 may also include at least one heat source 330, at least one cooling source 335, at least one temperature sensor 340, at least one power source 345, at least one vacuum source 350, at least one recovery stream 355, at least one evaporator 360, or any combination thereof.
[0129] In some examples, the at least one heat source 330 includes a furnace, a boiler, a heat pump, a stove, an oven, a flange heater, a circulation heater, a screw plug heater, or any combination thereof.
[0130] In some examples, the at least one cooling source 335 includes a refrigerant, a cooling jacket, an evaporative cooler, a cooling tower, pumpable ice, or any combination thereof.
[0131] In some examples, the at least one temperature sensor 340 includes a thermocouple, a temperature monitoring controller, a resistance temperature detector, a thermistor, a semiconductor-based integrated circuit, or any combination thereof.
[0132] In some examples, at least one power source 345 includes: electricity, mechanical power, at least one fossil fuel, coal, nuclear power, hydrogen, at least one fuel cell, at least one nuclear fission reactor, at least one nuclear fusion reactor, or any combination thereof.
[0133] In some examples, at least one vacuum source 350 can be used to perform the reactions or precipitations described herein at a pressure below ambient pressure. In some examples, at least one vacuum source 350 includes a rotary vane pump, a diaphragm pump, a piston pump, a scroll pump, a screw pump, an eccentric rotary pump, or any combination thereof.
[0134] In some examples, at least one recovery stream 355 combines the regenerated potassium chloride solution with the lean potassium chloride solution to replenish the potassium chloride solution. In some examples, at least one recovery stream 355 combines the regenerated sodium chloride solution with the lean sodium chloride solution to replenish the sodium chloride solution. In some examples, at least one recovery stream 355 can reintroduce the recovered potassium chloride into the electrolytic cell 305.
[0135] In some examples, at least one evaporator 360 can evaporate water from the lithium hydroxide solution to recrystallize the lithium hydroxide crystals. In some examples, at least one evaporator 360 can include: a rising film evaporator, a short tube vertical evaporator, a basket evaporator, a long tube vertical evaporator, a plate evaporator, a horizontal shell and tube evaporator, a tank evaporator, a rotary drum evaporator, or any combination thereof.
[0136] Figure 4 An example of at least one electrolytic cell 400 according to aspects of the present disclosure is shown. The electrolytic cell 400 may be a reference Figures 1 to 3 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. In one embodiment, electrolytic cell 400 includes: chlorine gas 405, hydrogen gas 410, potassium chloride solution 415 or sodium chloride solution 420, potassium hydroxide solution 425 or sodium hydroxide solution 430, and membrane 435. Potassium chloride solution 415 may be reference Figure 7 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. Potassium hydroxide solution 425 may be a reference Figure 7 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. The film 435 may be a reference Figure 5 and Figure 6 Examples of the corresponding elements described herein, or may include aspects of the corresponding elements, or may be any membrane, such as but not limited to a perfluorinated sulfonated membrane as described herein (e.g., ).
[0137] Figure 5 An exemplary current efficiency of a membrane 500 that can be used in accordance with aspects of the present disclosure is shown. The membrane 500 can be a reference Figure 4 and Figure 6 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. Specifically, the current efficiencies shown are associated with membranes 500-a and 500-b. Membranes 500-a and 500-b are available from DuPont TM Purchased Membrane. Exemplary current efficiencies are obtained from Fluorinated Ionomers (Second Edition), Plastics Design Library 2011, pages 81-156, which is incorporated herein by reference in its entirety for all purposes (hereinafter referred to as "Fluorinated Ionomers"). As shown in the figure, different types of membranes and different concentrations of potassium hydroxide or sodium hydroxide affect the efficiency of membrane electrolysis.
[0138] Figure 6 600 according to various aspects of the present disclosure. Figure 4 and Figure 5 Examples of the corresponding elements are described, or various aspects of the corresponding elements may be included. Figure 6 For use at 90°C with 32 wt% KOH and 170 g / l to 200 g / l KCl, DuPont TM Purchased 600-a, 600-b, 600-c, 600-d, and 600-e at different current densities. The exemplary voltages were obtained with the above-mentioned Fluorinated Ionomers. As shown, different types of membranes and different concentrations of potassium hydroxide can affect the efficiency of membrane electrolysis. In some instances, the presence of sodium hydroxide (in a potassium hydroxide solution or as a sodium hydroxide solution) can affect the efficiency to a certain extent without departing from the scope of the present disclosure. Figure 6 Efficiency not shown.
[0139] Figure 7 An exemplary crystallization reactor 700 according to aspects of the present disclosure is shown. The crystallization reactor 700 may be a reference Fig.17 In one embodiment, the crystallization reactor 700 includes: a reciprocal salt system 705, water 710, lithium chloride 715, potassium hydroxide solution 720, lithium hydroxide solution 725, and potassium chloride solution 730. The reciprocal salt system 705 can be reference Fig.15Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. In some examples, the reciprocal salt system 705 may be represented as follows: K + ,Li + ||Cl - ,OH - +H2O. Potassium hydroxide solution 720 can be used as a reference Figure 4 Examples of the corresponding elements described herein, or aspects of the corresponding elements may be included. The potassium chloride solution 730 may be a reference Figure 4 Examples of the corresponding elements described, or aspects of the corresponding elements may be included. In some examples, the crystallization reactor 700 is: a continuous crystallization reactor, an intermittent crystallization reactor, a stirred barrel crystallization reactor, a tank crystallization reactor, a cooling crystallization reactor, a direct contact cooling crystallization reactor, a steam-heated evaporation crystallization reactor, a forced circulation evaporation crystallization reactor, a DTB crystallization reactor, a turbulent crystallization reactor, a fluidized bed stirred crystallization reactor, a multi-stage vacuum crystallization reactor or any combination thereof.
[0140] Figure 8 An example of a method for producing lithium hydroxide according to aspects of the present disclosure is shown. In some cases, the operations described herein consist of multiple sub-steps or are performed in conjunction with other operations. In operation 800, the system electrolyzes a potassium chloride solution to produce a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas. In some cases, the operations of this step refer to reference Figures 1 to 4 In operation 805, the system reacts the potassium hydroxide solution with the lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide and water. In some cases, the operation of this step refers to reference Figures 1 to 3 In operation 810, the system precipitates potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals. In some cases, the operation of this step refers to reference Figure 2 and Figure 3 The crystallizer described herein may be carried out by means of the crystallizer.
[0141] Fig. 9 An example of a method for producing lithium hydroxide according to aspects of the present disclosure is shown. In operation 900, the system electrolyzes a potassium chloride solution to produce a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas. In some cases, the operation of this step refers to reference Figures 1 to 4 In operation 905, the system reacts the potassium hydroxide solution with the lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide and water. In some cases, the operation of this step refers to reference Figures 1 to 3In operation 910, the system precipitates potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals. In some cases, the operation of this step refers to reference Figure 2 and Figure 3 In operation 915, the system dissolves the potassium chloride crystals in water, brine or a lean potassium chloride solution to obtain a potassium chloride solution. In some cases, the operation of this step refers to reference Figure 3 In operation 920, the system repeats the steps of electrolysis, reaction, precipitation, dissolution, and filtration. In some cases, the operation of this step refers to reference Figures 1 to 4 The electrolytic cell, or can be carried out by the electrolytic cell.
[0142] Fig.10 An example of a method for producing lithium hydroxide according to aspects of the present disclosure is shown. In some cases, the operations described herein consist of multiple sub-steps or are performed in conjunction with other operations. In operation 1000, the system electrolyzes a potassium chloride solution to produce a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas. In some cases, the operations of this step refer to reference Figures 1 to 4 In operation 1005, the system reacts the potassium hydroxide solution with the lithium chloride solution to form a reciprocal salt system including potassium hydroxide, lithium chloride, potassium chloride, lithium hydroxide and water. In some cases, the operation of this step refers to reference Figures 1 to 3 In operation 1010, the system precipitates potassium chloride and lithium hydroxide from the reciprocal salt system to form lithium hydroxide crystals and potassium chloride crystals. In some cases, the operation of this step refers to reference Figure 2 and Figure 3 In operation 1015, the system purifies the lithium hydroxide crystals. In some cases, the operation of this step refers to reference Figure 3 The mixer may be carried out by means of the mixer.
[0143] Fig.11 An example of a method for producing lithium carbonate from lithium chloride and potassium chloride according to various aspects of the present disclosure is shown. In operation 1100, the system electrolyzes a potassium chloride solution to produce a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas. In some cases, the operation of this step refers to reference Figures 1 to 4 In operation 1105, the system reacts the potassium hydroxide solution with the carbon dioxide source to form a potassium carbonate solution. In some cases, the operation of this step refers to reference Figures 1 to 3In operation 1110, the system reacts the potassium carbonate solution with the lithium chloride solution to obtain a product mixture including potassium chloride and lithium carbonate solids. In some cases, the operation of this step refers to reference Figures 1 to 3 The reactor described above may be carried out by passing through the reactor.
[0144] Fig.12 An example of a method for producing lithium carbonate according to various aspects of the present disclosure is shown. In operation 1200, the system electrolyzes a potassium chloride solution to produce a potassium hydroxide solution, a lean potassium chloride solution, chlorine gas, and hydrogen gas. In some cases, the operation of this step refers to reference Figures 1 to 4 In operation 1205, the system reacts the potassium hydroxide solution with the carbon dioxide source to form a potassium carbonate solution. In some cases, the operation of this step refers to reference Figures 1 to 3 In operation 1210, the system reacts the potassium carbonate solution with the lithium chloride solution to obtain a product mixture including potassium chloride and lithium carbonate solids. In some cases, the operation of this step refers to reference Figures 1 to 3 In operation 1215, the system removes lithium carbonate solids from the mixture to form a regenerated potassium chloride solution. In some cases, the operation of this step refers to reference Figure 3 In operation 1220, the system combines the regenerated potassium chloride solution with the lean potassium chloride solution to replenish the potassium chloride solution. In some cases, the operation of this step refers to reference Figure 3 The mixer described above may be used to perform the above steps. In operation 1225, the system repeats the steps of electrolysis, reaction, removal, and merging.
[0145] Fig.13 An example of a method for producing lithium carbonate according to aspects of the present disclosure is shown. In operation 1300, the system electrolyzes a sodium chloride solution to produce a sodium hydroxide solution, a lean sodium chloride solution, chlorine gas, and hydrogen gas. In some cases, the operation of this step refers to reference Figures 1 to 4 In operation 1305, the system reacts the sodium hydroxide solution with the carbon dioxide source to form a sodium carbonate solution. In some cases, the operation of this step refers to reference Figures 1 to 3 In operation 1310, the system reacts the sodium carbonate solution with the sodium chloride solution to obtain a product mixture including sodium chloride and lithium carbonate solids. In some cases, the operation of this step refers to reference Figures 1 to 3 The reactor described above may be carried out by passing through the reactor.
[0146] Fig.14 An example of a method for producing lithium carbonate according to aspects of the present disclosure is shown. In operation 1400, the system electrolyzes a sodium chloride solution to produce a sodium hydroxide solution, a lean sodium chloride solution, chlorine gas, and hydrogen gas. In some cases, the operation of this step refers to reference Figures 1 to 4 In operation 1405, the system reacts the sodium hydroxide solution with the carbon dioxide source to form a sodium carbonate solution. In some cases, the operation of this step refers to reference Figures 1 to 3 In operation 1410, the system reacts the sodium carbonate solution with the sodium chloride solution to obtain a product mixture including potassium chloride and lithium carbonate solids. In some cases, the operation of this step refers to reference Figures 1 to 3 In operation 1415, the system removes lithium carbonate solids from the mixture to form a regenerated sodium chloride solution. In some cases, the operation of this step refers to reference Figure 3 In operation 1420, the system combines the regenerated sodium chloride solution with the lean sodium chloride solution to replenish the sodium chloride solution. In some cases, the operation of this step refers to reference Figure 3 The mixer described above may be used to perform the above steps. In operation 1425, the system repeats the steps of electrolysis, reaction, removal, and merging.
[0147] Fig.15 1 shows exemplary temperature and weight percentage data for a reciprocal salt system 1500 according to aspects of the present disclosure. The reciprocal salt system 1500 may be a reference Figure 7 Examples of corresponding elements described herein, or aspects of the corresponding elements may be included. These lines represent eutectic saturation points of lithium hydroxide and potassium chloride at different temperatures. These lines are generated using values in the disclosed scientific literature. In some instances (e.g., Example 3 below), this figure can be used to guide the selective precipitation of lithium hydroxide and potassium chloride in the present disclosure.
[0148] Fig.16 An exemplary reciprocal salt system according to aspects of the present disclosure is shown. picture. The diagrams are defined as in Beyond Discovery, available at https: / / www.beyonddiscovery.org / crystal-growth / 473-janecke-diagrams.html, last accessed on July 23, 2021. At least the foregoing portion of the Beyond Discovery website is incorporated herein by reference in its entirety for all purposes.
[0149] In the exemplary In Figure 1600, the corresponding reciprocal salt system can be represented as: K + ,Li + ||Cl – ,OH – +H2O. In the example In graph 1600, the molar ratios K / (K+Li) and Cl / (Cl+OH) are plotted. In graph 1600, lithium chloride (LiCl) and potassium hydroxide (KOH) are very soluble and do not precipitate in large amounts. In graph 1600, the highest yield is obtained using a stoichiometric mixture (M1) of lithium chloride (LiCl) and potassium chloride (KCl). A can be used, but the yield may not be as high.
[0150] As shown, mixture M1 can be cooled to 0°C (C1). During the cooling process, a solution C1 of molar composition can be formed. KCl can be separated, and solution C1 can be evaporated until point E1 at 100°C, at which point LiOH will crystallize according to some embodiments. The crystals can be separated. In some embodiments, solution E1 can be mixed with M1. The resulting mixture (at a point between E1 and M1) can then be cooled to C1 to form KCl. In some embodiments, evaporation, crystallization, separation and mixing can be repeated.
[0151] Non-limiting Example 1: Production of lithium hydroxide:
[0152] A lithium chloride solution having a lithium chloride concentration of 10 wt % to 50 wt % based on the weight of the lithium chloride solution is mixed with: (i) a potassium hydroxide solution having a potassium chloride concentration of 10 wt % to 40 wt % based on the weight of the solution; and (ii) a recovered potassium hydroxide solution. The resulting mixture is added to a crystallization reactor to obtain a reciprocal salt system. The reciprocal salt system is monitored to maintain the reciprocal salt system below the saturation point of lithium hydroxide (see, e.g. Fig.15 ).
[0153] The reciprocal salt system is cooled to selectively precipitate potassium chloride. The resulting potassium chloride crystals are separated using a centrifuge or a belt filter and dissolved in water or brine. Insoluble solids are filtered from the potassium chloride. The resulting solution is treated in an electrolytic cell to produce a lean potassium chloride solution, chlorine, potassium hydroxide solution and hydrogen, and to produce the recovered potassium hydroxide solution (ii) described above.
[0154] The reciprocal salt system is heated and the water is evaporated to selectively precipitate lithium hydroxide. The evaporative heating is performed until the solution is below the saturation point of potassium chloride, such as Fig.15 As shown. The crystallized lithium hydroxide monohydrate is then separated using a centrifuge. The solid lithium hydroxide monohydrate crystals are dissolved in water. The insoluble solids are then removed from the resulting lithium hydroxide solution using a polishing filter. The solution is evaporated until purified lithium hydroxide monohydrate crystals are formed. The lithium hydroxide monohydrate crystals are separated and washed using a centrifuge or a belt filter and are then dried and packaged.
[0155] Non-limiting Example 2: Production of lithium carbonate:
[0156] The potassium chloride or sodium chloride is treated in an electrolytic cell to form a lean potassium chloride solution or a lean sodium chloride solution, chlorine, hydrogen and a potassium hydroxide solution or a sodium hydroxide solution to obtain a potassium carbonate solution or a sodium carbonate solution.
[0157] The formed potassium hydroxide solution or sodium hydroxide solution is reacted with a carbon dioxide source to obtain potassium carbonate or sodium carbonate.
[0158] The lithium chloride solution is purified from the brine and reacted with a potassium carbonate or sodium carbonate solution at 60°C to 120°C to form a product mixture including lithium carbonate solid and potassium chloride or sodium chloride. The lithium carbonate solid is separated, washed, dried and collected.
[0159] The pH of the potassium chloride or sodium chloride solution is adjusted to remove dissolved carbonates. The potassium chloride solution or sodium chloride solution is then concentrated in an evaporator and combined with a lean potassium chloride solution or a lean sodium chloride solution to replenish the potassium chloride or sodium chloride solution.
[0160] Non-limiting Example 3: Relative solubility test of lithium hydroxide and potassium chloride:
[0161] Relative solubility testing was performed using the following experimental setup:
[0162] A three liter (3 L) glass-jacketed crystallizer reactor 1700 (eg Fig.17 As shown, at -9.8°C), it includes: a top mixer, an impeller and a baffle.
[0163] Connect to the heating and cooling system of the glass-jacketed crystallizer reactor 1700.
[0164] Thermocouples and temperature monitoring controllers.
[0165] Vacuum flasks, Buchner funnels and laboratory-scale centrifuges
[0166] Follow the following experimental procedures:
[0167] At a temperature exceeding 95° C., saturated solutions of LiOH and KCl were prepared with initial target weight percentages of 12 wt % and 32 wt %, respectively.
[0168] The saturated solution was kept at T>95°C for 1 hour and then cooled to 70°C, 40°C, 10°C and -10°C.
[0169] The saturated solution was maintained at each temperature for 1 hour and samples were taken according to the following procedure:
[0170] Solid and solution samples were collected at T>95°C, 40°C and -10°C (initial, intermediate, final) by dewatering using a lab-scale centrifuge and 28 μm filter media (polypropylene fabric).
[0171] The mass of filtrate and crystals collected was recorded.
[0172] Then samples were taken at 70°C and 10°C following the above procedure.
[0173] Fig.18 The results of the exemplary relative solubility test of the present embodiment are shown. The weight percentage shown corresponds to the weight percentage in the water phase (i.e., "in solution"). As shown, potassium chloride can be selectively precipitated at a relatively low temperature, as shown by the lower weight percentage of potassium chloride in the water phase at a relatively low temperature. On the contrary, lithium hydroxide can be selectively precipitated at a relatively high temperature, as shown by the lower weight percentage of lithium hydroxide in the water phase at the highest temperature.
[0174] Tables 1 and 2 below also show other results.
[0175] Table 1: Results of relative solubility tests
[0176]
[0177] Table 2: Results of relative solubility tests (continued)
[0178]
[0179] The above results indicate that in the present disclosure, lithium hydroxide and potassium chloride can be selectively precipitated from a reciprocal salt system.
[0180] Non-limiting Example 4: Simulated relative solubility test of lithium hydroxide and potassium nitrate:
[0181] Based on thermodynamic data, simulated relative solubility tests were performed on lithium hydroxide (LiOH) and potassium nitrate (KNO3) at different temperatures. The simulation used literature data to determine the thermodynamic values of each component, including ions and water, over a temperature range of 0°C to 90°C.
[0182] Fig.19 The simulation results are illustrated, showing the percentages of the components lithium hydroxide, potassium nitrate, lithium ions, potassium ions, nitrate ions, and water as a function of temperature.
[0183] The above results demonstrate that lithium hydroxide and potassium nitrate can be selectively precipitated from a reciprocal salt system according to the present disclosure.
[0184] The descriptions and drawings described herein represent exemplary configurations and do not represent all embodiments within the scope of the claims. For example, operations and steps may be rearranged, combined, or otherwise modified. In addition, structures and devices may be represented in the form of block diagrams to indicate the relationships between components and avoid confusion about the concepts being described. Similar components or features may have the same name but may be specifically labeled differently for different drawings.
[0185] Some modifications to the present disclosure may be apparent to those skilled in the art, and the principles defined herein may be applied to other variations without departing from the scope of the present disclosure. Therefore, the present disclosure is not limited to the examples and designs described herein, but is to conform to the broadest scope consistent with the principles and novel features disclosed herein. In addition to the benefits and improvements disclosed herein, other objects and advantages of the present disclosure will become apparent from the description in conjunction with the accompanying drawings. Detailed embodiments of the present disclosure are disclosed herein; however, it should be understood that the disclosed embodiments are merely illustrative of the present disclosure that may be implemented in various forms. In addition, each of the examples given with respect to the various embodiments of the present disclosure is intended to be illustrative rather than limiting.
[0186] In the present disclosure and the appended claims, the term "or" means including such a list, for example, a list of X, Y or Z means X, or Y, or Z, or XY, or XZ, or YZ or XYZ. The term "based on" is also not used to represent a closed set of conditions. For example, a step described as "based on condition A" can be based on condition A and condition B. In other words, the term "based on" should be interpreted as meaning "based at least in part on". Similarly, the words "a" or "an" mean "at least one".
[0187] Throughout the specification and claims, unless the context clearly states otherwise, the following terms adopt the meanings clearly associated with this article. The terms "in one embodiment", "in an embodiment" and "in some embodiments" used herein may, but do not necessarily refer to the same embodiment. In addition, the terms "in another embodiment" and "in some other embodiments" used herein may, but do not necessarily refer to different embodiments. All embodiments of the present disclosure can be combined without departing from the scope or principle of the present disclosure.
[0188] As used herein, unless the context clearly dictates otherwise, the term "based on" is not exclusive, but allows for being based on other factors not described. In addition, throughout the specification, the meanings of "a", "an", and "the" include plural references. The meaning of "in..." includes "in" and "on...".
[0189] All prior art patents, publications, and test methods cited herein are incorporated by reference in their entirety.
[0190] Changes, modifications and variations of the embodiments of the present disclosure described above will be apparent to those skilled in the art. All such changes, modifications, variations, etc. are intended to fall within the principles and scope of the present disclosure, which are limited only by the appended claims.
[0191] Any feature or element explicitly identified herein may also be specifically excluded as a feature or element of an embodiment of the present disclosure as defined in the claims.
[0192] As used herein, the term "consisting essentially of" limits the scope of a particular claim to the specified materials or steps and those materials or steps that do not materially affect the basic and novel features or characteristics of the particular claim.
[0193] The present disclosure described herein may be implemented in the absence of any element or elements, limitation or limitations not specifically disclosed herein. Thus, for example, in each instance herein, any of the terms "comprising," "consisting essentially of," and "consisting of" may be replaced with one of the other two terms. The terms and expressions used are used as descriptive terms rather than limiting terms, and the use of these terms and expressions is not intended to exclude any equivalents of the features shown and described or portions thereof, but it should be recognized that various modifications may be made within the scope of the present disclosure.
Claims
1. A method, include: The potassium hydroxide solution is reacted with a lithium chloride solution, a lithium nitrate solution, or any combination thereof to form a reciprocal salt system comprising: Potassium hydroxide, Lithium chloride, lithium nitrate or any combination thereof, Potassium chloride, potassium nitrate or any combination thereof; Lithium hydroxide; and Water; and The potassium chloride, the potassium nitrate or a combination thereof, and the lithium hydroxide are precipitated from the reciprocal salt system to form: Lithium hydroxide crystals, and Potassium chloride crystals, potassium nitrate crystals, or any combination thereof.
2. The method according to claim 1, further comprising: include: The lithium chloride solution, the lithium nitrate solution or the combination thereof is obtained by reacting calcium chloride, calcium nitrate or the combination thereof with a lithium sulfate solution.
3. The method according to claim 2, wherein the calcium chloride, the calcium nitrate or a combination thereof is reacted with a lithium sulfate solution. include: Calcium sulfate crystals are precipitated from the lithium chloride solution or the lithium nitrate solution.
4. The method according to claim 3, wherein the precipitating calcium sulfate crystals is carried out at a temperature of -10°C to 110°C.
5. The method of claim 2, wherein the lithium sulfate solution is produced by reacting spodumene with sulfuric acid.
6. The method according to claim 2, wherein the lithium sulfate solution is obtained from battery waste, black matter, other lithium-containing byproducts or waste.
7. The method of claim 2, wherein the lithium sulfate solution is obtained from brine.
8. The method according to claim 1, further comprising: include: The lithium nitrate solution is obtained by leaching black matter, battery waste, other lithium-containing byproducts or waste, or spodumene using nitric acid.
9. The method of claim 1, wherein the lithium hydroxide comprises lithium hydroxide monohydrate.
10. The method according to claim 1, further comprising: include: The lithium hydroxide crystals are purified.
11. The method according to claim 1, wherein the reacting and the precipitating are performed simultaneously, sequentially or in combination.
12. The method according to claim 1, further comprising: include: The lithium hydroxide crystals, the potassium chloride crystals, the potassium nitrate crystals, or any combination thereof are separated from the reciprocal salt system.
13. The method according to claim 1, further comprising: include: The lithium hydroxide crystals or the lithium hydroxide solution are reacted with carbon dioxide to form lithium carbonate solid.
14. The method according to claim 1, wherein the potassium chloride crystals or the potassium nitrate crystals and the lithium hydroxide crystals are precipitated from the reciprocal salt system. include: a cooling stage, wherein the cooling stage selectively crystallizes the potassium chloride crystals, the potassium nitrate crystals, or a combination thereof; and An evaporation heating stage, wherein the evaporation heating stage selectively precipitates the lithium hydroxide crystals.
15. A method, include: Potassium chloride or potassium nitrate and lithium hydroxide are precipitated from a reciprocal salt system to form: Lithium hydroxide crystals, and Potassium chloride crystals, potassium nitrate crystals, or any combination thereof.
16. The method of claim 15, wherein the reciprocal salt system is obtained by reacting a potassium hydroxide solution with a lithium chloride solution, a lithium nitrate solution, or any combination thereof.
17. A system, include: at least one reactor, wherein the at least one reactor is configured to react a potassium hydroxide solution with a lithium chloride solution, a lithium nitrate solution, or any combination thereof to form a reciprocal salt system comprising: Potassium hydroxide, Lithium chloride, lithium nitrate or any combination thereof, Potassium chloride, potassium nitrate or any combination thereof, lithium hydroxide; and Water; and at least one crystallizer, wherein the at least one crystallizer is configured to crystallize the potassium chloride, the potassium nitrate, or any combination thereof, and precipitate the lithium hydroxide from the reciprocal salt system to form: Lithium hydroxide crystals, and Potassium chloride crystals, potassium nitrate crystals, or any combination thereof.
18. The system of claim 17, further comprising at least one additional reactor.
19. The system of claim 18, wherein the at least one additional reactor is configured to react a lithium sulfate solution with a calcium chloride solution, a calcium nitrate solution, or any combination thereof to form the lithium chloride solution, the lithium nitrate solution, or any combination thereof, and calcium sulfate crystals.
20. The system of claim 18, wherein the at least one additional reactor is configured to leach the black material using nitric acid to form the lithium nitrate solution.
Citation Information
Cited By
Process for producing lithium hydroxide monohydrate
WO2026114726A1