Solid waste filling material based on fine-fraction gold tailings and preparation method of solid waste filling material
By using alkaline solid waste exciters and inorganic nanomaterials, the mechanical properties of fine-grain gold tailings solid waste gelling materials are improved, and the problems of low strength and high sinking of traditional filling materials are solved, thus achieving high Preparation of performance filling materials and environmentally friendly solid waste treatment.
Patent Information
- Application Number
- CN202411507899.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-28
AI Technical Summary
The treatment of fine-grain gold tailings has environmental pollution problems. Traditional gelling materials have low filling strength and high sinking, making it difficult to prepare high-performance filling materials.
The alkaline solid waste exciter and precursor materials are used as reinforcers, as well as inorganic nanomaterials, inorganic whiskers, triethanolamine and dopamine as reinforcers, and the mechanical properties of solid waste gelling materials are synergistically improved and high-performance solid waste filling materials are formed.
Improve the gelling performance and overall performance of solid waste materials, meet the P·O 52.5 cement standard, reduce production costs, and is suitable for filling of underground mine goafs with low glue ratio and low concentration, significantly improve compressive strength and Flexibility strength reduces the sinking rate.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic gelling materials, and in particular to a solid waste filling material based on fine-grained gold tailings and a preparation method thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Fine-grained gold tailings refer to the fine-grained tailings produced during the mining and processing of gold mines. These tailings are usually the "waste slag" discharged after the ore passes through the beneficiation plant to select valuable concentrates. Because these tailings particles are small, they are called fine-grained tailings.
[0004] The treatment of fine-grained gold tailings has always been a difficult problem in the mining industry. The traditional treatment method is to build a dedicated tailings pond for stacking; however, long-term stacking not only occupies a large amount of land, but also causes serious damage to the surrounding ecology. Gold tailings usually contain residual flotation agents and some heavy metal ions. These flotation agents and metal ions will enter farmland or groundwater with rainwater or tailings filtrate, causing huge pollution to the water bodies around the tailings pond; many harmful gases will be produced during the air-drying process of gold tailings, which will pollute the surrounding environment; and the fine-grained gold tailings after air-drying have a small particle size, and when encountering strong winds, they will be blown up to form air pollution. Therefore, it is particularly important to explore new methods for the treatment of fine-grained gold tailings.
[0005] At present, a method of using fine-grained gold tailings to prepare underground mine filling materials has been proposed and practiced. This method mixes fine-grained tailings with cementitious materials to prepare cementitious filling materials with higher strength for filling underground mines. This method can effectively treat fine-grained tailings and reduce the negative impact on the environment. However, when ordinary Portland cement is selected as a cementitious material and mixed with fine-grained tailings as a filling material, there are problems of low filling strength and high shrinkage. Therefore, preparing high-performance filling materials is the key to improving filling quality. Summary of the invention
[0006] In order to overcome the above problems, the present invention provides a solid waste filling material based on fine-grained gold tailings and a preparation method thereof.
[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions: The first aspect of the present invention provides a solid waste filling material based on fine-grained gold tailings, the raw materials of which include: Solid waste cementitious materials, fine-grained gold tailings, reinforcing agents and water; The solid waste gelling material includes alkaline solid waste activator and precursor material, the alkaline solid waste activator includes Bayer red mud, fluorgypsum and carbide slag; the precursor material includes slag, high-grade territorial water and waste glass powder; The reinforcing agent comprises inorganic nanomaterials, inorganic whiskers, triethanolamine and dopamine.
[0008] The second aspect of the present invention provides a method for preparing the solid waste filling material based on fine-grained gold tailings according to the first aspect, comprising: The solid waste cementitious material, fine-grained gold tailings, a reinforcing agent and water are mixed to obtain a solid waste filling material based on fine-grained gold tailings.
[0009] The beneficial effects of the present invention are: (1) The alkaline solid waste activator used in the present invention mainly comprises red mud and carbide slag to provide an alkaline environment for the precursor material, accelerate the disintegration of CaO, Al2O3 and other components in the glass powder of the precursor material, and form hydration products. Fluorogypsum in the alkaline solid waste activator provides sulfate ions, which will destroy the concentration balance of Ca²⁺ and Al³⁺ ions in the precursor material solution, and promote the hydration reaction to generate products such as calcium sulfate (AFt). In short, the synergistic effect of the alkaline environment and sulfate enables the activity of the precursor material to be fully exerted, improves the gelling properties and overall performance of the solid waste material, and provides strong support for the preparation of high-performance solid waste-based gelling materials. According to the indoor mortar test, the mechanical properties of the solid waste gelling material provided by the present invention meet the relevant standards of P·O 52.5 cement, and its 3-day compressive strength can reach 45.0 MPa, 3-day flexural strength can reach 7.0 MPa, 28-day compressive strength can reach 60.0 MPa, and 28-day flexural strength can reach 12.0 MPa.
[0010] (2) The inorganic nanomaterials, inorganic whiskers, triethanolamine and dopamine in the reinforcing agent of the present invention synergistically enhance the mechanical properties of the solid waste filling material based on fine-grained gold tailings. Specifically, the inorganic nanomaterials can fill the nano-scale voids in the matrix and improve the density of the overall filling material; the inorganic nanomaterials can serve as the attachment points of the hydration product CASH gel in the solid waste gelling material, thereby enabling the hydration reaction of the solid waste gelling material to proceed more effectively and improving the mechanical properties of the final solid waste gelling material; furthermore, the inorganic nanomaterials can participate in the hydration reaction of the solid waste gelling material to generate CASH gel. Dopamine can form a thin layer of reactive polymer composed of hydroxyl and amino groups on the surface of the inorganic whiskers, which can firmly adsorb the nanomaterials on the surface of the inorganic whiskers, thereby increasing the concentration of silicon ions in the pore solution of the filling material, promoting the formation of CASH gel, and thus improving the mechanical properties of the filling material. Triethanolamine molecules form a hydrophilic film on the surface of cement particles, reduce the surface tension of the solution, enhance the dispersibility and suspension stability of cementitious material particles in water, and not only promote the full contact between cement particles and water, but also accelerate the hydration reaction process of cement, thereby accelerating the formation of hydration products. In addition, triethanolamine also acts as a catalyst to further accelerate the coagulation and hardening process of cement, significantly enhancing the early strength of filling materials. Therefore, inorganic nanomaterials (nanoscopic), triethanolamine (nanoscopic), dopamine (nanoscopic) and inorganic whiskers (microscopic) achieve nano-microscopic synergistic enhancement.
[0011] (3) The present invention uses alkaline solid waste materials as active stimulants to synergistically stimulate a variety of bulk solid wastes to prepare solid waste cementitious materials, thereby eliminating the reliance on traditional high-energy cement. The solid waste cementitious materials prepared by the present invention are suitable for filling materials in underground mine goafs with low cement-solid ratio (cementitious material / fine-grained gold tailings) and low concentration (high water-cement ratio), which reduces production costs and promotes the full utilization of bulk solid wastes.
[0012] (4) The solid waste filling material based on fine-grained gold tailings provided by the present invention has a high strength grade in the early stage of curing and meets the requirements of JC / T 2478-2018 "Tailings Concrete for Filling Mine Goafs" for compressive strength (C2 grade), expansion (F1 grade) and shrinkage rate (S2 grade). DETAILED DESCRIPTION
[0013] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0014] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0015] A first typical embodiment of the present invention provides a solid waste filling material based on fine-grained gold tailings, the raw materials of which include: Solid waste cementitious materials, fine-grained gold tailings, reinforcing agents and water; The solid waste gelling material includes alkaline solid waste activator and precursor material, the alkaline solid waste activator includes Bayer red mud, fluorgypsum and carbide slag; the precursor material includes slag, high-grade territorial water and waste glass powder; The reinforcing agent comprises inorganic nanomaterials, inorganic whiskers, triethanolamine and dopamine.
[0016] In one or more embodiments, the mass ratio of the solid waste cementitious material to the fine-grained gold tailings is 1:(2-8).
[0017] In one or more embodiments, the mass ratio of the reinforcing agent to the solid waste gelling material is 1:(50-100).
[0018] In one or more embodiments, the mass ratio of water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the enhancer is 1:(1-4).
[0019] In one or more embodiments, in the solid waste gelling material, the mass ratio of the alkaline solid waste activator to the precursor material is 1:(4~20).
[0020] In one or more embodiments, in the alkaline solid waste activator, the mass ratio of Bayer process red mud, fluorgypsum and carbide slag is (5~8):(1~4):(1~3).
[0021] In one or more embodiments, in the precursor material, the mass ratio of slag, high-altitude land and waste glass powder is (5~7):(1~2):(1~4).
[0022] In one or more embodiments, in the reinforcing agent, the inorganic nanomaterial includes one or more of nano-silicon dioxide, nano-titanium dioxide or nano-aluminum oxide.
[0023] In one or more embodiments, in the reinforcing agent, the inorganic whiskers include one or more of calcium carbonate whiskers or calcium sulfate whiskers.
[0024] In one or more embodiments, in the enhancer, the mass ratio of the inorganic nanomaterial, the inorganic whisker, the triethanolamine and the dopamine is (2-5): (5-8): (1-3): (0.5-2).
[0025] In one or more embodiments, the fine-grained gold tailings have a particle size of less than 0.6 mm and a water content of less than 20%.
[0026] In one or more embodiments, in the alkaline solid waste activator, the pH value of Bayer process red mud leaching is 7~8.5.
[0027] In one or more embodiments, the CaSO4 mass fraction of fluorgypsum in the alkaline solid waste activator is higher than 85%.
[0028] In one or more embodiments, in the alkaline solid waste activator, the mass fraction of CaO in the carbide slag is higher than 75%.
[0029] In one or more embodiments, in the precursor material, the slag is S95 grade or above.
[0030] In one or more embodiments, in the precursor material, the total mass fraction of SiO2 and Al2O3 in the high-temperature region is greater than 95%.
[0031] In one or more embodiments, in the precursor material, the mass fraction of SiO2 in the waste glass powder is greater than 70%.
[0032] A second typical embodiment of the present invention provides a method for preparing the solid waste filling material based on fine-grained gold tailings according to the first aspect, comprising: The solid waste cementitious material, fine-grained gold tailings, a reinforcing agent and water are mixed to obtain a solid waste filling material based on fine-grained gold tailings.
[0033] In one or more embodiments, the solid waste cementitious material is dried and sealed and ground before being mixed with other materials.
[0034] Preferably, the drying temperature is 80-105°C, and the drying time is not less than 24 hours.
[0035] Preferably, the sealed grinding time is 10-30 min, the ball mill speed is 400-500 r / min; the specific surface area of the solid waste gelling material after sealed grinding is greater than 520 m 2 / kg.
[0036] In one or more embodiments, the reinforcing agent is subjected to a compound strengthening treatment before being mixed with other materials. The compound strengthening treatment method includes: placing the reinforcing agent in deionized water, stirring, filtering and drying to obtain a powdered reinforcing agent.
[0037] Preferably, the mass ratio of the enhancer to deionized water is 1:(45-55), preferably 1:50.
[0038] Preferably, the stirring time is 30 to 60 min.
[0039] Preferably, the drying temperature is 55-65° C., and the drying time is at least 24 hours.
[0040] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0041] The chemical compositions of the Bayer red mud, fluorgypsum, carbide slag, slag, tertiary ore and waste glass powder used in Examples 1 to 6 are shown in Table 1. In actual engineering applications, the pH values of red mud discharged from different factories are different, so the pH value of Bayer red mud leaching is limited to 7 to 8.5, and the pH value of Bayer red mud used in Examples 1 to 6 is 8.2.
[0042] Table 1 Chemical composition of Bayer red mud, fluorgypsum, carbide slag, slag, high-quality terroir and waste glass powder
[0043] The proportions of the raw materials in the solid waste filling materials based on fine-grained gold tailings in Examples 1 to 6 are shown in Table 2. Among them, the particle size of the fine-grained gold tailings in Examples 1 to 6 is 0.2 mm, and the water content is 18%.
[0044] Table 2 Proportions (mass ratio) of various raw materials in the solid waste filling materials based on fine-grained gold tailings in Examples 1 to 6
[0045] The composition ratios of the raw materials of the reinforcing agents used in Examples 1 to 6 are shown in Table 3.
[0046] Table 3 Composition ratio of each raw material based on the reinforcing agent used in Examples 1 to 6
[0047] Example 1 Preparation method of solid waste filling material based on fine-grained gold tailings: The Bayer red mud, fluorinated gypsum, carbide slag, slag, high-quality terrestrial waste and waste glass powder were dried at a temperature of 105°C for 36 hours. The dried Bayer red mud, fluorgypsum, carbide slag, slag, high-quality terroir and waste glass powder were weighed according to the formula ratio of Example 1 in Table 2, and placed in a ball mill for sealed grinding. The grinding time was 20 min and the ball mill speed was 400 r / min. The specific surface area was 550 m 2 / kg of solid waste cementitious materials; After weighing nano-silicon dioxide, calcium carbonate whiskers, triethanolamine and dopamine according to the formula ratio of Example 1 in Table 3, they were placed in deionized water (the mass ratio of the enhancer to the deionized water was 1:50) and magnetically stirred for 30 minutes, and then filtered and dried at 65° C. to obtain a powdered enhancer; The solid waste cementitious material, the reinforcing agent, the fine-grained gold tailings and water are mixed and stirred to obtain a solid waste filling material based on the fine-grained gold tailings, wherein the mass ratio of water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the reinforcing agent is 1:3.5.
[0048] Example 2 Preparation method of solid waste filling material based on fine-grained gold tailings: The Bayer red mud, fluorinated gypsum, carbide slag, slag, high-quality terroir and waste glass powder were dried at 80°C for 28 h. The dried Bayer red mud, fluorgypsum, carbide slag, slag, high-quality terroir and waste glass powder were weighed according to the formula ratio of Example 2 in Table 2, and placed in a ball mill for sealed grinding. The grinding time was 10 min and the ball mill speed was 500 r / min. The specific surface area was 530 m 2 / kg of solid waste cementitious materials; After weighing nano-silicon dioxide, calcium carbonate whiskers, triethanolamine and dopamine according to the formula ratio of Example 2 in Table 3, they were placed in deionized water (the mass ratio of the enhancer to the deionized water was 1:50) and magnetically stirred for 50 minutes, and then filtered and dried at 60° C. to obtain a powdered enhancer; The solid waste cementitious material, the reinforcing agent, the fine-grained gold tailings and water are mixed and stirred to obtain a solid waste filling material based on the fine-grained gold tailings, wherein the mass ratio of water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the reinforcing agent is 1:3.
[0049] Example 3 Preparation method of solid waste filling material based on fine-grained gold tailings: The Bayer red mud, fluorinated gypsum, carbide slag, slag, high-quality terroir and waste glass powder were dried at 85°C for 30 h. The dried Bayer red mud, fluorgypsum, carbide slag, slag, high-quality terroir and waste glass powder were weighed according to the formula ratio of Example 3 in Table 2, and placed in a ball mill for sealed grinding. The grinding time was 20 min and the ball mill speed was 420 r / min. The specific surface area was 580 m 2 / kg of solid waste cementitious materials; After weighing nano-silicon dioxide, calcium carbonate whiskers, triethanolamine and dopamine according to the formula ratio of Example 3 in Table 3, they were placed in deionized water (the mass ratio of the enhancer to the deionized water was 1:50) and magnetically stirred for 60 minutes, and then filtered and dried at 55° C. to obtain a powdered enhancer; The solid waste cementitious material, the reinforcing agent, the fine-grained gold tailings and water are mixed and stirred to obtain a solid waste filling material based on the fine-grained gold tailings, wherein the mass ratio of water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the reinforcing agent is 1:1.
[0050] Example 4 Preparation method of solid waste filling material based on fine-grained gold tailings: The Bayer red mud, fluorinated gypsum, carbide slag, slag, high-quality terroir and waste glass powder were dried at 95°C for 32 h. The dried Bayer red mud, fluorgypsum, carbide slag, slag, high-quality terroir and waste glass powder were weighed according to the formula ratio of Example 4 in Table 2, and placed in a ball mill for sealed grinding. The grinding time was 15 min and the ball mill speed was 450 r / min. The specific surface area was 550 m 2 / kg of solid waste cementitious materials; After weighing nano-silicon dioxide, calcium carbonate, triethanolamine and dopamine according to the formula ratio of Example 4 in Table 3, they were placed in deionized water (the mass ratio of the enhancer to the deionized water was 1:50) and magnetically stirred for 40 min, and then filtered and dried at 60° C. to obtain a powdered enhancer; The solid waste cementitious material, the reinforcing agent, the fine-grained gold tailings and water are mixed and stirred to obtain a solid waste filling material based on the fine-grained gold tailings, wherein the mass ratio of water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the reinforcing agent is 1:4.
[0051] Example 5 Preparation method of solid waste filling material based on fine-grained gold tailings: The Bayer red mud, fluorinated gypsum, carbide slag, slag, high-quality terrestrial waste and waste glass powder were dried at a temperature of 100°C for 30 hours. The dried Bayer red mud, fluorgypsum, carbide slag, slag, high-quality terroir and waste glass powder were weighed according to the formula ratio of Example 5 in Table 2, and placed in a ball mill for sealed grinding. The grinding time was 20 min and the ball mill speed was 500 r / min. The specific surface area was 550 m 2 / kg of solid waste cementitious materials; After weighing nano-silicon dioxide, calcium carbonate whiskers, triethanolamine and dopamine according to the formula ratio of Example 5 in Table 3, they were placed in deionized water (the mass ratio of the enhancer to the deionized water was 1:50) and magnetically stirred for 60 minutes, and then filtered and dried at 60° C. to obtain a powdered enhancer; The solid waste cementitious material, the reinforcing agent, the fine-grained gold tailings and water are mixed and stirred to obtain a solid waste filling material based on the fine-grained gold tailings, wherein the mass ratio of water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the reinforcing agent is 1:2.
[0052] Example 6 Preparation method of solid waste filling material based on fine-grained gold tailings: The Bayer red mud, fluorinated gypsum, carbide slag, slag, high-quality terrestrial waste and waste glass powder were dried at 80 °C for 25 h. The dried Bayer red mud, fluorgypsum, carbide slag, slag, high-quality terroir and waste glass powder were weighed according to the formula ratio of Example 6 in Table 2, and placed in a ball mill for sealed grinding. The grinding time was 18 min and the ball mill speed was 480 r / min. The specific surface area was 540 m 2 / kg of solid waste cementitious materials; After weighing nano-silicon dioxide, calcium carbonate whiskers, triethanolamine and dopamine according to the formula ratio of Example 6 in Table 3, they were placed in deionized water (the mass ratio of the enhancer to the deionized water was 1:50) and magnetically stirred for 30 minutes, and then filtered and dried at 60° C. to obtain a powdered enhancer; The solid waste cementitious material, the reinforcing agent, the fine-grained gold tailings and water are mixed and stirred to obtain a solid waste filling material based on the fine-grained gold tailings, wherein the mass ratio of water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the reinforcing agent is 1:2.5.
[0053] Comparative Example 1 The difference between Comparative Example 1 of the present invention and Example 1 is that the cementitious material used is ordinary Portland cement (P·O42.5 cement), and the solid waste cementitious material of the present invention is not used. Other methods and steps are the same as those of Example 1 and are not repeated here.
[0054] Comparative Example 2 The difference between Comparative Example 2 of the present invention and Example 1 is that the cementitious material used is commercial cement powder, and the solid waste cementitious material of the present invention is not used. Other methods and steps are the same as those in Example 1 and will not be repeated here.
[0055] Comparative Example 3 The difference between Comparative Example 3 of the present invention and Example 1 is that no enhancer is used, and other methods and steps are the same as those of Example 1, which will not be repeated here.
[0056] Performance Test: Referring to JC / T 2478-2018 "Tailings Concrete for Filling Mined-out Areas", the filling materials prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were tested for compressive strength, expansion and shrinkage, and the performance indicators are shown in Table 4 below.
[0057] Table 4 Performance test results of Examples 1 to 6 and Comparative Examples 1 to 3
[0058] It can be seen from Table 4 that, compared with Comparative Example 1, Comparative Example 2 and Comparative Example 3, when the solid waste filling material based on fine-grained gold tailings of the present invention is used for filling the goaf, the 7d and 28d compressive strengths of Examples 1 to 6 are greater than 1.20 MPa and 2.00 MPa, respectively, meeting the requirements for C2 strength grade tailings concrete in JC / T 2478-2018 "Tailings Concrete for Filling Goafs in Mines"; the 28 d shrinkage rate of Examples 1 to 6 is less than 6%, meeting the requirements for S2 shrinkage rate grade tailings concrete in JC / T 2478-2018 "Tailings Concrete for Filling Goafs in Mines"; the expansion degree of Examples 1 to 6 is greater than 190 mm, meeting the requirements of JC / T 2478-2018 "Tailings Concrete for Filling Mine Goafs" stipulates the requirements for F1 expansion grade tailings concrete; compared with ordinary Portland cement (Comparative Example 1) and commercial cement powder (Comparative Example 1), the 7-day compressive strength was increased by 29.2% and 19.2% or more, the 28-day compressive strength was increased by 39.1% and 13.4% or more, and the shrinkage was reduced by 30.9% and 20.8% or more, respectively. This shows that when the solid waste filling material based on fine-grained gold tailings of the present invention is used for filling goafs, the compressive strength of the filling material can be significantly improved and the shrinkage can be reduced.
[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A solid waste filling material based on fine-grained gold tailings, characterized in that: Its raw materials include: Solid waste cementitious materials, fine-grained gold tailings, reinforcing agents and water; The solid waste gelling material includes alkaline solid waste activator and precursor material, the alkaline solid waste activator includes Bayer red mud, fluorgypsum and carbide slag; the precursor material includes slag, high-grade territorial water and waste glass powder; The reinforcing agent comprises inorganic nanomaterials, inorganic whiskers, triethanolamine and dopamine.
2. The solid waste filling material based on fine-grained gold tailings according to claim 1, characterized in that: The mass ratio of the solid waste gelling material to the fine-grained gold tailings is 1:(2-8); The mass ratio of the reinforcing agent to the solid waste gelling material is 1:(50-100); The mass ratio of the water to the sum of the masses of the solid waste cementitious material, the fine-grained gold tailings and the enhancer is 1:(1-4).
3. The solid waste filling material based on fine-grained gold tailings according to claim 1, characterized in that: In the solid waste gelling material, the mass ratio of the alkaline solid waste activator to the precursor material is 1:(4~20); In the alkaline solid waste activator, the mass ratio of Bayer red mud, fluorgypsum and carbide slag is (5~8): (1~4): (1~3); In the precursor materials, the mass ratio of slag, high-altitude land and waste glass powder is (5~7):(1~2):(1~4).
4. The solid waste filling material based on fine-grained gold tailings according to claim 1, characterized in that: In the reinforcing agent, the inorganic nanomaterial includes one or more of nano silicon dioxide, nano titanium dioxide or nano aluminum oxide; In the reinforcing agent, the inorganic whiskers include one or more of calcium carbonate whiskers or calcium sulfate whiskers; In the enhancer, the mass ratio of inorganic nanomaterials, inorganic whiskers, triethanolamine and dopamine is (2~5):(5~8):(1~3):(0.5~2).
5. The solid waste filling material based on fine-grained gold tailings according to claim 1, characterized in that: The particle size of fine-grained gold tailings is less than 0.6 mm and the water content is less than 20%.
6. The solid waste filling material based on fine-grained gold tailings according to claim 1, characterized in that: Among alkaline solid waste activators, the pH value of Bayer red mud leaching is 7~8.5; Among the alkaline solid waste activators, the CaSO4 mass fraction of fluorgypsum is higher than 85%; Among the alkaline solid waste activators, the mass fraction of CaO in carbide slag is higher than 75%.
7. The solid waste filling material based on fine-grained gold tailings according to claim 1, characterized in that: Among the precursor materials, the slag is S95 grade or above; In the precursor material, the total mass fraction of SiO2 and Al2O3 in the high-temperature region is greater than 95%; Among the precursor materials, the mass fraction of SiO2 in the waste glass powder is greater than 70%.
8. The method for preparing a solid waste filling material based on fine-grained gold tailings according to any one of claims 1 to 7, characterized in that: include: The solid waste cementitious material, fine-grained gold tailings, a reinforcing agent and water are mixed to obtain a solid waste filling material based on fine-grained gold tailings.
9. The preparation method according to claim 8, characterized in that: The solid waste cementitious materials are dried and sealed and ground before being mixed with other materials; The drying temperature is 80~105℃, and the drying time is not less than 24 hours; The sealed grinding time is 10-30 min, and the ball mill speed is 400-500 r / min. The specific surface area of the solid waste gelling material after sealed grinding is greater than 520 m 2 / kg.
10. The preparation method according to claim 8, characterized in that: The reinforcing agent is subjected to a compound strengthening treatment before being mixed with other materials. The compound strengthening treatment method includes: placing the reinforcing agent in deionized water, stirring, filtering and drying to obtain a powdered reinforcing agent; The mass ratio of enhancer to deionized water is 1:(45~55); The stirring time is 30~60 min; The drying temperature is 55~65℃ and the drying time is at least 24 hours.
Citation Information
Patent Citations
Preparation method for geopolymer porous material
CN107032676A
Gold tailing curing agent as well as preparation method and use method thereof
CN111875303A
Method for preparing cemented filling material through cooperation of multi-source industrial waste residues and superfine tailings
CN116639945A
Inorganic binder stabilized gold tailing mixture and preparation and construction method thereof
CN117819887A
Nano-modified all-solid-waste mine filling material as well as preparation method and application thereof
CN118702459A
Cited By
High-strength lime-sand polymerized building material and preparation method thereof
CN120423829A
A high-strength lime-sand polymer building material and preparation method thereof
CN120423829B
Low-carbon gold tailing-based ultra-high-performance concrete material suitable for steep-gradient pavement and preparation method of low-carbon gold tailing-based ultra-high-performance concrete material
CN120554080A
Preparation method of road slope reinforcement and ecological regulation composite material based on biological mixed mediation mineralization
CN121270162A