Non-uniform solid solution strengthening and toughening ultrahigh-temperature composite ceramic and preparation method thereof
Through the non-uniform solid solution technology combining Poisson's ratio and particle size, the problems of insufficient toughness and poor density of low-temperature sintering caused by single-phase solid solution structure of ultra-high temperature ceramics during high-temperature sintering are solved, and high density and toughness are achieved. Ultra-high temperature composite ceramic preparation improves ablation resistance.
Patent Information
- Application Number
- CN202411265864.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
Existing ultra-high temperature ceramics are prone to form a single-phase solid solution structure when sintered at high temperatures, resulting in limited toughness improvement, and poor low-temperature sintering density, making it difficult to obtain ideal mechanical properties.
By using the combination of Poisson's ratio of powder and specific particle size ranges, combined with sintering aids, discharge plasma or hot press sintering process, non-uniform solid solution ultra-high temperature composite ceramics are prepared, and the powder composition and sintering conditions are controlled to achieve the goal of achieving the High density and toughness.
It has achieved the preparation of high-density non-uniform solid solution ultra-high temperature ceramics at low temperatures, and its toughness has been improved to 200% of traditional single-phase solid solution ceramics, and its resistance to ultra-high temperature ablation is improved.
Smart Images

Figure CN119038998A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ultra-high temperature ceramics, and relates to an ultra-high temperature composite ceramic strengthened by non-uniform solid solution and a preparation method thereof. Background Art
[0002] Ultrahigh temperature ceramics (UHTCs) composed of transition metal carbides, borides and nitrides have high melting point, corrosion resistance, high hardness and strength characteristics, and have great application potential in high-performance thermal protection systems for hypersonic vehicles and aero engines. However, due to the strong covalent bond characteristics, UHTCs have extremely low fracture toughness and cannot withstand complex mechanical loads such as impact stress and vibration. At present, the mechanical strengthening methods of UHTCs are mainly divided into fiber / second phase toughening and solid solution strengthening. The pinning of fibers / second phases in ceramics achieves a grain refinement effect, while causing local internal stress inhomogeneity; cracks can form complex extension paths when they extend, achieving more energy dissipation, and thus obtaining higher toughness. A series of composite ceramics such as Cf / HfC-SiC and ZrB2-SiC have been studied in depth. For the solid solution strengthening method, the lattice distortion effect produced by the multi-component single-phase solid solution significantly improves the hardness and strength, and under the synergistic effect of the components, it also exhibits stronger high-temperature ablation resistance, oxidation resistance, corrosion resistance and wear resistance. For example, Hf-Ta-C single-phase ceramics have stronger ultra-high temperature ablation resistance than pure binary HfC and TaC ceramics. This is attributed to the ultra-high melting point (Ta 0.8 Hf 0.2 C is 4215K), and on the other hand, it is attributed to the low thermal conductivity HfO2-Ta2O5 composite oxide produced after high-temperature oxidation of Hf-Ta-C single-phase ceramics. However, the composition and structure of this type of single-phase solid solution material are too uniform, and there is a lack of effective crack propagation barriers in the material when the crack propagates, so the toughness cannot be improved. Therefore, a potential toughening method is to accurately control the solid solution level of ultra-high temperature ceramics and form a complex multiphase structure through low-temperature sintering to indirectly improve the toughness.
[0003] At present, spark plasma sintering and hot pressing sintering are the mainstream technologies for preparing multi-element ultra-high temperature ceramics. However, due to the high melting point characteristics of ultra-high temperature ceramics, the sintering temperature required for complete densification of ceramics under this process usually needs to be above 2000°C. This means that when the theoretical equilibrium solid solubility between the raw materials of ultra-high temperature ceramics is too high (≥50% at 1800°C), due to the high sintering temperature and long sintering time, it is very easy to form a single-phase solid solution structure of ceramics, and the further improvement of ceramic toughness is limited; while low-temperature sintering (sintering temperature ≤1800°C) can slow down the mutual diffusion of elements in ceramics, but the density of the obtained ceramics is poor, and the ideal mechanical properties cannot be obtained. Therefore, it is an urgent problem to find a method for preparing fully densified non-uniform solid solution ultra-high temperature composite ceramics at low temperature. Summary of the invention
[0004] In view of this, an object of the present invention is to provide an ultra-high temperature composite ceramic with non-uniform solid solution strengthening and toughening. A second object is to provide a method for preparing the ultra-high temperature composite ceramic.
[0005] To achieve the above-mentioned object, the first aspect of the present invention provides a fully densified non-uniform solid solution strengthened ultra-high temperature composite ceramic:
[0006] The ultra-high temperature composite ceramic with inhomogeneous solid solution strengthening and toughening uses at least two transition metal carbides, borides or nitrides as initial powders. After sintering, the initial powders include a first type of sintered powder and a second type of sintered powder, the first type of sintered powder has a Poisson's ratio of less than 0.25, the second type of sintered powder has a Poisson's ratio of greater than 0.25, and a sintering aid.
[0007] Furthermore, the tough powder accounts for 10 mol% to 90 mol% of the total molar percentage of the two types of sintered powders.
[0008] Furthermore, the transition metal is selected from Hf, Ta, Zr, W, Ti, Nb metal elements, and the sintering aid is selected from SiC, MoSi2, Ta, W, SiO2, ZrO2, HfO2, Hf6Ta2O 17 At least one of .
[0009] Furthermore, the inhomogeneous solid solution strengthened ultra-high temperature composite ceramics use HfC and TaC as initial powders.
[0010] The second aspect of the present invention provides a method for preparing an ultra-high temperature composite ceramic with inhomogeneous solid solution toughening, comprising the following specific steps:
[0011] S1: taking at least two kinds of transition metal carbides, borides or nitrides as initial powders; sintering them in a high-temperature atmosphere sintering furnace to obtain sintered powders; the sintered powders are respectively a first type of sintered powder and a second type of sintered powder, the first type of sintered powder has a Poisson's ratio of less than 0.25, and the second type of sintered powder has a Poisson's ratio of greater than 0.25;
[0012] S2: crushing and screening the first type sintering powder and the second type sintering powder respectively, screening them into coarse powder with a particle size of 35-120 μm and fine powder with a particle size of 0.1-6.5 μm; and then adding sintering aids;
[0013] S3: Mix the powders evenly without destroying the initial particle size of the powders, and then dry and stir to mix evenly after mixing;
[0014] S4: sintering the mixed powder of step S3 to obtain a non-uniform solid solution multi-component ultra-high temperature composite ceramic, wherein the sintering is spark plasma sintering or hot pressing sintering.
[0015] Furthermore, the sintering condition in step S1 of the preparation method is that the vacuum degree in the furnace is ≤8.0×10 -3 Pa, sintering temperature 1600~2000℃, sintering time 3-12h.
[0016] Furthermore, in step S2 of the preparation method, the content of the fine powder is 10wt%-90wt% of the mass ratio of the single type of sintering powder, and the amount of sintering aid added is less than 10Vol% of the theoretical sum of the two types of sintering powder.
[0017] Furthermore, in step S3 of the preparation method, the powders are mixed uniformly by wet planetary ball milling, wet ultrasonic vibration or mechanical stirring.
[0018] Furthermore, the vacuum degree in the sintering furnace in step S4 of the preparation method is ≤8.0×10 -3 Pa, sintering temperature 1600-1900℃.
[0019] Furthermore, in step S4 of the preparation method, an axial pressure of 30 MPa to 60 MPa is applied to the mixed powder.
[0020] Furthermore, before heating in step S4 of the preparation method, the method further includes continuously introducing an inert gas into the vacuum chamber, and controlling the atmosphere pressure to be 0.4-2Pa.
[0021] Compared with the prior art, the beneficial technical effect of the present invention is that the mixing conditions and specific particle size of the sintered powder are limited by using powders with different Poisson's ratios, which provides a preliminary basis for non-uniform solid solution; the requirements for powder composition and high equilibrium solid solubility are met to ensure the generation of high-density crack deflection behavior, thereby improving toughness. In prior art research, if the raw material powder presents a high equilibrium solid solubility, it is made into a more brittle single-phase solid solution material, while the present invention achieves non-uniform solid solution by using powders with different Poisson's ratio ranges and proportioning them into a controllable particle size range.
[0022] Moreover, by using powders with large differences in particle size as raw materials, the use of sintering aids can be minimized, and low-temperature preparation of high-density or even completely dense non-uniform solid solution ultra-high temperature ceramics can be achieved; the obtained ultra-high temperature composite ceramics have better toughness than traditional single-phase solid solution ceramics of the same component without excessively weakening the hardness, and the toughening effect can reach up to 200%. Since only a low content of sintering aids is added, it is more conducive to the improvement of ultra-high temperature ablation resistance. The ultra-high temperature composite ceramics of the present invention and the preparation method thereof have a wide range of applications. As long as the mutual solid solubility of the components is high enough and large-particle powders with complete structures can be achieved, non-uniform solid solution sintering can be achieved; the ultra-high temperature composite ceramic process has good repeatability, and the degree of solid solution can be precisely controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0024] Figure 1 This is the backscattered electron microscopy morphology of HfC-TaC-HfO2 composite ceramics after spark plasma sintering densification;
[0025] Figure 2 This is the XRD diffraction result of HfC-TaC-HfO2 composite ceramics;
[0026] Figure 3 This is the EDS element surface distribution result of HfC-TaC-HfO2 composite ceramics;
[0027] Figure 4 The surface morphology of HfC-TaC-HfO2 composite ceramics after Vickers indentation test;
[0028] Figure 5 The crack propagation characteristics of HfC-TaC-HfO2 composite ceramics in Vickers indentation test;
[0029] Figure 6 The fracture toughness and hardness of HfC-TaC-HfO2 composite ceramics are compared with other similar ceramics. DETAILED DESCRIPTION
[0030] The preferred embodiment of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The experimental methods for which specific conditions are not specified in the embodiments are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0031] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0032] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0033] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0035] The present invention provides a non-uniform solid solution ultra-high temperature composite ceramic and a preparation method thereof, the preparation method comprising the following steps:
[0036] S1: Take at least two kinds of transition metal carbides, borides or nitrides as initial powders; sinter them in a high-temperature atmosphere sintering furnace to obtain sintered powders: the vacuum degree in the furnace is ≤8.0×10 -3Pa, sintering temperature 1600 ~ 2000 ℃, sintering time 3-12h; sintered powders are divided into first-class sintered powders and second-class sintered powders, wherein the first-class sintered powders require a Poisson's ratio less than 0.25, defined as brittle powders, and the second-class sintered powders require a Poisson's ratio greater than 0.25, defined as tough powders;
[0037] Preferably, inert Ar gas is continuously introduced into the vacuum chamber, and the atmosphere pressure is controlled at 1.6-10 Pa; then the initial powder is heated and sintered;
[0038] Preferably, the sintering temperature is 1800° C. and the sintering time is 5-10 hours.
[0039] More preferably, the sintering temperature is 1800° C. and the sintering time is 5 hours.
[0040] Preferably, the Poisson's ratio of the sintered powder can be obtained through calculation theory design, or through conventional experimental testing.
[0041] Computational theoretical design constructs a unit cell calculation model by regulating the design composition and fitting the ceramic crystal structure. The theoretical mechanical properties and Poisson's ratio of the ceramic are obtained through first-principles calculations. The calculation model contains 16 to 256 atoms, and metal elements occupy the cation sublattice positions in the model in a disordered manner. The calculation can use VASP and CASTEP software, or deep learning and high-throughput calculations to obtain the composition that meets the Poisson's ratio requirements.
[0042] Preferably, the raw materials obtained by the calculation theory design can be subjected to nanoindentation testing on the sintered powder after sintering to obtain the experimental Poisson's ratio and ensure that the sintered powder meets the Poisson's ratio requirements.
[0043] Preferably, the initial powder particle size is 50nm-20μm.
[0044] The transition metal is selected from Hf, Ta, Zr, W, Ti, and Nb metal elements.
[0045] Preferred starting powders are HfC and TaC.
[0046] S2: Crushing and screening the brittle powder and the tough powder respectively, and screening them into coarse powder with a particle size of 35-120μm and fine powder with a particle size of 0.1-6.5μm; then adding sintering aids, the tough powder accounts for 10mol%-90mol% of the total molar percentage of the two types of sintering powders, and the remainder is brittle powder. The content of fine powder is 10wt%-90wt% of the mass ratio of a single type of sintering powder, and the remainder is coarse powder. The amount of sintering aid added is less than 10Vol% of the theoretical volume sum of the two types of sintering powders.
[0047] Preferably, the content of fine powder is 40wt%-70wt% of the mass ratio of a single type of sintered powder, and the remainder is coarse powder.
[0048] Preferably, the amount of the sintering aid added is less than 5 Vol% of the sum of the theoretical volumes of the two types of sintering powders.
[0049] The powder after crushing and screening is a non-agglomerated powder with complete structure.
[0050] The sintering aid is selected from SiC, MoSi2, Ta (tantalum), W (tungsten), SiO2, ZrO2, HfO2, Hf6Ta2O 17 At least one of;
[0051] Preferably, the particle size of the sintering aid is 0.5-80 μm.
[0052] S3: Mix the powders evenly without destroying the initial particle size of the powders. The mixing process may be wet planetary ball milling, wet ultrasonic vibration or mechanical stirring. After mixing evenly, dry and stir to mix evenly.
[0053] In some of the embodiments, the drying may be performed by vacuum drying, the drying temperature is 80° C.-100° C., and the vacuum degree is less than 0.1 Pa; the dry powder is stirred and mixed and the final mixing is completed by dry mechanical stirring.
[0054] Preferably, the wet medium in wet planetary ball milling is ethanol, and the ball mill speed is 50 rpm; ethanol accounts for 15-40 Vol% of the total mass ratio of balls, materials and medium to reduce the damage to particles by ball milling and ensure that ball milling or vibration stirring only plays a mixing role.
[0055] S4: Sintering the mixed powder of step S3 by spark plasma sintering or hot pressing sintering to obtain a non-uniform solid solution multi-element ultra-high temperature composite ceramic;
[0056] The spark plasma sintering process comprises the following steps:
[0057] S4a: Place the mixed powder processed by S3 evenly in a mold. The mold material is graphite. The internal size of the mold is
[0058] Diameter 10mm-50mm;
[0059] S4b: Place the graphite abrasive tool of S4a in a spark plasma sintering device and evacuate the vacuum chamber to a vacuum degree of ≤8.0×10 -3 Pa;
[0060] Optionally, an inert gas is continuously introduced into the vacuum chamber, and the atmosphere pressure is controlled at 0.4-2Pa.
[0061] Optionally, the inert gas is Ar gas.
[0062] S4c: Apply 30MPa to 60MPa axial pressure to the graphite abrasive tool;
[0063] S4d: Turn on the heating power supply, sintering heating rate 50-100℃ / min, sintering temperature 1600-1900℃, pulse electric
[0064] Flow 1000-3000A, insulation time 20-120min;
[0065] S4e: After sintering is completed, the furnace is cooled to room temperature and taken out to obtain a non-uniform solid solution multi-element ultra-high temperature composite ceramic.
[0066] Or the hot pressing sintering process comprises the following steps:
[0067] S4a: Place the mixed powder processed by S3 evenly in a mold. The mold material is graphite. The internal size of the mold is
[0068] Diameter 10mm-50mm;
[0069] S4b: Place the graphite abrasive tool of S4a in a hot pressing sintering device and evacuate the vacuum chamber to a vacuum degree of ≤8.0×10 -3 Pa; then inert Ar gas is continuously introduced into the vacuum chamber, and the atmosphere pressure is controlled at 1Pa;
[0070] S4c: Apply 30MPa to 60MPa axial pressure to the graphite abrasive tool;
[0071] S4d: Turn on the heating power supply, sintering heating rate 10℃ / min, sintering temperature 1600-1900℃, holding time 2h;
[0072] S4e: After sintering is completed, the furnace is cooled to room temperature and taken out to obtain a non-uniform solid solution multi-element ultra-high temperature composite ceramic.
[0073] Example 1
[0074] A method for preparing a non-uniform solid solution HfC-TaC-HfO2 ultra-high temperature composite ceramic comprises the following steps:
[0075] S1: Take HfC (hafnium carbide, CAS: 12069-85-1) and TaC (tantalum carbide) powders as initial powders, sinter them in a high-temperature atmosphere sintering furnace to obtain sintered powders: the vacuum degree in the furnace is ≤8.0×10 -3 Pa, sintering temperature 1800℃, sintering time 5h.;
[0076] The initial powder particle size is 50nm-20μm. The theoretical equilibrium solid solubility of HfC-TaC at 1800℃ is continuous solid solution.
[0077] After sintering, the obtained HfC sintered powder has a Poisson's ratio of less than 0.25, which is a brittle powder, and the TaC sintered powder has a Poisson's ratio of greater than 0.25, which is a tough powder.
[0078] S2: Crush and screen the HfC sintered powder and TaC sintered powder, screen out the HfC sintered powder and TaC sintered powder that can pass through the 300-mesh sieve but not the 500-mesh sieve to obtain coarse powder; screen out the sintered powder and TaC sintered powder that pass through the 3000-mesh sieve to obtain fine powder; then add sintering aid HfO2 powder, wherein the molar ratio of HfC to TaC is 1:1, the mass ratio of coarse powder to fine powder in each sintering powder is 4:6, and the added amount of sintering aid HfO2 is 5Vol% of the theoretical volume sum of the two types of sintering powders, and the average particle size is 800 mesh.
[0079] S3: Without destroying the initial particle size of the powder, all the powders in step S2 are mixed uniformly by wet planetary ball milling, the wet medium is ethanol, and the ball mill speed is 50rpm; after mixing uniformly, they are dried in a vacuum dryer at a drying temperature of 80°C and a vacuum degree of less than 0.1Pa; then the dried powders are finally mixed by dry mechanical stirring.
[0080] S4: Sintering the mixed powder after the treatment in step S3 by spark plasma sintering process to obtain a non-uniform solid solution HfC-TaC-HfO2 ultra-high temperature composite ceramic, wherein the sintering process comprises the following steps:
[0081] S4a: Place the mixed powder processed by S3 evenly in a mold. The mold material is graphite. The internal size of the mold is
[0082] Diameter 20mm;
[0083] S4b: The graphite grinding tool of S4a is placed in a spark plasma sintering device, and the vacuum chamber is evacuated.
[0084] Emptyness≤8.0×10 -3 Pa;
[0085] S4c: applying 45 MPa axial pressure to the graphite abrasive tool;
[0086] S4d: Turn on the heating power supply, sintering heating rate 100℃ / min, sintering temperature 1800℃, pulse current 1500A, holding time 30min;
[0087] S4e: After sintering, the mixture is cooled to room temperature in the furnace and taken out to obtain a non-uniform solid solution HfC-TaC-HfO2 ultra-high temperature composite ceramic.
[0088] Example 2
[0089] A non-uniform solid solution ZrC-TiC-Hf6Ta2O 17 The preparation method of ultra-high temperature composite ceramics comprises the following steps:
[0090] S1: Take ZrC (zirconium carbide) and TiC (titanium carbide) powders as initial powders and sinter them in a high-temperature atmosphere sintering furnace to obtain sintered powders: the vacuum degree in the furnace is ≤7.0×10 -3 Pa, sintering temperature 1700℃, sintering time 4h.;
[0091] The initial powder particle size is 50nm-20μm.
[0092] After sintering, the Poisson's ratio of the obtained ZrC sintered powder is less than 0.25, which is a brittle powder, and the Poisson's ratio of the TiC sintered powder is greater than 0.25, which is a tough powder.
[0093] S2: crush and screen the ZrC sintered powder and TiC sintered powder, sieve out the ZrC sintered powder and TiC sintered powder that can pass through the 100-mesh sieve but not the 300-mesh sieve to obtain coarse powder; sieve out the ZrC and TiC powders that pass through the 2000-mesh sieve to obtain fine powder; then add the sintering aid Hf6Ta2O 17 The molar ratio of ZrC to TiC in the sintered powder is 6:4, the mass ratio of coarse powder to fine powder is 5:5, and the sintering aid Hf6Ta2O 17 The addition amount is 8Vol% of the theoretical volume of the two types of sintered powders, and the average particle size is 600 mesh;
[0094] S3: Without destroying the initial particle size of the powder, all the powders in step S2 are mixed uniformly by wet ultrasonic vibration stirring, the wet medium is ethanol, the ultrasonic frequency is 20kHz, and the stirrer speed is 50rpm; after mixing uniformly, they are dried in a vacuum dryer, the drying temperature is 100°C, and the vacuum degree is less than 0.1Pa; then the dried powder is finally mixed by dry mechanical stirring.
[0095] S4: Sintering the mixed powder after step S3 by spark plasma sintering to obtain ZrC-TiC-Hf6Ta2O 17 Ultra-high temperature composite ceramics, the sintering process comprises the following steps:
[0096] S4a: Place the mixed powder processed by S3 evenly in a mold. The mold material is graphite. The internal size of the mold is
[0097] Diameter 20mm;
[0098] S4b: The graphite grinding tool of S4a is placed in a spark plasma sintering device, and the vacuum chamber is evacuated.
[0099] Emptyness≤8.0×10 -3 Pa;
[0100] S4c: applying 50 MPa axial pressure to the graphite abrasive tool;
[0101] S4d: Turn on the heating power supply, sintering heating rate 80℃ / min, sintering temperature 1700℃, pulse current 1000A, holding time 30min;
[0102] S4e: After sintering, the furnace is cooled to room temperature and taken out to obtain a non-uniform solid solution ZrC-TiC-Hf6Ta2O 17 Ultra-high temperature composite ceramics.
[0103] Example 3
[0104] A non-uniform solid solution (Zr,Hf)C-(Ti,Ta)C-Hf6Ta2O 17 Ultra-high temperature composite ceramic and preparation method thereof, characterized in that it comprises the following steps:
[0105] S1: Select ZrC, TiC, HfC, and TaC with a particle size of 50 nm-20 μm as the initial powders, and sinter the ZrC-HfC powder and TiC-TaC powder in a high-temperature atmosphere sintering furnace to obtain sintered powders: the vacuum degree in the furnace is ≤7.0×10 -3 Pa, sintering temperature 1800℃, sintering time 5h.;
[0106] After sintering, the obtained (Zr, Hf)C sintered powder has a Poisson's ratio of less than 0.25, which is a brittle powder, and the (Ti, Ta)C sintered powder has a Poisson's ratio of greater than 0.25, which is a tough powder.
[0107] S2: The (Zr, Hf) C sintered powder and (Ti, Ta) C sintered powder are crushed and screened respectively, and the (Zr, Hf) C sintered powder and (Ti, Ta) C sintered powder that can pass through the 100-mesh sieve but cannot pass through the 300-mesh sieve are screened out to obtain coarse powder; the (Zr, Hf) C sintered powder and (Ti, Ta) C sintered powder that pass through the 2000-mesh sieve are screened out to obtain fine powder; and a sintering aid Hf6Ta2O is added. 17 The molar ratio of (Zr, Hf) C and (Ti, Ta) C in the sintered powder is 6:4, the mass ratio of coarse powder to fine powder is 5:5, and the sintering aid Hf6Ta2O 17The addition amount is 5Vol% of the theoretical volume of the two types of sintered powders, and the average particle size is 600 mesh;
[0108] S3: Without destroying the initial particle size of the powder, all the powders in step S2 are mixed uniformly by wet ultrasonic vibration stirring, the wet medium is ethanol, the ultrasonic frequency is 20kHz, and the stirrer speed is 50rpm; after mixing uniformly, they are dried in a vacuum dryer, the drying temperature is 100°C, and the vacuum degree is less than 0.1Pa; then the dried powder is finally mixed by dry mechanical stirring.
[0109] S4: Sintering the mixed powder after the treatment in step S3 by spark plasma sintering to obtain (Zr, Hf)C-(Ti, Ta)C-Hf6Ta2O 17 Ultra-high temperature composite ceramics, the sintering process comprises the following steps:
[0110] S4a: Place the mixed powder processed by S3 flatly in a grinding tool, the material of the grinding tool is graphite, and the inner size of the grinding tool has a diameter of 20 mm;
[0111] S4b: Place the graphite abrasive tool of S4a in a spark plasma sintering device and evacuate the vacuum chamber to a vacuum degree of ≤8.0×10 -3 Pa;
[0112] S4c: applying 50 MPa axial pressure to the graphite abrasive tool;
[0113] S4d: Turn on the heating power supply, sintering heating rate 80℃ / min, sintering temperature 1800℃, pulse current 1000A, holding time 20min;
[0114] S4e: After sintering, the furnace is cooled to room temperature and taken out to obtain a non-uniform solid solution (Zr, Hf)C-(Ti, Ta)C-Hf6Ta2O 17 Ultra-high temperature composite ceramics.
[0115] Example 4
[0116] A non-uniform solid solution (Zr,Hf)C-(Ti,Ta)C-Hf6Ta2O 17 Ultra-high temperature composite ceramic and preparation method thereof, characterized in that it comprises the following steps:
[0117] Steps S1 to S3 are the same as those in Example 3. Step S4 uses a hot pressing sintering process to sinter the mixed powder treated in step S3 to obtain (Zr, Hf)C-(Ti, Ta)C-Hf6Ta2O 17 Ultra-high temperature composite ceramics, the specific sintering process is as follows:
[0118] S4a: Place the mixed powder processed by S3 flatly in a grinding tool, the material of the grinding tool is graphite, and the inner size of the grinding tool has a diameter of 20 mm;
[0119] S4b: Place the graphite abrasive tool of S4a in a hot pressing sintering device and evacuate the vacuum chamber to a vacuum degree of ≤8.0×10 -3 Pa; then inert Ar gas is continuously introduced into the vacuum chamber, and the atmosphere pressure is controlled at 1Pa;
[0120] S4c: applying 50 MPa axial pressure to the graphite abrasive tool;
[0121] S4d: Turn on the heating power, sintering heating rate 10℃ / min, sintering temperature 1800℃, holding time 2h;
[0122] S4e: After sintering, the furnace is cooled to room temperature and taken out to obtain a non-uniform solid solution (Zr, Hf)C-(Ti, Ta)C-Hf6Ta2O 17 Ultra-high temperature composite ceramics.
[0123] Example 5
[0124] The non-uniform solid solution HfC-TaC-HfO2 ultra-high temperature composite ceramic prepared in Example 1 was subjected to structural component characteristic analysis and mechanical property testing. The results are as follows: Figures 1 to 5 shown. Figure 1 The backscattered electron microscope morphology of the inhomogeneous solid solution HfC-TaC-HfO2 ultra-high temperature composite ceramic reflects a dense and complex multiphase structure. The ceramic density is ≥95%. The metal elements contained in the ultra-high temperature ceramic are unevenly distributed, and the solid solubility between the ceramic raw materials is less than the theoretical equilibrium solid solubility at the sintering preparation temperature. Figure 2 This is the XRD diffraction result of ultra-high temperature composite ceramics; Figure 3 The EDS element surface distribution results reflect the inhomogeneous solid solution characteristics of ultra-high temperature composite ceramics; Figure 4 The surface morphology of ultra-high temperature composite ceramics after Vickers indentation test: Figure 5 This is the crack propagation characteristics of ultra-high temperature composite ceramics in the Vickers indentation test. It can be seen that the complex phase structure enhances the crack deflection path. Figure 6 This is a lateral comparison result of the fracture toughness and hardness of the ultra-high temperature composite ceramic of the present invention with other similar ceramics, where the label This work is HfC-TaC-HfO2 of the present invention. It can be seen that compared with the single-phase solid solution Hf-Ta-C material, the non-uniform solid solution mechanism doubles the toughness of the ceramic.
[0125] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. Ultra-high temperature composite ceramics with non-uniform solid solution toughening, characterized in that: At least two transition metal carbides, borides or nitrides are used as initial powders. After sintering, the initial powders include a first type of sintered powder and a second type of sintered powder. The Poisson's ratio of the first type of sintered powder is less than 0.25, and the Poisson's ratio of the second type of sintered powder is greater than 0.25, as well as a sintering aid.
2. The ultra-high temperature composite ceramic with non-uniform solid solution toughening according to claim 1, characterized in that: The tough powder accounts for 10 mol% to 90 mol% of the total molar percentage of the two types of sintered powders.
3. The ultra-high temperature composite ceramic with non-uniform solid solution toughening according to claim 1, characterized in that: The transition metal is selected from Hf, Ta, Zr, W, Ti, Nb metal elements, and the sintering aid is selected from SiC, MoSi2, Ta, W, SiO2, ZrO2, HfO2, Hf6Ta2O 17 At least one of .
4. The method for preparing the ultrahigh temperature composite ceramic according to any one of claims 1 to 3, characterized in that: The specific steps include: S1: taking at least two kinds of transition metal carbides, borides or nitrides as initial powders; sintering them in a high-temperature atmosphere sintering furnace to obtain sintered powders; the sintered powders are respectively a first type of sintered powder and a second type of sintered powder, the first type of sintered powder has a Poisson's ratio of less than 0.25, and the second type of sintered powder has a Poisson's ratio of greater than 0.25; S2: crushing and screening the first type sintering powder and the second type sintering powder respectively, screening them into coarse powder with a particle size of 35-120 μm and fine powder with a particle size of 0.1-6.5 μm; and then adding sintering aids; S3: Mix the powders evenly without destroying the initial particle size of the powders, and then dry and stir to mix evenly after mixing; S4: sintering the mixed powder of step S3 to obtain a non-uniform solid solution multi-component ultra-high temperature composite ceramic, wherein the sintering is spark plasma sintering or hot pressing sintering.
5. The method for preparing the ultrahigh temperature composite ceramic according to claim 4, characterized in that: In step S1, the sintering condition is that the vacuum degree in the furnace is ≤8.0×10 -3 Pa, sintering temperature 1600~2000℃, sintering time 3-12h.
6. The method for preparing the ultrahigh temperature composite ceramic according to claim 4, characterized in that: The content of the fine powder in step S2 is 10wt%-90wt% of the mass ratio of the single type of sintering powder, and the amount of sintering aid added is less than 10Vol% of the theoretical volume sum of the two types of sintering powder.
7. The method for preparing the ultrahigh temperature composite ceramic according to claim 4, characterized in that: In step S3, the powders are mixed uniformly by wet planetary ball milling, wet ultrasonic vibration or mechanical stirring.
8. The method for preparing the ultrahigh temperature composite ceramic according to claim 4, characterized in that: The vacuum degree in the furnace for sintering in step S4 is ≤8.0×10 -3 Pa, sintering temperature 1600-1900℃.
9. The method for preparing the ultrahigh temperature composite ceramic according to claim 4, characterized in that: In step S4, an axial pressure of 30 MPa to 60 MPa is applied to the mixed powder.
10. The method for preparing ultrahigh temperature composite ceramics according to claim 4, characterized in that: Before heating in step S4, the process also includes continuously introducing an inert gas into the vacuum chamber, and controlling the atmosphere pressure to be 0.4-2Pa.
Citation Information
Patent Citations
Preparation method of high-density ultra-high-temperature Ta4HfC5 ceramic block material
CN107857592A
Multiphase synergistic ultrahigh-temperature ceramic-based composite material and preparation method thereof
CN117088692A
Cited By
Method for preparing (ZrxTa (1-x) B2)-SiC antioxidant ceramic through hot-pressing rapid sintering
CN117586023A
A hot pressing rapid sintering preparation (Zr x Ta 1-x B2) - Method of SiC oxidation resistant ceramics
CN117586023B