Preparation method of ternary composite oxide and application of ternary composite oxide in low-temperature efficient photo-thermal catalytic oxidation of VOCs (Volatile Organic Compounds)

CuMgCe composite oxide was prepared by solution combustion and subjected to thermal or photothermal reduction treatment, which solved the problem of insufficient low-temperature catalytic activity of MgCe composite oxide, improved its catalytic performance and stability at low temperatures, and achieved efficient VOC removal at low temperatures effect.

CN119034753APending Publication Date: 2024-11-29HEBEI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411143018.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing MgCe composite oxides have insufficient catalytic activity at low temperatures, and have problems with high complete oxidation temperature, poor water resistance and stability. No photothermal catalytic study on efficient removal of VOCs at low temperatures has been found.

Method used

CuMgCe ternary composite oxide is prepared by solution combustion method, and thermal reduction or photothermal reduction pretreatment is performed before photothermal catalysis. By introducing CuO, the light absorption capacity and carrier separation efficiency of the catalyst are improved, and the X element is promoted from high valence state to Transfer of low-price states to increase oxygen vacancy content.

Benefits of technology

The catalytic activity and stability of CuMgCe composite oxide at low temperatures are improved, the degradation ability of VOCs is enhanced, and the photothermal catalytic oxidation effect at low temperatures is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034753A_ABST
    Figure CN119034753A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a ternary composite oxide and application of the ternary composite oxide to low-temperature efficient photo-thermal catalytic oxidation of VOCs, and belongs to the technical field of material synthesizing.The preparation method of the ternary composite oxide comprises the following steps that S1, magnesium nitrate hexahydrate, dextrose monohydrate, cerium nitrate hexahydrate and nitric acid X are mixed and heated to be combusted, and a solid product is obtained; s2, calcining the solid product to obtain an XMgCe ternary composite oxide; and S3, before the photo-thermal catalytic reaction, putting the ternary composite oxide into a quartz tube, and carrying out thermal reduction or photo-thermal reduction pretreatment. According to the scheme, the obtained ternary composite oxide is subjected to thermal reduction or photo-thermal reduction, so that the X element can be promoted to be transferred from a high valence state to a low valence state, the content of the low-valence-state X element in the composite oxide is increased, and meanwhile, the concentration of oxygen vacancies in the composite oxide is also increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material synthesis, and specifically relates to a method for preparing a ternary composite oxide and its application in low-temperature and high-efficiency photothermal catalytic oxidation of VOCs. Background Art

[0002] The emission of VOCs seriously threatens human health. Photothermal catalytic treatment of VOCs is generally considered to be a promising technology. However, the activity of most non-precious metal catalysts at low temperatures does not meet people's expectations. Therefore, it is very meaningful to study materials that can efficiently remove VOCs at low temperatures.

[0003] CeO2 is one of the important rare earth metal oxides. Nanostructured CeO2 has a large number of defects, which can serve as surface active catalytic sites. Therefore, CeO2 is often used as one of the active components of VOCs catalysis and is a widely used component or active phase in many redox catalytic processes.

[0004] However, due to the high price of rare earth metals, their large-scale application is limited. Researchers have tried to combine rare earth metals with other common cheap carriers, such as MgO, Al2O3 and molecular sieves to reduce their industrial demand. Among these carriers, MgO is more attractive to some extent due to its rich surface defects, excellent heat resistance and low price.

[0005] However, existing MgCe composite oxides still have problems such as high temperature required for complete oxidation, poor water resistance and stability. CuO has a narrow band gap, strong electron migration ability and excellent oxidation performance, and CuO has rich surface chemical properties, so it is often used in the treatment of VOCs. However, there are no reports on the research of MgCe composite oxides for low-temperature and efficient removal of VOCs by photothermal catalytic oxidation of VOCs.

[0006] In this scheme, CuMgCe ternary composite oxide is prepared by solution combustion method. In order to further improve the low-temperature and efficient catalytic oxidation activity of CuMgCe ternary composite oxide and obtain more low-cost active sites, this scheme specifically proposes to perform thermal reduction or photothermal reduction pretreatment on it. Summary of the invention

[0007] Therefore, the technical problem to be solved by the present invention is to overcome the defect of low catalytic activity of magnesium-cerium composite oxide in the prior art, thereby providing a method for preparing a ternary composite oxide.

[0008] The present invention also provides an application of a ternary composite oxide prepared by the preparation method in low-temperature and high-efficiency photothermal catalytic oxidation of VOCs.

[0009] To this end, the present invention provides the following technical solution, a method for preparing a ternary composite oxide, comprising the following steps:

[0010] S1, mixing magnesium nitrate hexahydrate, glucose monohydrate, cerium nitrate hexahydrate and nitric acid X and heating them to burn to obtain a solid product;

[0011] S2, calcining the solid product to obtain XMgCe ternary composite oxide;

[0012] S3, before performing the photothermal catalytic oxidation reaction, placing the ternary composite oxide in a quartz tube for thermal reduction or photothermal reduction pretreatment.

[0013] As a preferred embodiment, the element X is one or more of copper, cobalt, iron or nickel.

[0014] As a preferred solution, in step S3, the quartz tube is heated at a temperature of 200-350°C and thermally reduced for 3-5 hours in a hydrogen atmosphere.

[0015] As a preferred embodiment, in step S3, the quartz tube is irradiated and heated with a xenon lamp at a temperature of 200-350° C., and the photothermal reduction is performed for 0.25-1 hour in a hydrogen atmosphere.

[0016] As a preferred solution, during the heating process of the quartz tube, the heating rate is 1-10°C.

[0017] As a preferred solution, in step S2, the calcination temperature is 400-600°C, and the calcination time is 2-4 hours.

[0018] As a preferred embodiment, the element X is preferably copper.

[0019] As a preferred embodiment, the mass ratio of the magnesium nitrate hexahydrate, the cerium nitrate hexahydrate and the nitric acid X is: 2.56:3.256:(0-0.8).

[0020] The present invention also provides an application of a ternary composite oxide prepared by the method for preparing the ternary composite oxide as described above in low-temperature photothermal and efficient catalytic oxidation of VOCs.

[0021] The technical solution of the present invention has the following advantages:

[0022] 1. The present invention provides a method for preparing a ternary composite oxide. The introduction of CuO makes the MgCe composite oxide have strong light absorption ability, narrow band gap width, good carrier separation efficiency and low resistance value, improves the mobility of lattice oxygen, enhances the oxygen storage and release capacity in the low temperature zone, and is conducive to the increase of oxygen vacancy content.

[0023] 2. The present invention provides a method for preparing a ternary composite oxide, which can promote the transfer of element X from a high valence state to a low valence state by subjecting the obtained ternary composite oxide to thermal reduction or photothermal reduction before performing a photothermal catalytic oxidation reaction, thereby increasing the content of the low valence element X in the composite oxide, and also increasing the concentration of oxygen vacancies in the composite oxide.

[0024] In summary, increasing the number of low-valent metal ions and the concentration of oxygen vacancies can achieve low-temperature and efficient degradation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 XRD spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3 of the present invention;

[0027] Figure 2 Scanning electron microscopy (SEM), transmission electron microscopy (TEM) and Mapping of CMC-TR prepared in Example 2 of the present invention;

[0028] Figure 3 Scanning electron microscopy (SEM), transmission electron microscopy (TEM) and mapping of CMC-PTR prepared in Example 3 of the present invention;

[0029] Figure 4 The UV-visible diffuse reflectance spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Examples 1, 2 and 3 of the present invention;

[0030] Figure 5 The transient fluorescence spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Examples 1, 2 and 3 of the present invention;

[0031] Figure 6 The electrochemical impedance spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Examples 1, 2 and 3 of the present invention;

[0032] Figure 7Photocurrent response test of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3 of the present invention;

[0033] Figure 8 EPR spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3 of the present invention under (a) dark and (b) light conditions;

[0034] Fig. 9 The O2-TPD test spectrum of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3 of the present invention;

[0035] Fig.10 This is the toluene degradation activity diagram in Experimental Example 1 of the present invention;

[0036] Fig.11 This is the toluene degradation activity diagram in Experimental Example 2 of the present invention;

[0037] Fig.12 This is a stability diagram of the ternary composite oxidation in Experimental Example 3 of the present invention;

[0038] Fig.13 This is the toluene degradation activity diagram in Example 3 of the present invention;

[0039] Fig.14 It is the UV-visible diffuse reflectance spectra of the ternary composite oxides prepared in Example 6, Example 9 and Example 12 of the present invention. DETAILED DESCRIPTION

[0040] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0041] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0042] Example 1

[0043] Weigh 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.5680g of copper nitrate hexahydrate and 0.9900g of glucose monohydrate into a 250mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, calcine it at 500°C in an air atmosphere for 3 hours to obtain a ternary composite oxide CuMgCe, and name the ternary composite oxide CMC.

[0044] Example 2

[0045] Weigh 2.5600 g of magnesium nitrate hexahydrate, 3.2600 g of cerium nitrate hexahydrate, 0.5680 g of copper nitrate hexahydrate and 0.9900 g of glucose monohydrate into a 250 mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, calcine it at 500 ° C in an air atmosphere for 3 hours to obtain a ternary composite oxide CuMgCe;

[0046] Weigh 0.1 g of the above-mentioned ternary composite oxide and place it in a quartz tube. Heat it to 300°C at a rate of 10°C / min in an atmosphere of 10% hydrogen and 90% helium, and thermally reduce it in flowing hydrogen for 4 hours to obtain the thermally reduced ternary composite oxide CuMgCe-TR. The thermally reduced ternary composite oxide is named CMC-TR.

[0047] Example 3

[0048] Weigh 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.5680g of copper nitrate hexahydrate and 0.9900g of glucose monohydrate into a 250mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials are slowly melted into a solution, heat until burned to obtain a solid product, grind it thoroughly, place it in a muffle furnace, and calcine it at 500°C in an air atmosphere for 3 hours to obtain a ternary composite oxide CuMgCe;

[0049] 0.1 g of the above-mentioned ternary composite oxide was weighed and placed in a quartz tube. Under the irradiation of a 1.5 W double-sided xenon lamp light source, the temperature was raised to 300°C at a rate of 10°C / min in an atmosphere of 10% hydrogen and 90% helium, and photothermal reduction was carried out in flowing hydrogen for 0.5 hours to obtain the ternary composite oxide CuMgCe-PTR after photothermal reduction, and the ternary composite oxide after photothermal reduction was named CMC-PTR.

[0050] Figure 1The XRD spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3 show that the characteristic peaks of CMC, CMC-TR and CMC-PTR ternary composite oxides at 42.9° and 62.3° correspond to the (200) and (220) crystal planes of MgO (PDF#45-0946), and the characteristic peaks at 28.6°, 33.1°, 47.5° and 56.4° correspond to the (111), (200), (220) and (311) crystal planes of CeO2 (PDF#43-1002). By magnifying the XRD images, it is found that CMC-TR and CMC-PTR have a slight displacement at 42.9°, which is due to lattice distortion during hydrogen thermal or photothermal treatment.

[0051] Figure 2 The scanning electron microscope (SEM), transmission electron microscope (TEM) and mapping maps of the CMC-TR prepared in Example 2;

[0052] Figure 2 (a) is a scanning electron microscope (SEM) image, from which it can be seen that the CMC-TR catalyst exhibits a small number of pores and unevenly distributed mesopores. Figure 2 (b) is a transmission electron microscope (TEM) image. It is found that the lattice fringe spacing is 0.27nm, 0.31nm and 0.21nm, corresponding to the (200) and (111) crystal planes of CeO2 and the (200) crystal plane of MgO. Figure 2 (c) is the mapping map, from which we can see the uniform distribution of Cu, Mg, Ce, and O elements, proving the successful preparation of CMC-TR ternary composite oxide.

[0053] Figure 3 Scanning electron microscopy (SEM), transmission electron microscopy (TEM) and mapping of CMC-PTR prepared in Example 3;

[0054] Figure 3 (d) is a scanning electron microscope (SEM) image. From the image, we can see that CMC-PTR ternary composite oxide shows a large number of pores and unevenly distributed mesopores. Figure 3 (e) is a transmission electron microscope (TEM) spectrum. It is found that the lattice fringes are 0.27nm, 0.31nm and 0.21nm apart, corresponding to the (200) and (111) crystal planes of CeO and the (200) crystal plane of MgO. In addition, no lattice fringes corresponding to CuO are found, which is consistent with the results of XRD. Figure 3(f) is the mapping spectrum, from which we can see the presence of Cu element, and the uniform distribution of Cu, Mg, Ce, and O elements, proving the successful synthesis of CMC-PTR ternary composite oxide.

[0055] Figure 4 The UV-visible diffuse reflectance spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3 are shown. As can be seen from the figure, the maximum absorption band edge of CMC is concentrated at 200-600nm, and the maximum absorption band edge of CMC-TR and CMC-PTR is concentrated at 200-800nm. After hydrogen pure heat or photothermal reduction treatment, the light absorption capacity of the ternary composite oxide is improved.

[0056] Figure 5 The transient fluorescence spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3. As can be seen from the figure, the photogenerated carrier lifetimes of CMC, CMC-TR and CMC-PTR are 0.22, 0.21 and 0.23 ns, respectively. The photogenerated carrier lifetimes of the samples are extended after photothermal reduction treatment, which is beneficial to improving the photocatalytic performance of the ternary composite oxides.

[0057] Figure 6 The electrochemical impedance spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3. As can be seen from the figure, CMC has the largest arc inner diameter, indicating that it has the largest electron transfer impedance value, and CMC-PTR has the smallest arc inner diameter, that is, it has the smallest electronic impedance value.

[0058] Figure 7 Photocurrent response test of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3.

[0059] As can be seen from the figure, CMC-PTR has a stronger photocurrent response intensity than CMC-TR, indicating that after hydrogen photothermal treatment, the carrier separation efficiency of the ternary composite oxide is enhanced and the electron transfer capacity is enhanced. These results show that CMC-PTR has the smallest electron transfer resistance value and the largest carrier separation efficiency, which is consistent with the conclusions obtained from transient fluorescence.

[0060] Figure 8 EPR spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3 under dark conditions (a) and light conditions (b); In order to verify the effect of different reduction conditions on the oxygen vacancy concentration, electron paramagnetic resonance (EPR) tests were carried out on the ternary composite oxides. Figure 8 As shown in Figure 2, an obvious paramagnetic signal peak appears at g = 2.0005, which is attributed to the unpaired electrons generated by oxygen vacancies. Figure 8 It can be seen from (a) that CMC, CMC-TR and CMC-PTR can all produce a small amount of oxygen vacancies under dark conditions at room temperature. After the introduction of light, the oxygen vacancy concentration of the CMC sample did not change significantly, the oxygen vacancy concentration of the CMC-TR sample increased slightly, and the oxygen vacancy concentration of the CMC-PTR sample increased significantly. This shows that under hydrogen thermal conditions, hydrogen atoms can interact with adsorbed oxygen, surface lattice oxygen or bulk lattice oxygen on the catalyst, and while producing oxygen vacancies, it will also change the properties of the ternary composite oxide. Introducing light under hydrogen thermal conditions will increase the interaction between hydrogen atoms and the catalyst, prompting the generation of more oxygen vacancies.

[0061] Fig. 9 O2-TPD test spectra of CMC, CMC-TR and CMC-PTR ternary composite oxides prepared in Example 1, Example 2 and Example 3.

[0062] Depend on Fig. 9 As shown in the figure, three desorption peaks appeared on the desorption curves of CMC, CMC-TR and CMC-PTR, among which the peak detected near 100 to 300 °C can be explained as the desorption of chemically adsorbed oxygen, the peak observed between 300 and 600 °C can be attributed to surface lattice oxygen, and the peak appearing at 600 to 800 °C is assigned to bulk lattice oxygen. The first desorption signal peak appeared near 175 °C for CMC, the first desorption peak signal peak appeared near 150 °C for CMC-TR, and the first desorption peak signal peak was detected at about 140 °C for CMC-TPR, and the signal peak intensity gradually increased. It can be seen that CMC-PTR has the strongest activation ability for molecular oxygen, and CMC has the weakest activation ability.

[0063] Experimental Example 1

[0064] Air was introduced into the quartz tubes containing CMC prepared in Example 1, CMC-TR prepared in Example 2, and CMC-PTR prepared in Example 3, respectively. After the air was introduced, the tubes were irradiated with a xenon lamp, toluene was introduced, toluene was bubbled into the quartz tubes at 45 mL / min of argon, 40 mL / min of air flow was used to provide an oxygen source for the reactants, and 15 mL / min of argon was used as a balance gas. Toluene was bubbled into circulating water at 3°C ​​to produce a toluene concentration of 2500 ppm. The total flow rate through the catalyst bed was fixed at 100 mL / min, and the gas weight hourly space velocity (GHSV) was 60,000 mL·g -1 h -1 ,During the experiment, samples were taken and the toluene concentration data was detected by gas chromatograph.

[0065] Fig.10 This is the toluene degradation activity diagram in Experimental Example 1;

[0066] The conversion rate of ternary composite oxide CMC to 2500ppm toluene is only 10% at 100℃, and 50% at 150℃. The conversion rate of ternary composite oxide CMC-TR to 2500ppm toluene is more than 90% at 50℃, and the conversion rate of ternary composite oxide CMC-TPR to 2500ppm toluene is 95% at 50℃.

[0067] Experimental Example 2

[0068] Air was introduced into the quartz tubes containing CMC prepared in Example 1, CMC-TR prepared in Example 2, and CMC-PTR prepared in Example 3, respectively. After the air was introduced, the tubes were irradiated with a xenon lamp, toluene was introduced, and toluene was bubbled into the quartz tubes at 45 mL / min of argon gas, and an air flow of 40 mL / min provided an oxygen source for the reactants, and 15 mL / min of argon gas was used as a balance gas. Toluene was bubbled into circulating water at 3°C ​​to produce toluene concentrations of 100 ppm, 200 ppm, 300 ppm, 100 ppm, 400 ppm, 500 ppm, and 1000 ppm, respectively. The total flow rate through the catalyst bed was fixed at 100 mL / min, and the gas weight hourly space velocity (GHSV) was 60,000 mL·g -1 h -1 ,During the experiment, samples were taken and the toluene concentration data was detected by gas chromatograph.

[0069] Fig.11 This is the toluene degradation activity diagram in Experimental Example 2;

[0070] Experimental Example 2 compares the degradation activities of CMC, CMC-TR, and CMC-PTR on toluene of different concentrations (100-1000ppm). As can be seen from the figure, under the condition of a single-side light source, the conversion rate of CMC on low-concentration toluene is only about 40%, the conversion rate of CMC-TR on low-concentration toluene is about 60%, and the conversion rate of CMC-PTR on toluene reaches 95%. This fully demonstrates that CMC-PTR after photothermal reduction treatment can not only improve the activity of ternary composite oxides on high-concentration (2500ppm) toluene, but also further improve the activity of ternary composite oxides on low-concentration (100-1000ppm) toluene.

[0071] Experimental Example 3

[0072] Air was introduced into the quartz tubes containing the CMC-TR prepared in Example 2 and the CMC-PTR prepared in Example 3, respectively. After the air was introduced, the tubes were irradiated with a xenon lamp, toluene was introduced, and toluene was bubbled into the quartz tubes with 45 mL / min of argon gas, and an air flow of 40 mL / min provided an oxygen source for the reactants, and 15 mL / min of argon gas was used as a balance gas. Toluene was bubbled in circulating water at 3°C ​​to produce a toluene concentration of 2500 ppm, respectively. The total flow rate through the catalyst bed was fixed at 100 mL / min, the gas weight hourly space velocity (GHSV) was 60,000 mL·g-1h-1, and the experiment lasted for 70 hours. During the experiment, samples were taken and the toluene concentration data was detected by gas chromatograph.

[0073] Fig.12 12( a ) is the stability diagram of CMC-TR and 12( b ) is the stability diagram of CMC-PTR.

[0074] In order to evaluate the stability of CMC-TR and CMC-PTR ternary composite oxides, stability tests were conducted on them. It can be seen from the figure that in the 70h stability test, the toluene conversion rate of CMC-PTR ternary composite oxide did not decrease, and the toluene conversion rate at 72h was still 99.0%, while the toluene conversion rate of CMC-TR ternary composite oxide decreased at 38h, and the toluene conversion rate dropped to 92% at 72h. This shows that CMC-PTR ternary composite oxide has better stability than CMC-TR ternary composite oxide, which may be because hydrogen atoms in CMC-PTR ternary composite oxide are more likely to react with lattice oxygen, thereby producing more oxygen vacancies. In addition, from the Cu 2p The results show that CMC-PTR ternary composite oxide can produce more Cu + The presence of a large amount of low-valent Cu will promote the dissociation and activation of the surrounding oxygen atoms, producing more active oxygen to participate in the oxidation reaction of toluene.

[0075] Example 4 - Iron

[0076] Weigh 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.4747g of ferric nitrate nonahydrate and 0.9900g of glucose monohydrate into a 250mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, and calcine it at 600°C in an air atmosphere for 2 hours to obtain the ternary composite oxide FeMgCe.

[0077] Example 5 - Iron

[0078] Weigh 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.4747g of ferric nitrate nonahydrate and 0.9900g of glucose monohydrate into a 250mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, and calcine it at 600°C in an air atmosphere for 2 hours to obtain the ternary composite oxide FeMgCe.

[0079] 0.1 g of the above ternary composite oxide was weighed and placed in a quartz tube, heated to 200°C at a rate of 8°C / min in an atmosphere of 5% hydrogen and 95% helium, and thermally reduced in flowing hydrogen for 5 hours to obtain the thermally reduced ternary composite oxide FeMgCe-TR.

[0080] Example 6 - Iron

[0081] Weigh 2.5600 g of magnesium nitrate hexahydrate, 3.2600 g of cerium nitrate hexahydrate, 0.4747 g of ferric nitrate nonahydrate and 0.9900 g of glucose monohydrate into a 250 mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until burning to obtain a solid product, grind it thoroughly and place it in a muffle furnace, calcine it at 600 ° C in an air atmosphere for 2 hours to obtain a ternary composite oxide FeMgCe;

[0082] 0.1 g of the above-mentioned ternary composite oxide was weighed and placed in a quartz tube. Under the irradiation of a 1.5 W double-sided xenon lamp light source, the temperature was raised to 200°C at a rate of 8°C / min in an atmosphere of 10% hydrogen and 90% helium, and photothermally reduced in flowing hydrogen for 1 hour to obtain the photothermally reduced ternary composite oxide FeMgCe-PTR.

[0083] Example 7 - Cobalt

[0084] Take 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.3300g of cobalt nitrate trihydrate and 0.9900g of glucose monohydrate in a 250mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, calcine it at 400°C in an air atmosphere for 4 hours to obtain the ternary composite oxide CoMgCe.

[0085] Example 8 - Cobalt

[0086] Take 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.3300g of cobalt nitrate trihydrate and 0.9900g of glucose monohydrate in a 250mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, calcine it at 400°C in an air atmosphere for 4 hours to obtain the ternary composite oxide CoMgCe.

[0087] 0.1 g of the above ternary composite oxide was weighed and placed in a quartz tube, heated to 350° C. at a rate of 5° C. / min in a helium atmosphere, and thermally reduced in flowing hydrogen for 3.5 hours to obtain the thermally reduced ternary composite oxide CoMgCe-TR.

[0088] Example 9 - Cobalt

[0089] 2.5600 g of magnesium nitrate hexahydrate, 3.2600 g of cerium nitrate hexahydrate, 0.3300 g of cobalt nitrate trihydrate and 0.9900 g of glucose monohydrate were placed in a 250 mL beaker, and the beaker was placed in an electronic heating furnace. After the raw materials were slowly melted into a solution, they were stirred evenly, heated until burned to obtain a solid product, which was fully ground and placed in a muffle furnace. It was calcined at 400 ° C in an air atmosphere for 4 hours to obtain a ternary composite oxide CoMgCe;

[0090] 0.1 g of the above-mentioned ternary composite oxide was weighed and placed in a quartz tube. Under the irradiation of a 1.5 W double-sided xenon lamp light source, the temperature was raised to 350°C at a rate of 5°C / min in a helium atmosphere, and photothermally reduced in flowing hydrogen for 0.25 hours to obtain the ternary composite oxide CoMgCe-PTR after photothermally reduced.

[0091] Example 10 - Nickel

[0092] Take 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.3300g of nickel nitrate hexahydrate and 0.9900g of glucose monohydrate in a 250ml beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, calcine it at 550℃ in an air atmosphere for 3.5 hours to obtain a ternary composite oxide NiMgCe.

[0093] Experimental Example 11—Nickel

[0094] Take 2.5600g of magnesium nitrate hexahydrate, 3.2600g of cerium nitrate hexahydrate, 0.3300g of nickel nitrate hexahydrate and 0.9900g of glucose monohydrate in a 250mL beaker, place the beaker in an electronic heating furnace, stir evenly after the raw materials slowly melt into a solution, heat until combustion to obtain a solid product, grind it thoroughly and place it in a muffle furnace, calcine it at 550℃ in an air atmosphere for 3.5 hours to obtain a ternary composite oxide NiMgCe.

[0095] 0.1 g of the above ternary composite oxide was weighed and placed in a quartz tube, heated to 300° C. at a rate of 1° C. / min in an atmosphere of 10% hydrogen and 90% helium, and thermally reduced in flowing hydrogen for 4 hours to obtain the thermally reduced ternary composite oxide NiMgCe-TR.

[0096] Example 12 - Nickel

[0097] 2.5600 g of magnesium nitrate hexahydrate, 3.2600 g of cerium nitrate hexahydrate, 0.3300 g of nickel nitrate hexahydrate and 0.9900 g of glucose monohydrate were placed in a 250 mL beaker, and the beaker was placed in an electronic heating furnace. After the raw materials were slowly melted into a solution, they were stirred evenly, heated until burned to obtain a solid product, which was fully ground and placed in a muffle furnace. It was calcined at 550 ° C in an air atmosphere for 3.5 hours to obtain a ternary composite oxide NiMgCe;

[0098] 0.1 g of the above-mentioned ternary composite oxide was weighed and placed in a quartz tube. Under the irradiation of a 1.5 W double-sided xenon lamp light source, the temperature was raised to 320°C at a rate of 1°C / min in a helium atmosphere, and photothermally reduced in flowing hydrogen for 0.75 hours to obtain the photothermally reduced ternary composite oxide NiMgCe-PTR.

[0099] Experimental Example 4

[0100] Air was introduced into the quartz tubes containing the composite oxides prepared in Examples 4 to 12, and then irradiated with a xenon lamp. Toluene was introduced, and toluene was bubbled into the quartz tubes at 45 mL / min of argon. An air flow of 40 mL / min was used as an oxygen source for the reactants, and 15 mL / min of argon was used as a balance gas. Toluene was bubbled into circulating water at 3°C ​​to produce a toluene concentration of 2500 ppm. The total flow rate through the catalyst bed was fixed at 100 mL / min, and the gas weight hourly space velocity (GHSV) was 60,000 mL·g -1 h -1 ,During the experiment, samples were taken and the toluene concentration data was detected by gas chromatograph.

[0101] Fig.13 This is the toluene degradation activity diagram in Experimental Example 4;

[0102] As can be seen from the figure, the degradation rates of toluene of the prepared ternary composite oxides FeMgCe, CoMgCe and NiMgCe are improved after photoreduction and photothermal reduction. After the preparation of the ternary composite oxides, photoreduction or photothermal reduction can improve their activity before photothermal catalytic oxidation reaction, and it is universal for some elements.

[0103] Fig.14 The UV-visible diffuse reflectance spectra of the ternary composite oxides prepared in Example 6, Example 9 and Example 12 are shown. As can be seen from the figure, the prepared samples also have good absorption intensity in the visible light region.

[0104] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a ternary composite oxide, characterized in that: The following steps are involved: S1, mixing magnesium nitrate hexahydrate, glucose monohydrate, cerium nitrate hexahydrate and nitric acid X and heating them to burn to obtain a solid product; S2, calcining the solid product to obtain XMgCe ternary composite oxide; S3, before performing the photothermal catalytic oxidation reaction, placing the ternary composite oxide in a quartz tube for thermal reduction or photothermal reduction pretreatment.

2. The method for preparing the ternary composite oxide according to claim 1, characterized in that: The element X is one or more of copper, cobalt, iron or nickel.

3. The method for preparing the ternary composite oxide according to claim 1, characterized in that: In step S2, the calcination temperature is 400-600°C, and the calcination time is 2-4 hours.

4. The method for preparing the ternary composite oxide according to claim 1, characterized in that: In step S3, the quartz tube is heated at a temperature of 200-350° C. in a hydrogen atmosphere for thermal reduction for 3-5 hours.

5. The method for preparing the ternary composite oxide according to claim 1, characterized in that: In step S3, the quartz tube is irradiated with a xenon lamp and heated at a temperature of 200-350° C. in a hydrogen atmosphere for photothermal reduction for 0.25-1 hour.

6. The method for preparing the ternary composite oxide according to claim 4 or 5, characterized in that: During the heating process of the quartz tube, the heating rate is 1-10°C.

7. The method for preparing the ternary composite oxide according to claim 2, characterized in that: The element X is preferably copper.

8. The method for preparing the ternary composite oxide according to claim 1, characterized in that: The mass ratio of the magnesium nitrate hexahydrate, the cerium nitrate hexahydrate and the nitric acid X is: 2.56:3.256:(0-0.8).

9. Use of the ternary composite oxide prepared by the method for preparing the ternary composite oxide as claimed in any one of claims 1 to 8 in low-temperature and high-efficiency photothermal catalytic oxidation of VOCs.

10. The use of the low-temperature and high-efficiency photothermal catalytic oxidation of VOCs according to claim 9, characterized in that: The VOCs is toluene, and the concentration of toluene is 1500ppm-2500ppm.