ALD coating device, ALD coating equipment and multi-component film deposition method
By designing an ALD coating device with both time-type and space-type functions, using the combined structure of the spray module and the heating module, selecting the deposition method according to the proportion of the film component, the multi-component film deposition efficiency in the prior art is solved. The problems of low and poor uniformity achieve more efficient and uniform film deposition.
Patent Information
- Application Number
- CN202411159124.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
AI Technical Summary
When the existing ALD devices deposit multi-component film layers, the production efficiency is low and the film formation uniformity is poor. In particular, the time-type devices have cross-contamination problems, and the base of the space-type device needs to be frequently transmitted, so the efficiency is not high.
Design an ALD coating device with both time-type and space-type deposition functions, and distributes up and down in the deposition chamber through the spray module and the heating module to form a deposition channel, using oxygen source spray parts, metal source spray parts, and isolated air sprays. The shower and air extraction parts form spatial and temporal deposition units, and different deposition methods are selected according to the proportion of the film layer components to avoid cross-contamination.
The production efficiency and film formation quality of the multi-component film layer are improved, the deposition uniformity is ensured, and the production cost is reduced.
Smart Images

Figure CN119020755A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of film coating technology, and in particular to an ALD film coating device, an ALD film coating equipment and a multi-component film layer deposition method. Background Art
[0002] Currently, there are two main types of ALD devices on the market: time type and space type.
[0003] For multi-component films such as AZO and ITO, two oxide layers with different component proportions need to be deposited alternately. When a time-type ALD device is used to deposit multi-component films, the production efficiency is very low, and the spray system will have shared pipelines, which will cause cross-contamination problems. When a space-type ALD device is used to deposit multi-component films, the substrate needs to be transferred back and forth between the two chambers, the production efficiency is still low, and the film uniformity is poor. Summary of the invention
[0004] The object of the present invention is to provide an ALD coating device, which has both time-type and space-type deposition functions, can adopt different deposition methods for film layers with different proportions in a multi-component film layer, and has the characteristics of higher production efficiency and better film quality.
[0005] Another object of the present invention is to provide an ALD coating device, which has both time-type and space-type deposition functions, can adopt different deposition methods for film layers with different proportions in a multi-component film layer, and has the characteristics of higher production efficiency and better film quality.
[0006] Another object of the present invention is to provide a multi-component film deposition method, which has the characteristics of higher deposition efficiency and better uniformity.
[0007] The embodiment of the present invention provides a technical solution:
[0008] An ALD coating device comprises a deposition chamber, a spray module and a heating module, wherein the spray module and the heating module are arranged up and down in the deposition chamber, and a deposition channel is formed between the spray module and the heating module for the coating substrate to move;
[0009] The spray module includes an oxygen source spray component, a first metal source spray component, an isolation gas spray component, an exhaust component and a second metal source spray component. The oxygen source spray component, the first metal source spray component, the isolation gas spray component and the exhaust component are arranged along the deposition channel to form a space-type deposition unit; the second metal source spray component is arranged in the deposition chamber, and forms a time-type deposition unit with the oxygen source spray component, the isolation gas spray component and the exhaust component.
[0010] In the ALD coating device provided by the embodiment of the present invention, the oxygen source spray part, the first metal source spray part, the isolated gas spray part and the exhaust part constitute a space-type deposition unit, which can perform space-type deposition on the film layer with a higher proportion of components in the multi-component film layer to improve production efficiency; the second metal source spray part and the oxygen source spray part, the isolation gas spray part and the exhaust part constitute a time-type deposition unit, which can perform time-type deposition on the film layer with a lower proportion of components in the multi-component film layer to improve deposition uniformity, avoid cross contamination caused by shared pipelines, and ensure the quality of deposited film layers. Therefore, the ALD coating device provided by the embodiment of the present invention has both time-type and space-type deposition functions, and has the characteristics of higher production efficiency and better film quality when depositing multi-component film layers, and can reduce production costs.
[0011] The embodiment of the present invention also provides a technical solution:
[0012] An ALD coating device comprises a loading and unloading device, a plurality of functional devices and the aforementioned ALD coating device, wherein the ALD coating device comprises a deposition chamber, a spray module and a heating module, wherein the spray module and the heating module are arranged up and down in the deposition chamber, and a deposition channel for the coating substrate to move is formed between the spray module and the heating module; the spray module comprises an oxygen source spray component, a first metal source spray component, an isolation gas spray component, an exhaust component and a second metal source spray component, wherein the oxygen source spray component, the first metal source spray component, the isolation gas spray component and the exhaust component are arranged along the deposition channel to form a space-type deposition unit; the second metal source spray component is arranged in the deposition chamber, and forms a time-type deposition unit with the oxygen source spray component, the isolation gas spray component and the exhaust component;
[0013] The loading end of the loading and unloading device is connected to one end of the ALD coating device through a part of the multiple functional devices, and the unloading end of the loading and unloading device is connected to the other end of the ALD coating device through the remaining part of the multiple functional devices.
[0014] The ALD coating device provided by the embodiment of the present invention comprises an oxygen source spray part, a first metal source spray part, an isolated gas spray part and an exhaust part, which form a spatial deposition unit, and can perform spatial deposition on a film layer with a higher component ratio in a multi-component film layer to improve production efficiency, and multiple oxygen source spray parts and multiple first metal source spray parts are arranged at equal intervals to ensure the uniformity of spatial deposition; the second metal source spray part of the ALD coating device, the oxygen source spray part, the isolation gas spray part and the exhaust part form a time deposition unit, and can perform time deposition on a film layer with a lower component ratio in a multi-component film layer to further improve deposition uniformity, and the configuration of the second metal source spray part allows different metal sources to be sprayed through different pipelines, thereby avoiding cross contamination and improving film quality. Therefore, the ALD coating device provided by the embodiment of the present invention has both time-type and space-type deposition functions, and has the characteristics of higher production efficiency and better film quality.
[0015] The embodiment of the present invention also provides a technical solution:
[0016] A multi-component film deposition method is applied to the aforementioned ALD coating device, the ALD coating device comprising a deposition chamber, a spray module and a heating module, the spray module and the heating module are arranged up and down in the deposition chamber, and a deposition channel for the coating substrate to move is formed between the two; the spray module comprises an oxygen source spray component, a first metal source spray component, an isolation gas spray component, an exhaust component and a second metal source spray component, the oxygen source spray component, the first metal source spray component, the isolation gas spray component and the exhaust component are arranged along the deposition channel to form a space-type deposition unit; the second metal source spray component is arranged in the deposition chamber, and together with the oxygen source spray component, the isolation gas spray component and the exhaust component, forms a time-type deposition unit; the multi-component film deposition method comprises:
[0017] Controlling the plurality of oxygen source spray parts, the plurality of the first metal source spray parts, the plurality of the isolation gas spray parts and the plurality of the exhaust parts to remain open, and controlling the second metal source spray part to remain closed;
[0018] Controlling the film-coated substrate to reciprocate in the deposition channel, and sequentially chemically absorbing the oxygen source gas sprayed by the oxygen source spraying member and the first metal source gas sprayed by the first metal source spraying member to obtain a first film layer;
[0019] Controlling the plurality of first metal source spray parts to remain closed, and controlling the plurality of oxygen source spray parts to be opened and then closed, so that the plurality of oxygen source spray parts spray oxygen source gas for chemical adsorption of the coating substrate in the deposition channel;
[0020] Controlling the plurality of isolation gas spraying parts and the plurality of exhaust parts to be opened and then closed, so that the isolation gas sprayed by the isolation gas spraying parts can take away the residual oxygen source gas in the deposition channel;
[0021] Controlling the second metal source spraying element to be turned on and then turned off, so that the plurality of second metal source spraying elements spray the second metal source gas for chemical adsorption on the coating substrate to obtain a second film layer;
[0022] The plurality of isolation gas spray parts and the plurality of exhaust parts are controlled to be opened and then closed, so that the isolation gas sprayed by the isolation gas spray parts can take away the second metal source gas and gaseous by-products remaining in the deposition channel.
[0023] The multi-component film deposition method provided by the embodiment of the present invention benefits from the beneficial effects of the ALD coating device and can perform spatial deposition on film layers with a higher component ratio to improve production efficiency; and perform temporal deposition on film layers with a lower component ratio to improve deposition uniformity. Therefore, the multi-component film deposition method provided by the embodiment of the present invention has the characteristics of higher deposition efficiency and better film quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other related drawings can also be obtained based on these drawings without creative work.
[0025] Figure 1 A schematic structural diagram of an ALD coating device provided by an embodiment of the present invention;
[0026] Figure 2 It is a structural schematic diagram of the spray module of the ALD coating device;
[0027] Figure 3 A schematic diagram of the structure of an ALD coating device provided by an embodiment of the present invention;
[0028] Figure 4 A flowchart of a multi-component film deposition method provided for an embodiment of the present invention.
[0029] Icons: 100-ALD coating device; 110-deposition chamber; 120-spray module; 121-oxygen source spray component; 122-first metal source spray component; 123-isolation gas spray component; 124-exhaust component; 125-second metal source spray component; 130-heating module; 140-deposition channel; 150-reciprocating conveying module; 200-ALD coating equipment; 210-loading and unloading device; 220-preheating device; 230-feeding device; 240-discharging device; 250-lifting device; 260-return device. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0031] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0033] In the description of the present invention, it should be understood that the terms "upper", "lower", "inside", "outside", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, or are directions or positional relationships in which the product of the invention is usually placed when in use, or are directions or positional relationships commonly understood by those skilled in the art. These directions or positional relationships are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.
[0034] Furthermore, the terms “first”, “second”, etc. are merely used for distinguishing descriptions and should not be understood as indicating or implying relative importance.
[0035] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms such as "setting" and "connection" should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0036] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings.
[0037] Example
[0038] See also Figure 1 , Figure 1 FIG. 1 is a schematic structural diagram of an ALD coating device 100 provided in this embodiment.
[0039] The ALD coating device 100 provided in this embodiment includes a deposition chamber 110, a spray module 120 and a heating module 130. The spray module 120 and the heating module 130 are distributed up and down in the deposition chamber 110, and a deposition channel 140 for the coating substrate to move is formed between the spray module 120 and the heating module 130.
[0040] The ALD coating device 100 provided in this embodiment has both spatial deposition function and temporal deposition function. In practical applications, while the coating substrate moves along the deposition channel 140, spatial deposition and temporal deposition on the coating substrate can be completed step by step.
[0041] Please refer to Figure 2 , Figure 2 FIG. 1 is a schematic structural diagram of the spray module 120 .
[0042] The spray module 120 of the ALD coating device 100 includes an oxygen source spray component 121, a first metal source spray component 122, an isolation gas spray component 123, an exhaust component 124 and a second metal source spray component 125. The oxygen source spray component 121 is used to spray oxygen source gas to the deposition channel 140, the first metal source spray component 122 is used to spray the first metal source gas to the deposition channel 140, the isolation gas spray component 123 is used to spray isolation gas to the deposition channel 140, the exhaust component 124 is used to exhaust and discharge to the outside, and the second metal source spray component 125 is used to spray the second metal source gas to the deposition channel 140.
[0043] The oxygen source spraying member 121, the first metal source spraying member 122, the isolation gas spraying member 123 and the exhaust member 124 constitute a spatial deposition unit. Specifically, a plurality of oxygen source spraying members 121 and a plurality of first metal source spraying members 122 are sequentially arranged at intervals along the deposition channel 140, and an isolation gas spraying member 123 and an exhaust member 124 are arranged between any adjacent oxygen source spraying members 121 and first metal source spraying members 122.
[0044] In practical applications, the oxygen source spraying member 121, the first metal source spraying member 122 and the isolation gas spraying member can each form different gas atmosphere fields at different positions of the deposition channel 140. The oxygen source spraying member 121 can continuously spray the oxygen source gas to form the oxygen source gas atmosphere field, the isolation gas spraying member can continuously spray the isolation gas to form the isolation gas atmosphere field, and the first metal source spraying member 122 can continuously spray the first metal source gas to form the first metal source gas atmosphere field.
[0045] Since the isolation gas spraying part is located between the oxygen source spraying part 121 and the first metal source spraying part 122, that is, the isolation gas atmosphere field is located between the oxygen source gas atmosphere field and the first metal source gas atmosphere field, the isolation of the oxygen source gas atmosphere field and the first metal source gas atmosphere field is achieved. The exhaust part 124 is used to extract the excess gas from the deposition channel 140 between the oxygen source gas atmosphere field and the first metal source gas atmosphere field, so as to achieve the reflux of the oxygen source gas, the isolation gas and the first metal source gas, so as to maintain the stability of each gas atmosphere field state.
[0046] In actual applications, during the movement of the coated substrate along the deposition channel 140, it passes through the oxygen source gas atmosphere, the isolation gas atmosphere and the first metal source gas atmosphere in sequence. During the process of passing through the oxygen source gas atmosphere, the surface of the coated substrate chemically adsorbs the oxygen source gas; during the process of passing through the isolation gas atmosphere, under the action of the exhaust component 124, the isolation gas blows away the unadsorbed oxygen source gas remaining on the surface of the coated substrate; during the process of passing through the first metal source gas atmosphere, the surface of the coated substrate chemically adsorbs the first metal source gas again, thereby completing an ALD deposition reaction to form a first film layer.
[0047] In this embodiment, in the arrangement queue composed of multiple oxygen source spray parts 121 and multiple first metal source spray parts 122, the head and the end of the arrangement queue are both oxygen source spray parts 121. It is ensured that during the reciprocating motion of the coating substrate along the deposition channel 140, the coating substrate can pass through the oxygen source gas atmosphere and the first metal source gas atmosphere respectively, ensuring that the first film layer can be continuously deposited during the reciprocating motion, thereby improving the deposition efficiency. In addition, the head and the end of the arrangement queue are both oxygen source spray parts 121, which can control the influence range of the first metal source gas, avoid the first metal source from diffusing in large quantities to other positions of the cavity, avoid the generation and accumulation of dust, and also ensure the safety of the cavity opening.
[0048] In addition, isolation gas spraying parts 123 and exhaust parts 124 are arranged at both ends of the array consisting of a plurality of oxygen source spraying parts 121 and a plurality of first metal source spraying parts 122. The purpose is to isolate the two end areas of the deposition chamber 110 from the deposition channel 140 to prevent other gases in the deposition chamber 110 from entering along the deposition channel 140, thereby affecting the deposition quality of the film layer.
[0049] In this embodiment, an isolation gas spraying member 123 and an exhaust member 124 are arranged at both ends of the arrangement queue, and the exhaust member 124 is located between the isolation gas spraying member 123 and the oxygen source spraying member 121. It can be understood that the isolation gas spraying member 123 and the exhaust member 124 at both ends of the arrangement queue, the exhaust member 124 extracts the excess isolation gas and the excess oxygen source gas and completes the reflux.
[0050] Between the adjacent oxygen source spraying member 121 and the first metal source spraying member 122 , an isolation gas spraying member 123 and two exhaust members 124 are arranged, and the isolation gas spraying member 123 is located between the two exhaust members 124 .
[0051] In practical applications, in the area between the adjacent oxygen source spraying member 121 and the first metal source spraying member 122, one of the two exhaust members 124 can exhaust part of the excess oxygen source gas sprayed by the adjacent oxygen source spraying member 121 and part of the excess isolation gas sprayed by the isolation gas spraying member 123; the remaining one of the two exhaust members 124 can exhaust part of the excess first metal source gas sprayed by the adjacent first metal source spraying member 122 and part of the excess isolation gas sprayed by the isolation gas spraying member 123. This prevents the isolation gas from entering the oxygen source gas atmosphere field or the first metal source gas atmosphere field, and also prevents the oxygen source gas atmosphere field from cross-mixing with the first metal source gas atmosphere field.
[0052] It is understandable that, in the process of the coated substrate passing through the deposition channel 140, the coated substrate will alternately pass through multiple oxygen source gas atmosphere fields and the first metal source gas atmosphere fields in sequence, and can repeatedly complete multiple deposition reactions to form first film layers of different thicknesses. Limited by the size of the deposition chamber 110 and the spray module 120, if the required first film layer thickness is large, the coated substrate can be controlled to reciprocate multiple times in the deposition channel 140, thereby achieving multiple spatial depositions to obtain a first film layer that meets the thickness requirements.
[0053] In this embodiment, the ALD coating device 100 further includes a reciprocating conveying module 150, which is disposed in the deposition channel 140 and is used to convey the coating substrate to move back and forth in the deposition channel 140. It can be understood that in actual applications, the coating substrate is usually loaded on a carrier, that is, the reciprocating conveying module 150 actually conveys the carrier to move in the deposition channel 140.
[0054] The oxygen source spraying part 121, the second metal source spraying part 125, the isolation gas spraying part 123 and the exhaust part 124 constitute a time-type deposition unit. It is understandable that in the process of space-type deposition, in order to avoid cross-contamination of different metal source gases, the second metal source spraying part 125 needs to be kept closed. Similarly, in the process of space-type deposition, the first metal source spraying part 122 also needs to be kept closed.
[0055] For time-based deposition, the oxygen source spray component 121, the isolation gas spray component 123, and the second metal source spray component 125 are all pulse-controlled while the first metal source spray component 122 remains closed. Specifically, when the film-coated substrate is in the deposition channel 140, the plurality of oxygen source spray components 121 are first controlled to be opened and then closed, so as to pulse-spray the oxygen source gas into the deposition channel 140, so that the surface of the film-coated substrate adsorbs the oxygen source gas molecules, so that the oxygen source gas molecules react at the surface active sites of the film-coated substrate to form a saturated monolayer.
[0056] Then, the plurality of isolation gas spray parts 123 and the plurality of exhaust parts 124 are controlled to be opened and then closed, so as to purge the deposition chamber 110 with the isolation gas to remove the residual oxygen source gas and reaction byproducts. Then, the second metal source spray part 125 is controlled to be opened and then closed, so as to spray the second metal source gas into the deposition channel 140, so that the coating substrate that has completed the adsorption of the oxygen source gas molecules chemically adsorbs the second metal source gas molecules again, so that the second metal source gas molecules react with the saturated monolayer to generate a second film layer.
[0057] Finally, the plurality of isolation gas spraying components 123 and the plurality of exhaust components 124 are controlled to be opened and then closed, so as to purge the deposition chamber 110 again with the isolation gas to remove the residual second metal source gas and reaction byproducts.
[0058] In order to ensure deposition uniformity and deposition efficiency, in this embodiment, the number of the second metal source spraying parts 125 is multiple, and the multiple second metal source spraying parts 125 are arranged at equal intervals along the deposition channel 140. In addition, in order to further improve deposition uniformity and deposition efficiency, during the time-based deposition process, the reciprocating conveying module 150 can also convey the coating substrate to move back and forth in the deposition channel 140.
[0059] As a preference, in this embodiment, in the extension direction of the deposition channel 140, the plurality of second metal source spraying parts 125 are respectively arranged adjacent to the plurality of oxygen source spraying parts 121. This is equivalent to a one-to-one correspondence between the spraying positions of the plurality of second metal source spraying parts 125 and the plurality of oxygen source spraying parts 121, that is, there is no isolation gas spraying part 123 and exhaust part 124 between any second metal source spraying part 125 and its adjacent oxygen source spraying part 121, which can further improve the film formation uniformity of the time-based deposition film layer, shorten the movement stroke of the coating substrate during the deposition process, and improve the deposition efficiency.
[0060] Furthermore, since dust is mainly generated near the metal source spray port during the spatial deposition of the film layer, multiple second metal source spray parts 125 and multiple oxygen source spray parts 121 are respectively arranged correspondingly, which can reduce the generation of dust during the deposition process.
[0061] Specifically, in the spray module 120 of this embodiment, the isolation gas spray component 123, the exhaust component 124, the second metal source spray component 125, the oxygen source spray component 121, the exhaust component 124, the isolation gas spray component 123, the exhaust component 124, the first metal source spray component 122, and the exhaust component 124 are arranged in the order Figure 2 In the state shown, they are arranged from left to right in sequence to form an arrangement unit.
[0062] Multiple layout units Figure 2 In the figure, the unit queue is formed from left to right, and at the rightmost end of the unit queue, the isolation gas spray part 123, the exhaust part 124, the second metal source spray part 125, the oxygen source spray part 121, the exhaust part 124, and the isolation gas spray part 123 are arranged from left to right. It can be understood that in this embodiment, multiple oxygen source spray parts 121 are connected to the same oxygen source pipeline, and the oxygen source pipeline can input external oxygen source gas into multiple oxygen source spray parts 121 for separate spraying. The oxygen source gas can be gaseous water, hydrogen peroxide, and plasma state oxygen. Multiple isolation gas spray parts 123 are connected to the same isolation gas pipeline, and the isolation gas pipeline can input external isolation gas into multiple isolation gas spray parts 123 for separate spraying. The isolation gas can be an inert gas such as nitrogen.
[0063] Similarly, multiple first metal source spraying parts 122 are connected to the same first metal source pipeline, and the first metal source pipeline inputs the external first metal source gas to the multiple first metal source spraying parts 122 for spraying respectively. Multiple second metal source spraying parts 125 are connected to the same second metal source pipeline, and the second metal source pipeline inputs the external second metal source gas to the multiple second metal source spraying parts 125 for spraying respectively.
[0064] Taking the deposition of AZO thin film as an example, the deposition of the zinc oxide film layer with a larger component proportion is completed by a space-type deposition unit, that is, the first film layer is a zinc oxide film layer, and the first metal source gas is a zinc source gas; the deposition of the aluminum oxide film layer with a smaller component proportion is completed by a time-type deposition unit, that is, the second film layer is an aluminum oxide film layer, and the second metal source gas is an aluminum source gas.
[0065] Taking the deposition of ITO thin film as an example, the deposition of the indium oxide film layer with a larger component proportion is completed by a space-type deposition unit, that is, the first film layer is an indium oxide film layer, and the first metal source gas is an indium source gas; the deposition of the tin oxide film layer with a smaller component proportion is completed by a time-type deposition unit, that is, the second film layer is a tin oxide film layer, and the second metal source gas is a tin source gas.
[0066] It can be seen that in the ALD coating device 100 provided in this embodiment, the oxygen source spray component 121, the first metal source spray component 122, the isolated gas spray component 123 and the exhaust component 124 in the spray module 120 form a space-type deposition unit, which can perform space-type deposition on the film layer with a higher proportion of components in the multi-component film layer to improve production efficiency. The second metal source spray component 125, the oxygen source spray component 121, the isolated gas spray component 123 and the exhaust component 124 in the spray module 120 form a time-type deposition unit, which can perform time-type deposition on the film layer with a lower proportion of components in the multi-component film layer to improve deposition uniformity. In addition, different reaction gases are sprayed synchronously by different spray components, which can avoid cross contamination and further improve the film quality.
[0067] Therefore, the ALD coating device 100 provided in the embodiment of the present invention has both time-based and space-based deposition functions, and has the advantages of higher production efficiency and better film formation uniformity.
[0068] This embodiment also provides an ALD coating device 200, see Figure 3 , Figure 3 FIG. 2 is a schematic structural diagram of the ALD coating device 200 .
[0069] The ALD coating device 200 provided in this embodiment includes a loading and unloading device 210, a plurality of functional devices, and the aforementioned ALD coating device 100. The loading and unloading device 210 has a loading end for loading a coating substrate, and a unloading end for unloading a coating substrate. The loading end of the loading and unloading device 210 is connected to one end of the ALD coating device 100 through a portion of the plurality of functional devices, and the unloading end of the loading and unloading device 210 is connected to the other end of the ALD coating device 100 through the remaining portion of the plurality of functional devices.
[0070] It can be understood that in actual applications, the coated substrate is loaded onto the carrier from the loading end. After loading is completed, the carrier drives the coated substrate to pass through multiple functional devices in sequence and then enter the ALD coating device 100. In the process of passing through multiple functional devices, multiple functional devices perform pre-coating processing on the coated substrate.
[0071] In this embodiment, the multiple functional devices include a preheating device 220 located between the loading end of the loading and unloading device 210 and the ALD coating device 100. The preheating device 220 is used to preheat the coating substrate during its passage so that the temperature of the coating substrate reaches the temperature requirement of ALD deposition.
[0072] During the process of the coating substrate passing through the deposition chamber 110 of the ALD coating device 100, at least one of the spatial deposition and the temporal deposition can be completed. After the coating substrate leaves the ALD coating device 100 after the thin film deposition is completed, it is processed by multiple functional devices and then reaches the unloading end of the loading and unloading device, and the unloading is completed.
[0073] Specifically, in the present embodiment, in addition to the preheating device 220, the plurality of functional devices further include a feeding device 230, a discharging device 240, a lifting device 250 and a return device 260. The loading end of the loading and unloading device 210, the feeding device 230, the preheating device 220, the ALD coating device 100, the discharging device 240, the lifting device 250, the return device 260 and the unloading end of the loading and unloading device 210 are sequentially connected to form a conveying path, and a conveying mechanism is arranged on the conveying path for conveying the coated substrate, and the reciprocating conveying module 150 of the ALD coating device 100 is a part of the conveying mechanism.
[0074] Benefiting from the beneficial effects of the ALD coating device 100, the ALD coating equipment 200 provided in this embodiment has both time-based and space-based deposition functions, and has the advantages of higher production efficiency and better film formation uniformity.
[0075] In addition, this embodiment also provides a multi-component film deposition method, which is applied to the aforementioned ALD coating device 100. Figure 4 , Figure 4 The flowchart of the multi-component film deposition method is shown. The multi-component film deposition method provided in this embodiment may include:
[0076] Step S101 , while controlling the second metal source spraying member 125 to remain closed, controlling the plurality of oxygen source spraying members 121 , the plurality of first metal source spraying members 122 , the plurality of isolation gas spraying members 123 and the plurality of exhaust members 124 to open.
[0077] In step S102, the coating substrate is controlled to move along the deposition channel 140, and sequentially passes through the oxygen source gas atmosphere formed by the oxygen source spray component 121, the isolation gas atmosphere formed by the isolation gas spray component 123, and the first metal source gas atmosphere formed by the first metal source spray component 122 to obtain a first film layer.
[0078] In step S103 , while controlling the plurality of first metal source spray components 122 to remain closed, the plurality of oxygen source spray components 121 are controlled to be opened and then closed, so that the coating substrate in the deposition channel 140 chemically absorbs the oxygen source gas sprayed by the plurality of oxygen source spray components 121 .
[0079] In step S104 , the plurality of isolation gas spraying parts 123 and the plurality of exhaust parts 124 are controlled to be opened and then closed, so that the isolation gas sprayed by the isolation gas spraying parts 123 can take away the residual oxygen source gas in the deposition channel 140 .
[0080] Step S105 , controlling the second metal source spraying member 125 to be opened and then closed, so that the coating substrate that has absorbed the oxygen source gas chemically absorbs the second metal source gas sprayed by the plurality of second metal source spraying members 125 to obtain a second film layer.
[0081] Step S101 and step S102 are actually steps of spatial deposition. During the movement of the coated substrate along the deposition channel 140, it passes through the oxygen source gas atmosphere, the isolation gas atmosphere and the first metal source gas atmosphere in sequence. During the process of passing through the oxygen source gas atmosphere, the surface of the coated substrate chemically adsorbs the oxygen source gas; during the process of passing through the isolation gas atmosphere, under the action of the exhaust component 124, the isolation gas blows away the oxygen source gas remaining on the surface of the coated substrate that has not been adsorbed; during the process of passing through the first metal source gas atmosphere, the surface of the coated substrate chemically adsorbs the first metal source gas again, thereby forming a first film layer.
[0082] Step S103, step S104 and step S105 are actually time-based deposition steps. When the coated substrate is in the deposition channel 140, the multiple oxygen source spray parts 121 are first controlled to open and then closed to spray the oxygen source gas pulse into the deposition channel 140, so that the surface of the coated substrate adsorbs the oxygen source gas molecules, so that the oxygen source gas molecules react at the surface active points of the coated substrate to form a saturated monolayer. Then, the multiple isolation gas spray parts 123 and the multiple exhaust parts 124 are controlled to open and then closed to purge the deposition chamber 110 with isolation gas to remove residual oxygen source gas and reaction by-products. Then, the second metal source spray part 125 is controlled to open and then closed to spray the second metal source gas into the deposition channel 140, so that the coated substrate that has completed the adsorption of oxygen source gas molecules chemically adsorbs the second metal source gas molecules again, so that the second metal source gas molecules react with the saturated monolayer to generate a second film layer.
[0083] In fact, after step S105, step S106 can also be included to control multiple isolation gas spray parts 123 and multiple exhaust parts 124 to be opened and then closed, so that the isolation gas sprayed by the isolation gas spray parts 123 can take away the second metal source gas and gaseous by-products remaining in the deposition channel 140.
[0084] It should be noted that the spatial deposition step composed of step S101 and step S102 and the temporal deposition step composed of step S103, step S104 and step S105 can be performed in sequence when forming a multi-component film layer. In other cases, there may be no sequence of execution between the two, and when forming a single-component film layer, one can be selected and executed according to actual process requirements.
[0085] In summary, the multi-component film deposition method provided in this embodiment combines spatial deposition with temporal deposition, and has the characteristics of higher deposition efficiency and better film quality.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An ALD coating device, characterized in that: It comprises a deposition chamber (110), a spray module (120) and a heating module (130), wherein the spray module (120) and the heating module (130) are both accommodated in the deposition chamber (110), and a deposition channel (140) is provided between the spray module (120) and the heating module (130); The spray module (120) comprises an oxygen source spray component (121), a first metal source spray component (122), an isolation gas spray component (123), an exhaust component (124) and a second metal source spray component (125); a plurality of the oxygen source spray components (121) and a plurality of the first metal source spray components (122) are sequentially arranged at intervals along the deposition channel (140); the isolation gas spray component (123) and the exhaust component (124) are arranged between any adjacent oxygen source spray components (121) and the first metal source spray components (122); the first metal source spray component (122) and the second metal source spray component (125) are used to spray different metal source gases into the deposition channel (140).
2. The ALD coating device according to claim 1, characterized in that: There are multiple second metal source spraying parts (125), and the multiple second metal source spraying parts (125) are arranged in sequence at equal intervals along the deposition channel (140).
3. The ALD coating device according to claim 2, characterized in that: In the extension direction of the deposition channel (140), the plurality of second metal source spraying elements (125) are respectively arranged adjacent to the plurality of oxygen source spraying elements (121).
4. The ALD coating device according to claim 1, characterized in that: In an arrangement queue consisting of a plurality of the oxygen source spraying elements (121) and a plurality of the first metal source spraying elements (122), the head end and the tail end of the arrangement queue are both the oxygen source spraying elements (121).
5. The ALD coating device according to claim 1, characterized in that: An isolation gas spray component (123) and an exhaust component (124) are arranged at both ends of an arrangement queue consisting of a plurality of the oxygen source spray components (121) and a plurality of the first metal source spray components (122), and the exhaust component (124) is located between the isolation gas spray component (123) and the oxygen source spray component (121).
6. The ALD coating device according to claim 1, characterized in that: An isolation gas spraying component (123) and two exhaust components (124) are arranged between the adjacent oxygen source spraying components (121) and the first metal source spraying component (122), and the isolation gas spraying component (123) is located between the two exhaust components (124).
7. The ALD coating device according to claim 1, characterized in that: The ALD coating device (100) further comprises a reciprocating transport module (150), which is accommodated in the deposition chamber (110) and located between the spray module (120) and the heating module (130). The reciprocating transport module (150) is used to transport the coating substrate to move back and forth in the deposition channel (140).
8. An ALD coating device, characterized in that: It comprises a loading and unloading device (210), a plurality of functional devices and an ALD coating device (100) as described in any one of claims 1 to 7, wherein the loading end of the loading and unloading device (210) is connected to one end of the ALD coating device (100) through a portion of the plurality of functional devices, and the unloading end of the loading and unloading device (210) is connected to the other end of the ALD coating device (100) through the remaining portion of the plurality of functional devices.
9. The ALD coating device according to claim 8, characterized in that: The plurality of functional devices include a preheating device (220) located between the loading end of the loading and unloading device (210) and the ALD coating device (100).
10. A multi-component film deposition method, applied to the ALD coating device (100) according to any one of claims 1 to 7, characterized in that: The multi-component film deposition method comprises: While controlling the second metal source spray component (125) to remain closed, controlling the plurality of oxygen source spray components (121), the plurality of first metal source spray components (122), the plurality of isolation gas spray components (123) and the plurality of exhaust components (124) to open; Controlling the coating substrate to move along the deposition channel (140), passing through the oxygen source gas atmosphere formed by the oxygen source spray component (121), the isolation gas atmosphere formed by the isolation gas spray component (123), and the first metal source gas atmosphere formed by the first metal source spray component (122) in sequence, so as to obtain a first film layer; While controlling the plurality of first metal source spray parts (122) to remain closed, controlling the plurality of oxygen source spray parts (121) to be opened and then closed, so that the coating substrate in the deposition channel (140) chemically absorbs the oxygen source gas sprayed by the plurality of oxygen source spray parts (121); Controlling the plurality of isolation gas spraying parts (123) and the plurality of exhaust parts (124) to be opened and then closed, so that the isolation gas sprayed by the isolation gas spraying parts (123) can take away the oxygen source gas remaining in the deposition channel (140); The second metal source spraying element (125) is controlled to be opened and then closed, so that the coating substrate that has absorbed the oxygen source gas chemically absorbs the second metal source gas sprayed by the plurality of second metal source spraying elements (125) to obtain a second film layer.