Polyelectrolyte loose nanofiltration membrane with high permeation flux and preparation method and application thereof
Through alternate self-assembly, the polyelectrolyte loose nanofiltration membrane is solved, and the existing nanofiltration membrane has low permeability flux and poor separation selectivity is achieved, which is effective for dyes and salts. Separation.
Patent Information
- Application Number
- CN202411265288.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
The existing nanofiltration membrane has low permeability flux and poor separation selectivity, making it difficult to achieve high selectivity separation of dyes and salts.
A polyelectrolyte loose nanofiltration membrane formed by alternately self-assembly of anionic polyelectrolyte with a rigid backbone and a cationic polyelectrolyte with a flexible backbone is used to form a loose structure through the interaction of charge and hydrogen bonds, which improves the looseness and selectivity of the membrane.
High permeability flux and high selective separation are achieved, which can effectively intercept dyes and allow salt to pass through, reduce production costs and facilitate large-scale application.
Smart Images

Figure CN119034484A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanofiltration membranes, and in particular relates to a polyelectrolyte loose nanofiltration membrane with high permeation flux and a preparation method and application thereof. Background Art
[0002] The textile printing and dyeing industry is a traditional industry with high water consumption, and the wastewater it produces has become one of the main industrial wastewaters. Direct discharge of printing and dyeing wastewater will not only cause harm to the environment and human health, but also waste a large amount of dyes and inorganic salts. Traditional treatment methods for printing and dyeing wastewater, such as flocculation sedimentation, biodegradation, adsorption and oxidation catalysis, have problems such as high cost and low recovery rate of dyes and salts. Nanofiltration technology has attracted widespread attention in the field of printing and dyeing wastewater treatment due to its advantages such as low energy consumption, high separation efficiency and no secondary pollution. Loose nanofiltration membranes have a large molecular weight cutoff (500-2000Da), allowing most inorganic salts to pass through and being able to retain large-volume dye molecules. They are widely used in the selective separation of dyes and salts.
[0003] The preparation methods of nanofiltration membrane mainly include interfacial polymerization, layer-by-layer self-assembly, surface deposition, etc. Among them, the polyelectrolyte layer-by-layer self-assembly membrane preparation method is a clean and efficient membrane preparation method. At present, the polyelectrolytes commonly used in polyelectrolyte nanofiltration membranes include polyethyleneimine, polyallylamine hydrochloride, polyallyldimethylammonium chloride, polyvinyl sulfate, polyacrylic acid and sodium polystyrene sulfonate, etc. For example, although the Chinese invention patent with publication number CN 111992040 A prepares polyelectrolyte nanofiltration membranes, these polyelectrolytes have highly flexible molecular main chains and high charge density. The prepared polyelectrolyte nanofiltration membranes have a relatively dense structure and are mainly used for the separation of monovalent / divalent salts or monovalent / multivalent salts, and the permeability of water and salts is poor; at the same time, the cross-linking agent added during the preparation process further makes it difficult to achieve high selective separation of dyes and salts. Summary of the invention
[0004] In view of the above problems, the purpose of the present invention is to provide a polyelectrolyte loose nanofiltration membrane with high permeability flux and a preparation method thereof, so as to overcome the problems of low permeability flux, poor separation selectivity and difficulty in achieving high selective separation of dyes and salts in existing nanofiltration membranes.
[0005] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:
[0006] In a first aspect, the present invention provides a polyelectrolyte loose nanofiltration membrane with high permeation flux, comprising an ultrafiltration membrane and a polyelectrolyte layer supported on the surface thereof, wherein the polyelectrolyte layer is self-assembled by alternating cationic polyelectrolyte layers and anionic polyelectrolyte layers; wherein the cationic polyelectrolyte layer in the polyelectrolyte layer is supported on the surface of the ultrafiltration membrane;
[0007] The anionic polyelectrolyte layer is composed of anionic polyelectrolytes having a rigid main chain;
[0008] The cationic polyelectrolyte layer is composed of a cationic polyelectrolyte having a flexible main chain;
[0009] The pure water flux of the polyelectrolyte loose nanofiltration membrane is 150-350LMH.
[0010] The polyelectrolyte loose nanofiltration membrane provided by the present invention is formed by self-assembly layer by layer of anionic polyelectrolytes with rigid main chains and cationic polyelectrolytes with flexible main chains by means of charge interaction and hydrogen bond interaction. There are many large-volume benzene rings in the anionic polyelectrolyte molecules with rigid main chains, and the bending of their molecular skeletons is limited, so it is easy to form a loose molecular structure, produce a large free volume, and improve the looseness of the membrane. The pure water flux of the prepared loose nanofiltration membrane is 150-280LMH; the surface is flat and has many small pores, and the separation layer is thin, with a thickness of 20-40nm. The loose membrane structure realizes high permeability of salts and high retention rate of dyes, thereby realizing high selective separation of dyes / salts.
[0011] In some other embodiments, the ultrafiltration membrane has a molecular weight cutoff of 100 to 200 Kda;
[0012] Preferably, the ultrafiltration membrane is one or more of a polysulfone ultrafiltration membrane, a polyethersulfone ultrafiltration membrane or a polyacrylonitrile ultrafiltration membrane.
[0013] In some other embodiments, the cationic polyelectrolyte is one or more of polyethyleneimine, polyacrylamide, polyvinyl alcohol, and polyallylamine hydrochloride cationic polyelectrolytes;
[0014] Preferably, the average molecular weight of the polyethyleneimine is 20,000-30,000;
[0015] The average molecular weight of polyallylamine hydrochloride is 10,000-20,000.
[0016] In some other embodiments, the anionic polyelectrolyte is one or more of sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, and sulfonated polyimide anionic polyelectrolyte.
[0017] In a second aspect, the present invention provides a method for preparing the polyelectrolyte loose nanofiltration membrane with high permeation flux as described in the first aspect, comprising the following steps:
[0018] (1) Spraying a cationic polyelectrolyte aqueous solution on the surface of an ultrafiltration membrane, leaving it to stand at room temperature, and then rinsing it with deionized water;
[0019] (2) spraying an aqueous solution of anionic polyelectrolyte on the surface of the sample obtained in step (1), letting it stand at room temperature and then rinsing it with deionized water to obtain a polyelectrolyte loose nanofiltration membrane;
[0020] (3) Repeat steps (1) and (2) to obtain a multilayer polyelectrolyte loose nanofiltration membrane.
[0021] The preparation method of the polyelectrolyte loose nanofiltration membrane of the present invention has many types of raw materials and a wide range of sources; the spraying method can effectively shorten the membrane preparation time and improve the membrane preparation efficiency; the membrane preparation solvent is water, which not only greatly reduces the production cost, but is also green and environmentally friendly, and the membrane preparation method is easy to promote and apply on a large scale. At the same time, the structure of the polyelectrolyte loose nanofiltration membrane can be flexibly adjusted according to the type, concentration, number of assembled layers, etc. of the polyelectrolyte, so as to meet different application requirements.
[0022] In some other embodiments, in step (1), the concentration of the cationic polyelectrolyte is 0.3-1.5 g / L; the spraying pressure is 0.2-0.4 MPa; the standing time is 5-20 min; and the deionized water rinsing time is 1-5 min.
[0023] In some other embodiments, in step (2), the preparation method of the anionic polyelectrolyte is: stirring and dissolving the raw materials and concentrated sulfuric acid, and reacting under a nitrogen atmosphere; after the reaction is completed, pouring the reaction solution into ice water, neutralizing the remaining acid with sodium hydroxide, separating and purifying, and freeze-drying to obtain the anionic polyelectrolyte; the raw material is one of polysulfone, polyethersulfone, polyetheretherketone or polyimide with a rigid main chain;
[0024] Preferably, the stirring and dissolving temperature is 30-40° C., and the stirring time is 6-8 h; the reaction temperature is 70-80° C., and the reaction time is 8-12 h.
[0025] In some other embodiments, in step (2), the concentration of the anionic polyelectrolyte is 0.3-1.5 g / L; the spraying pressure is 0.2-0.4 MPa; the standing time is 5-20 min; and the deionized water rinsing time is 1-5 min.
[0026] In some other embodiments, in step (3), the multi-layered polyelectrolyte loose nanofiltration membrane is an alternating anionic polyelectrolyte layer and cationic polyelectrolyte layer;
[0027] The cationic polyelectrolyte layer in the polyelectrolyte layer is supported on the surface of the ultrafiltration membrane.
[0028] In a third aspect, the present invention provides an application of the polyelectrolyte loose nanofiltration membrane with high permeability flux described in the first aspect in the selective separation of dyes and salts or in wastewater treatment; preferably, the salt includes sodium chloride and sodium sulfate; the dye includes Congo red; preferably, the wastewater is textile printing and dyeing wastewater.
[0029] The beneficial effects of the present invention are:
[0030] (1) The polyelectrolyte loose nanofiltration membrane prepared by the present invention is made of engineering plastics with a rigid skeleton as raw materials, and an anionic polyelectrolyte with a rigid main chain is prepared by a simple electrophilic substitution reaction, and assembled with a cationic polyelectrolyte with a flexible main chain to prepare a loose nanofiltration membrane material with high flux and high separation selectivity. The rigid anionic polyelectrolyte contains high-density and large-volume benzene rings, and because the intramolecular rotation and bending are limited, the molecular chain is usually in a stretched or expanded state, and the rigid stacking between the molecular chains will form a large free volume, thereby obtaining a loose membrane structure, allowing salt to pass through, and effectively intercepting dye molecules, to achieve efficient separation of dye / salt.
[0031] (2) The preparation method of the polyelectrolyte loose nanofiltration membrane of the present invention has many types of raw materials with wide sources; the spraying method can effectively shorten the membrane preparation time and improve the membrane making efficiency; the membrane making solvent is water, which not only greatly reduces the production cost but also is green and environmentally friendly. The membrane making method is easy to promote and apply on a large scale.
[0032] (3) The polyelectrolyte loose nanofiltration membrane prepared by the present invention has excellent water permeability and dye / salt separation selectivity. In an implementation case where sulfonated polysulfone is used as an anionic polyelectrolyte and polyethyleneimine is used as a cationic polyelectrolyte, the pure water flux is 228.0LMH. When the raw material liquid is a mixed solution of Congo red (0.2 g / L) and sodium chloride (10 g / L), the membrane permeation flux is 120.0LMH, the retention rate of sodium chloride is only 1.2%, the retention rate of Congo red is 99.7%, and the separation selectivity is 83.1. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is the pure water flux of Examples 1-5 of the present invention and Comparative Example 1;
[0034] Figure 2 The scanning electron microscope images of the surface and the cross section of Example 3 and Comparative Example 1 of the present invention are shown in FIG. 1 : (a) is a surface scanning electron microscope image of Example 3, (b) is a cross section scanning electron microscope image of Example 3, (c) is a surface scanning electron microscope image of Comparative Example 1, and (d) is a cross section scanning electron microscope image of Comparative Example 1;
[0035] Figure 3 The maximum molecular weight cut-off (a) and probability density function (b) of Example 3 and Comparative Example 1 of the present invention;
[0036] Figure 4 The separation performance of Example 3 of the present invention and Comparative Example 1 on the dye / salt mixture. DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with implementation cases, which do not limit the present invention in any form.
[0038] 1. Preparation of polyelectrolyte loose nanofiltration membrane with high permeation flux
[0039] Example 1
[0040] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polysulfone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 80°C under a nitrogen atmosphere and the reaction was carried out for 12 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0041] (2) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.5 g / L polyethyleneimine aqueous solution is prepared. By spraying, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.2 MPa and maintained at room temperature for 10 minutes.
[0042] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0043] (4) Prepare a sulfonated polysulfone aqueous solution (1 g / L), and spray 8 ml of the sulfonated polysulfone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.2 MPa by spraying, and keep it at room temperature for 10 minutes to ensure sufficient reaction.
[0044] (5) The sample obtained in step (4) was rinsed with deionized water for 1 minute to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 1.0.
[0045] Example 2
[0046] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polysulfone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 80°C under a nitrogen atmosphere and the reaction was carried out for 12 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0047] (2) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.5 g / L polyethyleneimine aqueous solution is prepared. By spraying, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.2 MPa and maintained at room temperature for 10 minutes.
[0048] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0049] (4) Prepare a sulfonated polysulfone aqueous solution (1 g / L), and spray 8 ml of the sulfonated polysulfone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.2 MPa by spraying, and keep it at room temperature for 10 minutes to ensure sufficient reaction.
[0050] (5) Rinse the membrane surface of the sample obtained in step (4) with deionized water for 1 min.
[0051] (6) Repeat steps (2) and (3) to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 1.5.
[0052] Example 3
[0053] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polysulfone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 80°C under a nitrogen atmosphere and the reaction was carried out for 12 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0054] (2) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.5 g / L polyethyleneimine aqueous solution is prepared. By spraying, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.2 MPa and maintained at room temperature for 10 minutes.
[0055] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0056] (4) Prepare a sulfonated polysulfone aqueous solution (1 g / L), and spray 8 ml of the sulfonated polysulfone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.2 MPa by spraying, and keep it at room temperature for 10 minutes to ensure sufficient reaction.
[0057] (5) Rinse the membrane surface of the sample obtained in step (4) with deionized water for 1 min.
[0058] (6) Repeat steps (2)(3)(4)(5) to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 2.0.
[0059] Example 4
[0060] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polysulfone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 80°C under a nitrogen atmosphere and the reaction was carried out for 12 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0061] (2) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.5 g / L polyethyleneimine aqueous solution is prepared. By spraying, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.2 MPa and maintained at room temperature for 10 minutes.
[0062] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0063] (4) Prepare a sulfonated polysulfone aqueous solution (1 g / L), and spray 8 ml of the sulfonated polysulfone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.2 MPa by spraying, and keep it at room temperature for 10 minutes to ensure sufficient reaction.
[0064] (5) Rinse the membrane surface of the sample obtained in step (4) with deionized water for 1 min.
[0065] (6) After repeating steps (2)(3)(4)(5), continue to repeat (2) and (3) to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 2.5.
[0066] Example 5
[0067] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polysulfone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 80°C under a nitrogen atmosphere and the reaction was carried out for 12 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0068] (2) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.5 g / L polyethyleneimine aqueous solution is prepared. By spraying, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.2 MPa and maintained at room temperature for 10 minutes.
[0069] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0070] (4) Prepare a sulfonated polysulfone aqueous solution (1 g / L), and spray 8 ml of the sulfonated polysulfone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.2 MPa by spraying, and keep it at room temperature for 10 minutes to ensure sufficient reaction.
[0071] (5) Rinse the membrane surface of the sample obtained in step (4) with deionized water for 1 min.
[0072] (6) Repeat steps (2)(3)(4)(5) twice to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 3.0.
[0073] Example 6
[0074] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polysulfone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 80°C under a nitrogen atmosphere and the reaction was carried out for 12 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0075] (2) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.3 g / L polyethyleneimine aqueous solution is prepared. By spraying, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.2 MPa and maintained at room temperature for 10 minutes.
[0076] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0077] (4) Prepare a sulfonated polysulfone aqueous solution (0.5 g / L), and spray 8 ml of the sulfonated polysulfone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.2 MPa by spraying, and keep it at room temperature for 10 minutes to ensure sufficient reaction.
[0078] (5) The sample obtained in step (4) was rinsed with deionized water for 1 minute to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 1.0.
[0079] Example 7
[0080] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polyetheretherketone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 80°C under a nitrogen atmosphere and the reaction was carried out for 12 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0081] (2) The cationic polyelectrolyte is commercial polyallylamine hydrochloride (Mw is 15,000), and a 0.5 g / L aqueous solution of polyallylamine hydrochloride is prepared. By spraying, 8 ml of the aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.2 MPa and maintained at room temperature for 10 minutes.
[0082] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0083] (4) Prepare a sulfonated polyetheretherketone aqueous solution (1 g / L), and spray 8 ml of the sulfonated polyetheretherketone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.2 MPa by spraying, and keep it at room temperature for 10 minutes to ensure sufficient reaction.
[0084] (5) Rinse the membrane surface of the sample obtained in step (4) with deionized water for 1 min.
[0085] (6) Repeat steps (2)(3)(4)(5) to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 2.0.
[0086] Example 8
[0087] (1) Preparation of anionic polyelectrolyte (rigid main chain): The dried polysulfone and concentrated sulfuric acid were added to a three-necked flask in sequence, and mechanically stirred at 40°C for 6 h until completely dissolved. The temperature was raised to 70°C under a nitrogen atmosphere and the reaction was carried out for 8 h. The reaction solution was poured into ice water, and the remaining acid was neutralized with sodium hydroxide to a pH of 7. The precipitated sodium sulfate was filtered out, and the filtrate was separated and purified using a dialysis membrane with a molecular weight cutoff of 2000 Da. The anionic polyelectrolyte solid was obtained from the dialyzate by freeze drying and set aside.
[0088] (2) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.5 g / L polyethyleneimine aqueous solution is prepared. By spraying, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane under a gas pressure of 0.3 MPa and maintained at room temperature for 15 minutes.
[0089] (3) Rinse the membrane surface of the sample obtained in step (2) with deionized water for 1 min.
[0090] (4) Prepare a sulfonated polysulfone aqueous solution (1 g / L), and spray 8 ml of the sulfonated polysulfone aqueous solution on the membrane obtained in step (3) at a gas pressure of 0.3 MPa by spraying, and keep it at room temperature for 15 minutes to ensure sufficient reaction.
[0091] (5) Rinse the membrane surface of the sample obtained in step (4) with deionized water for 1 min.
[0092] (6) Repeat steps (2)(3)(4)(5) to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 2.0.
[0093] Comparative Example 1
[0094] (1) The cationic polyelectrolyte is commercial polyethyleneimine (Mw is 25,000), and a 0.5 g / L polyethyleneimine aqueous solution is prepared. The spraying method is: under a gas pressure of 0.2 MPa, 8 ml of the polyethyleneimine aqueous solution is evenly sprayed on the surface of the ultrafiltration membrane and maintained at room temperature for 10 minutes.
[0095] (2) Rinse the membrane surface of the sample obtained in step (1) with deionized water for 1 min.
[0096] (3) The anionic polyelectrolyte is commercial sodium polystyrene sulfonate (Mw is about 70,000), and a 0.86 g / L sodium polystyrene sulfonate aqueous solution is prepared. By spraying, 8 ml of the sodium polystyrene sulfonate aqueous solution is evenly sprayed on the surface of the membrane obtained in step (2) under a gas pressure of 0.2 MPa, and maintained at room temperature for 10 minutes.
[0097] (4) Rinse the membrane surface of the sample obtained in step (3) with deionized water for 1 min.
[0098] (5) Repeat steps (1)(2)(3)(4) to obtain a polyelectrolyte loose nanofiltration membrane with an assembly layer number of 2.0.
[0099] Comparative Example 2
[0100] The difference from Example 1 is that in step (3), the sample surface obtained is sprayed with a crosslinking agent aqueous solution and allowed to stand for 5-20 minutes; in step (4), 8 ml of a sulfonated polysulfone aqueous solution is sprayed on the surface on which the crosslinking agent is sprayed. The crosslinking agent aqueous solution is a 0.05 mol / L succinaldehyde solution. The other preparation steps are exactly the same as in Example 1.
[0101] 2. Performance Test
[0102] Figure 1 is the pure water flux of Examples 1-8 and Comparative Examples 1-2. Figure 1 It can be seen that the embodiments of the present invention all have a relatively high pure water flux of 150-350 LMH, while the pure water flux of Comparative Examples 1-2 is relatively low.
[0103] Figure 2 The surface and cross-sectional scanning electron microscope images of Example 3 and Comparative Example 1 are shown. Figure 2 a) is flat and has many small holes, while the surface of the comparative example ( Figure 2 c) Relatively compact. The separation layer of Example 3 is relatively thin, with a thickness of only about 40 nanometers, while the separation layer of the comparative example is relatively thick, about 190 nanometers. This is mainly because the rigid anionic polyelectrolyte in the example causes a large steric hindrance to the reaction of the sulfonic acid group and the amine group, and the reaction amount of the anionic and cationic polyelectrolytes is small.
[0104] Figure 3 The maximum molecular weight cut-off and pore size distribution diagram of Example 3 and Comparative Example 1 are shown in FIG. Figure 3 It can be seen that the maximum molecular weight cutoff and the average pore size of Example 3 are greater than those of Comparative Example 1, and the separation layer structure of Example 3 is looser.
[0105] Figure 4 The separation performance of Example 3 and the comparative example for the mixture of Congo red / sodium chloride and Congo red / sodium sulfate. Compared with the comparative example 1, the water flux of Example 3 is about 4 times that of the comparative example, and has a higher permeability of sodium sulfate, and can efficiently intercept Congo red. The embodiment is a loose nanofiltration membrane material with high permeability.
[0106] Permeation and separation performance tests
[0107] The test method is as follows:
[0108] A cross-flow filtration device was used with a test temperature of 25°C, a pressure of 0.3 MPa, a dye concentration of 0.2 g / L, and a salt concentration of 1 g / L. Before the formal test, the membrane was pre-pressed for 30 minutes, and the produced water was collected for 10 minutes each time. The produced water volume was used to calculate the water flux, and the conductivity or absorbance of the produced water and feed liquid was used to calculate the retention rate of salt or dye.
[0109]
[0110] Where J is the water flux (L m -2 h -1 , LMH), Δt is the collection time (hour), ΔV is the water volume (L), A is the effective filtration area (m 2 ).
[0111]
[0112] Where R is the retention rate of salt or dye, C p is the conductivity or absorbance of the produced water, C f is the conductivity or absorbance of the feed solution.
[0113]
[0114] Where J is the water flux (LMH) and ΔP is the test pressure (bar).
[0115] The retention results of dyes and salts for the above Examples 1-5 and Comparative Example 1 are shown in Table 1. All tests were repeated three times, and the errors were all within a reasonable range.
[0116] Table 1 Retention rates of sodium chloride, sodium sulfate and Congo red, and pure water permeability
[0117]
[0118]
[0119] As shown in Table 1, Examples 1-8 all have lower sodium chloride and sodium sulfate interception rates and higher Congo red interception rates. This is mainly because sulfonated polysulfone has a rigid skeleton, intramolecular rotation potential, and the molecular chain is usually in a stretched and expanded state. Sodium polystyrene sulfonate has a flexible skeleton, intramolecular rotation potential, and the molecular chain is usually in a random curled shape. The benzene ring and low molecular weight in sulfonated polysulfone enhance its rigidity. On the one hand, the stacking of sulfonated polysulfone molecular chains easily produces a large free volume. On the other hand, the rigid skeleton bending of sulfonated polysulfone is limited to cause steric hindrance to the reaction between sulfonic acid groups and amine groups, thereby causing its molecular structure to be loose. Sodium polystyrene sulfonate has a flexible skeleton and a high-density sulfonic acid group. When it reacts with polyethyleneimine, the mutual entanglement between the molecular chains forms a dense molecular structure. So when the number of assembly layers is the same as 2.0, the salt interception rate and water flux of Comparative Example 1 are lower than those of Example 3. The use of a cross-linking agent can make the membrane structure more compact. Therefore, when the number of assembled layers is the same as 1.0, compared with Example 1, the salt and dye retention rates of Comparative Example 2 increase, and the pure water permeability decreases.
[0120] Finally, it should be noted that the above embodiments are only some preferred cases of the present invention and cannot be used to limit the present invention. The present invention is described in detail with reference to the embodiments, and those skilled in the art can make relevant technical modifications or replacements according to the records in the embodiments. Therefore, within the spirit and principles of the present invention, any equivalent modifications, replacements, improvements, etc. are within the scope of protection of the present invention.
Claims
1. A polyelectrolyte loose nanofiltration membrane with high permeation flux, characterized in that: The invention comprises an ultrafiltration membrane and a polyelectrolyte layer loaded on the surface thereof, wherein the polyelectrolyte layer is self-assembled by alternating cationic polyelectrolyte layers and anionic polyelectrolyte layers; wherein the cationic polyelectrolyte layer in the polyelectrolyte layer is loaded on the surface of the ultrafiltration membrane; The anionic polyelectrolyte layer is composed of anionic polyelectrolytes having a rigid main chain; The cationic polyelectrolyte layer is composed of a cationic polyelectrolyte having a flexible main chain; The pure water flux of the polyelectrolyte loose nanofiltration membrane is 150-350LMH.
2. The polyelectrolyte loose nanofiltration membrane with high permeation flux according to claim 1, characterized in that: The molecular weight cut-off of the ultrafiltration membrane is 100-200Kda; Preferably, the ultrafiltration membrane is one or more of a polysulfone ultrafiltration membrane, a polyethersulfone ultrafiltration membrane or a polyacrylonitrile ultrafiltration membrane.
3. The polyelectrolyte loose nanofiltration membrane with high permeation flux according to claim 1, characterized in that: The cationic polyelectrolyte is one or more of polyethyleneimine, polyacrylamide, polyvinyl alcohol, and polyallylamine hydrochloride cationic polyelectrolytes; Preferably, the average molecular weight of the polyethyleneimine is 20,000-30,000; The average molecular weight of polyallylamine hydrochloride is 10,000-20,000.
4. The polyelectrolyte loose nanofiltration membrane with high permeation flux according to claim 1, characterized in that: The anionic polyelectrolyte is one or more of sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, and sulfonated polyimide anionic polyelectrolyte.
5. A method for preparing a polyelectrolyte loose nanofiltration membrane with high permeation flux according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Spraying a cationic polyelectrolyte aqueous solution on the surface of an ultrafiltration membrane, leaving it to stand at room temperature, and then rinsing it with deionized water; (2) spraying an aqueous solution of anionic polyelectrolyte on the surface of the sample obtained in step (1), letting it stand at room temperature and then rinsing it with deionized water to obtain a polyelectrolyte loose nanofiltration membrane; (3) Repeat steps (1) and (2) to obtain a multilayer polyelectrolyte loose nanofiltration membrane.
6. The preparation method according to claim 5, characterized in that: In step (1), the concentration of the cationic polyelectrolyte is 0.3-1.5 g / L; the spraying pressure is 0.2-0.4 MPa; the standing time is 5-20 min; and the deionized water rinsing time is 1-5 min.
7. The preparation method according to claim 5, characterized in that: In step (2), the preparation method of the anionic polyelectrolyte is as follows: stirring and dissolving the raw materials and concentrated sulfuric acid, and reacting them under a nitrogen atmosphere; after the reaction is completed, pouring the reaction solution into ice water, neutralizing the remaining acid with sodium hydroxide, separating and purifying, and freeze-drying to obtain the anionic polyelectrolyte; the raw material is one of polysulfone, polyethersulfone, polyetheretherketone or polyimide; Preferably, the stirring and dissolving temperature is 30-40° C., and the stirring time is 6-8 h; the reaction temperature is 70-80° C., and the reaction time is 8-12 h.
8. The preparation method according to claim 5, characterized in that: In step (2), the concentration of the anionic polyelectrolyte is 0.3-1.5 g / L; the spraying pressure is 0.2-0.4 MPa; the standing time is 5-20 min; and the deionized water rinsing time is 1-5 min.
9. The preparation method according to claim 5, characterized in that: In step (3), the multi-layered polyelectrolyte loose nanofiltration membrane is composed of alternating anionic polyelectrolyte layers and cationic polyelectrolyte layers; The cationic polyelectrolyte layer in the polyelectrolyte layer is supported on the surface of the ultrafiltration membrane.
10. Use of the polyelectrolyte loose nanofiltration membrane with high permeability flux as claimed in any one of claims 1 to 4 in the selective separation of dyes and salts or in wastewater treatment; preferably, the salt comprises sodium chloride and sodium sulfate; the dye comprises Congo red; preferably, the wastewater is textile printing and dyeing wastewater.