White lignin as well as extraction method and application thereof

By employing low-temperature enzymatic hydrolysis and organic solvent extraction methods, the problem of dark lignin color in existing technologies has been solved, achieving efficient extraction and high-value-added utilization of white lignin, which is suitable for cosmetics, 3D printing, and thin film manufacturing.

CN119039611AActive Publication Date: 2024-11-29SOUTH CHINA UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410853729.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-29
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing technologies have difficulty effectively extracting white lignin, resulting in lignin products with a darker color, which limits their application in fields such as sunscreens, dispersants, coatings, and packaging.

Method used

White nut shell powder was treated with sodium hydroxide solution at low temperature, followed by enzymatic hydrolysis with cellulase and hemicellulase. Then, it was extracted with organic solvent and inorganic alkali. By adjusting the pH value and anti-oxidation treatment, white lignin precipitate was obtained.

Benefits of technology

It achieves efficient extraction of white lignin under mild conditions, with a whiteness between 80 and 90.4 degrees, suitable for cosmetics, 3D printing and film manufacturing. It also has ultraviolet absorption properties, realizing high-value utilization and environmental friendliness of lignin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039611A_ABST
    Figure CN119039611A_ABST
Patent Text Reader

Abstract

The invention discloses an extraction method of white lignin, which comprises the following steps: washing white shells, drying, crushing and sieving to obtain crushed materials with different sizes; performing pretreatment suction filtration on the crushed material to obtain filter residues, performing enzymolysis on the filter residues to obtain lignin-rich residues, finally adding an alcohol organic solvent, and performing centrifugation to separate out white lignin precipitate; the invention further discloses white lignin and application, the problem that white lignin cannot be directly extracted from plants is solved, damage to a lignin substructure in the treatment process can be reduced at low reaction temperature and short reaction time, generation of multiple chromophoric groups is avoided, a lignin product is made to be dark brown, and the color of the lignin product is improved. Therefore, effective extraction of the white lignin under the mild condition is realized, the whiteness of the extracted white lignin is 80-90.4 degrees, the white lignin can be used as an active component or an additive to be applied to products with strict requirements on color, and the application field of the lignin is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomass refining, and specifically relates to white lignin and an extraction method and application thereof. Background Art

[0002] With the increasing consumption of fossil resources, the shortage of resources has also brought about a series of environmental pollution and other problems, increasing the demand for alternative and sustainable resources. Lignin is the second largest biomass resource in the plant kingdom after cellulose. It has a natural three-dimensional network structure, high carbon content, good renewability and degradability. Its source is natural, safe, green and easy to obtain. If it is applied in the production and life fields, it will have good economic benefits. At the same time, it can also make rational use of natural resources and has good application prospects.

[0003] The color of natural lignin is white or nearly colorless, but due to the strict extraction technology (high temperature, high alkali, high acid value, etc.), the original structure of lignin is even destroyed, resulting in a variety of chromophores, making the lignin product appear dark brown. The darker apparent color of lignin can easily stain the product, which greatly limits its development and utilization in the fields of sunscreen, dispersants, coatings and packaging.

[0004] In order to improve the high-value utilization of lignin resources, it is necessary to reduce the color of lignin-based polymers. Therefore, domestic and foreign scholars have conducted some research on how to obtain light-colored lignin. Zhang Hui (Decolorization of lignin and its application in lignin-based chemicals, doctoral dissertation of South China University of Technology, 2018) explored the effect of structural changes on macroscopic color by studying the preparation method and microscopic size of lignin, and found that the microstructure of lignin has a certain relationship with its apparent color; Lee et al. (Preparation and Application of Light-Colored Lignin Nanoparticles for Broad-Spectrum Sunscreens, Polymers, 2020, 12: 699) uses rice husk as raw material, treats it with cellulase, and then extracts it in a solvent under mild conditions to finally obtain lighter-colored lignin; Chinese patent publication CN115838482A discloses a two-step high-boiling alcohol acid catalysis method for extracting light-colored lignin; Cui Ying et al. (Process optimization for rapid extraction of light-colored sugarcane bagasse lignin in one step, Fine Chemicals, 2020, 37(09): 1864-1869+1925) used p-toluenesulfonic acid (p-TsOH) to separate and extract sugarcane bagasse to prepare lighter-colored lignin.

[0005] Although there are some methods for extracting light-colored lignin, there is no literature report on the extraction of white lignin. How to avoid discoloration of natural lignin during the preparation process is the key to preparing white lignin. Therefore, it is necessary to further develop new methods for separating and extracting lignin. Summary of the invention

[0006] In order to overcome the above shortcomings of the prior art, the purpose of the present invention is to provide a method for extracting white lignin to solve the problem that the lignin extracted from plants in the prior art is dark in color.

[0007] Another object of the present invention is to provide a white lignin.

[0008] Another object of the present invention is to provide an application of white lignin.

[0009] The purpose of the present invention is achieved through the following technical solutions:

[0010] A method for extracting white lignin comprises the following steps:

[0011] (1) Wash and dry the white fruit shells, crush and sieve them to obtain crushed materials of different sizes;

[0012] (2) preparing a sodium hydroxide solution, mixing the crushed material in step (1) with the sodium hydroxide solution to obtain a mixed solution, reacting the mixed solution under low temperature conditions, neutralizing it with acid, filtering it with suction, and washing it to obtain a filter residue;

[0013] (3) preparing a buffer solution, mixing the filter residue in step (2) with the buffer solution, adding cellulase and hemicellulase, reacting in a water bath shaker for 72 hours, and then centrifuging and washing until neutral to obtain a lignin-rich residue;

[0014] (4) mixing the lignin-rich residue in step (3) with an alcohol organic solvent, adding an inorganic base, heating and centrifuging to obtain a supernatant, adjusting the pH value of the supernatant, standing for 2 to 12 hours, and precipitating a white lignin precipitate;

[0015] (5) The white lignin precipitate in step (4) is washed with an acidic aqueous solution to remove excess acid and salt, an antioxidant and a polyol are added to obtain a white slurry, and the white slurry is freeze-dried to obtain white lignin.

[0016] Preferably, the white husk is a discarded husk or seed coat that is white or light yellow in appearance.

[0017] Preferably, the white nut shell includes one or more of ginkgo nut shell, pumpkin seed shell, pistachio shell, white kidney bean skin, white lima bean skin, safflower seed skin and white toothpick melon seed skin.

[0018] Preferably, the specific step of drying in step (1) is to dry the washed white fruit shell in a hot air oven at 50-70° C. for 4-8 hours.

[0019] Preferably, the specific steps of crushing and screening in step (1) are as follows:

[0020] The white fruit shell is crushed into 40-80 mesh powder, then ground with a ball mill at a speed of 500 r / min for 6-24 hours, and finally sieved with a 100-300 mesh sieve to obtain a crushed material.

[0021] Preferably, the specific steps of adding acid for neutralization in step (1) are as follows:

[0022] Add acidic aqueous solution to the mixture to adjust the pH to neutral.

[0023] Preferably, the concentration of the sodium hydroxide solution in step (2) is 3 to 10 wt %.

[0024] Preferably, in step (2), the mass ratio of the crushed material to the sodium hydroxide solution is 1:1 to 20.

[0025] Preferably, the specific steps of reacting the mixed solution under low temperature conditions in step (2) are:

[0026] The mixture is stirred at -15 to 0°C for 1 to 5 hours, then frozen for 10 to 24 hours, and finally placed at room temperature to thaw, and the thawed mixture is stirred at room temperature.

[0027] More preferably, the specific step of stirring is stirring at a rotation speed of 200 to 800 r / min for 6 to 24 hours.

[0028] Preferably, in step (3), the mass ratio of the filter residue to the buffer solution is 1:1 to 20.

[0029] Preferably, the concentration of the buffer solution in step (3) is 0.1 to 1 mol·L -1 , pH is 4.3~6.5.

[0030] More preferably, the buffer solution includes one or more of sodium acetate, sodium phosphate and sodium citrate.

[0031] Preferably, in step (3), the amount of the cellulase used is 1-10 wt %, and the amount of the hemicellulase used is 0.1-3 wt %.

[0032] Preferably, the cellulase and hemicellulase include cellulase and hemicellulase provided by Novozymes, Sundry or Gemet.

[0033] Preferably, the water temperature of the water bath shaker reaction in step (3) is 40-50° C., and the speed is 100-220 r / min.

[0034] Preferably, the specific step of centrifugation in step (3) is centrifugation at 3000-10000 r / min for 10-20 min.

[0035] Preferably, the alcohol organic solvent in step (4) includes one or more of 1,4-butanediol, 1,3-butanediol, glycerol, ethylene glycol, propylene glycol and isopropanol.

[0036] Preferably, the solid-liquid ratio of the lignin-rich residue to the organic solvent is 1 g: 10-20 mL.

[0037] Preferably, the inorganic base in step (4) includes one or more of NaOH, KOH, Na2CO3, Ba(OH)2, Ca(OH)2, Mg(OH)2 and NaHCO3.

[0038] Preferably, the specific step of heating in step (4) is heating to 60-100° C. in an oil bath or a water bath, and keeping the temperature for 1-3 hours.

[0039] More preferably, the heating temperature is 60° C. and the insulation reaction time is 3 hours.

[0040] Preferably, the specific steps of adjusting the pH value of the supernatant in step (4) are as follows:

[0041] An acidic solution was added to adjust the pH value of the supernatant to 2-4.

[0042] More preferably, the acidic solution includes one or more of acetic acid, hydrochloric acid and citric acid.

[0043] Preferably, the acidic aqueous solution in step (5) comprises one or more of glycolic acid, malic acid, citric acid and acetic acid.

[0044] More preferably, the concentration of the acidic aqueous solution is 0.1-0.5 wt %.

[0045] Preferably, in step (5), the mass ratio of the antioxidant to the white lignin precipitate is 1:2-10.

[0046] More preferably, the antioxidant is ascorbic acid.

[0047] More preferably, the concentration of ascorbic acid is 0.1-0.4 wt %.

[0048] Preferably, the concentration of the polyol is 0.1-0.4 wt %.

[0049] Preferably, the mass ratio of the polyol to the white lignin precipitate is 1 g: 2-10 mL.

[0050] A white lignin extracted by a white lignin extraction method.

[0051] An application of white lignin for use in the cosmetics, 3D printing and film manufacturing industries.

[0052] The present invention has the following advantages and beneficial effects compared with the prior art:

[0053] (1) The present invention discloses a method for extracting white lignin, which directly extracts white lignin from plants; in the early stage, the fruit shell crushed material is subjected to alkalization and freeze-thaw to improve the enzymatic hydrolysis efficiency, retain more lignin, and thus facilitate the extraction of lignin. The cellulose and hemicellulose are removed by enzymatic hydrolysis, and then the lignin is dissolved by an organic solvent. The low reaction temperature and short reaction time can reduce the destruction of the lignin substructure during the treatment process, avoid the generation of multiple chromophores, and make the lignin product present a dark brown color, thereby achieving efficient extraction of white lignin under mild conditions. The extracted white lignin has a whiteness between 80 and 90.4 degrees, and can be mixed with other components to prepare a lignin-based biocomposite material.

[0054] (2) The process for extracting white lignin provided by the present invention is simple and feasible, and the obtained lignin has high purity and can be widely used in various industrial and agricultural products, realizing high added value utilization of lignin in multiple fields. In addition, the white lignin has certain ultraviolet absorption properties and can be used in the field of sun protection.

[0055] (3) The present invention utilizes fruit shell waste, such as ginkgo shells, pumpkin seed shells, pistachio shells, white lentil skins, safflower seed skins or white toothpick melon seed skins, to recycle biomass. This method is in line with the concept of green development and can effectively alleviate environmental pressure. The production process is simple and easy to control, has low equipment requirements and low reagent costs, and shows good industrialization potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 The present invention is a flow chart of a method for extracting white lignin.

[0057] Figure 2 This is a color comparison chart of the white lignin of Example 1 of the present invention and commercial lignin.

[0058] Figure 3 The infrared absorption spectra of the white lignin of Example 1 of the present invention and the commercial lignin are shown in FIG.

[0059] Figure 4The UV absorption spectra of the white lignin of Example 1 of the present invention and the commercial lignin are shown in FIG. DETAILED DESCRIPTION

[0060] The purpose of the present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments cannot be described one by one here, but the implementation mode of the present invention is not therefore limited to the following embodiments.

[0061] (1) Wash the pistachio shells, dry them in a hot air oven at 50° C. for 8 h, crush them mechanically with a household mixer, continue to ball mill them in a planetary ball mill for 8 h, and then pass them through a 150-mesh sieve to obtain a crushed material;

[0062] (2) Weigh 20 g of the material obtained in step (1), mix with 300 mL of 5 wt% sodium hydroxide solution, stir at -6 °C for 3 h, put into a refrigerator for 10 h, stir at room temperature for 12 h after the material is thawed, and then filter and wash to obtain a residue;

[0063] (3) The filter residue obtained in step (2) was mixed with 150 mL of 0.1 mol·L -1 The mixture was mixed with sodium acetate buffer solution, adjusted to pH 6.4, and 0.45 g of cellulase and 0.15 g of hemicellulase (Novozyme enzyme) were added. The mixture was reacted in a water bath shaker at 45°C and 200 r / min for 72 h, and then centrifuged at 4000 r / min for 10 min, and washed with distilled water until neutral;

[0064] (4) The material obtained in step (3) was mixed with 135 mL of a 90 wt% glycerol / water solution, and 2 g of sodium hydroxide was added as a catalyst. The mixture was heated to 60° C. for reaction for 3 h, and then centrifuged to obtain a supernatant. An acetic acid aqueous solution was added to adjust the pH value of the supernatant to 2.3, and the mixture was allowed to stand for 24 h to obtain a white lignin precipitate.

[0065] (5) The lignin precipitate obtained in step (4) was washed with 0.5 wt % acetic acid solution to remove excess acid and salt, and 10 mL of 0.2 wt % ascorbic acid and polyvinyl alcohol solution was added to obtain a white slurry, which was freeze-dried to obtain the white lignin.

[0066] The whiteness test was performed on the white lignin extracted in this example.

[0067] The whiteness test is as follows:

[0068] The lignin powder was pressed into tablets and its infrared spectrum was measured using a Fourier transform infrared spectrometer (Nicolet IS50-Nicolet Continuum, Thermo Fisher Scientific, USA) with a scanning range of 4000-400 cm -1. The white lignin extracted in this example was dissolved in a DMSO solution, and its ultraviolet absorbance at UVB (290-320nm) and UVA (320-400nm) was measured using a UV-1780 ultraviolet spectrometer (Shimadzu, Japan). The lignin powder was tested using an X-Rite 500 series colorimeter, and the color parameters L*, a*, and b* of the test samples were recorded after calibration. Each sample was tested five times, and the data were averaged. The L* value represents the brightness of the color, with values ​​ranging from 0 (black) to 100 (white); a* represents the red and green of lignin, with a positive value being red and a negative value being green; b* represents the yellow and blue of lignin, with a positive value being yellow and a negative value being blue. The whiteness (WI) is calculated using the following formula:

[0069]

[0070] The color data are shown in Table 1, and the whiteness value of lignin was determined to be 90.40.

[0071] Example 2

[0072] (1) Wash the white lentil husk, dry it in a hot air oven at 50°C for 8 h, mechanically crush it, ball mill it for 8 h, and then pass it through a 100-mesh sieve;

[0073] (2) Weigh 20 g of the material obtained in step (1), mix with 300 mL of 4 wt% sodium hydroxide solution, stir at -6 °C for 3 h, put in a refrigerator for 10 h, stir at room temperature for 12 h after the material is thawed, and then filter and wash to obtain a residue;

[0074] (3) The filter residue obtained in step (2) was mixed with 150 mL of 0.1 mol·L -1 The mixture was mixed with sodium dihydrogen phosphate / sodium phosphate buffer solution, adjusted to pH 6.0, added with 0.45 g of cellulase and 0.15 g of hemicellulase (Xindeli enzyme), reacted in a water bath shaker at 45°C and 200 r / min for 72 h, then centrifuged at 4000 r / min for 10 min, and washed with distilled water until neutral;

[0075] (4) The material obtained in step (3) was mixed with 135 mL of 90 wt% ethylene glycol / water solution, and 2 g of sodium phosphate was added as a catalyst. The mixture was heated to 60° C. for reaction for 3 h, and then centrifuged to obtain a supernatant. An acetic acid aqueous solution was added to adjust the pH value of the supernatant to 2.3, and the mixture was allowed to stand for 24 h to obtain a white lignin precipitate.

[0076] (5) The lignin precipitate obtained in step (4) was washed with 0.5wt% citric acid solution to remove excess acid and salt, and 10mL 0.1wt% ascorbic acid and low molecular weight chitosan solution were added to obtain a white slurry, which was freeze-dried to obtain the white lignin. The white lignin extracted in this example was tested for whiteness, and the detection method was the same as that in Example 1. The color data is shown in Table 1. The test results showed that the whiteness value of the lignin was 82.30.

[0077] Example 3

[0078] (1) Wash the ginkgo husks, dry them in a hot air oven at 50°C for 8 h, mechanically crush them, ball mill them for 8 h, and then pass them through a 100-mesh sieve;

[0079] (2) Weigh 20 g of the material obtained in step (1), mix with 300 mL of 3 wt% sodium hydroxide solution, stir at -6 °C for 3 h, put in a refrigerator for 10 h, stir at room temperature for 12 h after the material is thawed, and then filter and wash to obtain a residue;

[0080] (3) The filter residue obtained in step (2) was mixed with 150 mL of 0.1 mol·L -1 The mixture was mixed with sodium citrate buffer solution, adjusted to pH 6.3, added with 0.45 g cellulase and 0.15 g hemicellulase (Gemette enzyme), reacted in a water bath shaker at 45°C and 200 r / min for 72 h, then centrifuged at 4000 r / min for 10 min, and washed with distilled water until neutral;

[0081] (4) The material obtained in step (3) was mixed with 135 mL of 90 wt% 1,3-butanediol / water solution, and 2 g of sodium carbonate was added as a catalyst. The mixture was heated to 60° C. for reaction for 3 h, and then centrifuged to obtain a supernatant. An acetic acid aqueous solution was added to adjust the pH value of the supernatant to 2.3, and the mixture was allowed to stand for 24 h to obtain a white lignin precipitate.

[0082] (5) The lignin precipitate obtained in step (4) was washed with 0.5wt% citric acid solution to remove excess acid and salt, and 15mL 0.3wt% ascorbic acid and 1,4-butanediol solution were added to obtain a white slurry, which was freeze-dried to obtain the white lignin. The white lignin extracted in this example was tested for whiteness, and the detection method was the same as that in Example 1. The color data is shown in Table 1. The test results showed that the whiteness value of the lignin was 89.91.

[0083] Example 4

[0084] (1) Wash the white pumpkin seed peels, dry them in a hot air oven at 50°C for 8 h, mechanically crush them, ball mill them for 8 h, and then pass them through a 100-mesh sieve;

[0085] (2) Weigh 20 g of the crushed material, mix it with 300 mL of 3 wt% sodium hydroxide solution, stir it at -6°C for 3 h, put it in a refrigerator for 10 h, stir it at room temperature for 12 h after the material is thawed, and then filter and wash it to obtain a filter residue;

[0086] (3) The filter residue obtained in step (2) was mixed with 150 mL of 0.1 mol·L -1 The mixture was mixed with sodium acetate buffer solution, adjusted to pH 6.2, and 0.45 g of cellulase and 0.15 g of hemicellulase (Novozyme enzyme) were added. The mixture was reacted in a water bath shaker at 45°C and 200 r / min for 72 h, and then centrifuged at 4000 r / min for 10 min, and washed with distilled water until neutral;

[0087] (4) The material obtained in step (3) was mixed with 135 mL of 90 wt% 1,4-butanediol / water solution, and 2 g of sodium hydroxide was added as a catalyst. The mixture was heated to 60° C. for reaction for 3 h, and then centrifuged to obtain a supernatant. An acetic acid aqueous solution was added to adjust the pH value of the supernatant to 2.3, and the mixture was allowed to stand for 24 h to obtain a white lignin precipitate.

[0088] (5) The lignin precipitate obtained in step (4) was washed with 0.5wt% citric acid solution to remove excess acid and salt, and 10mL 0.1wt% ascorbic acid and polyethylene glycol 4000 solution were added to obtain a white slurry, which was freeze-dried to obtain the white lignin. The white lignin extracted in this example was tested for whiteness, and the detection method was the same as that in Example 1. The color data is shown in Table 1. The test results showed that the whiteness value of the lignin was 87.24.

[0089] Example 5

[0090] (1) Wash the white lentil husk, dry it in a hot air oven at 50°C for 8 h, mechanically crush it, ball mill it for 8 h, and then pass it through a 100-mesh sieve;

[0091] (2) Weigh 20 g of the material obtained in step (1), mix with 300 mL of 3 wt% sodium hydroxide solution, stir at -6 °C for 3 h, put in a refrigerator for 10 h, stir at room temperature for 12 h after the material is thawed, and then filter and wash to obtain a residue;

[0092] (3) The filter residue obtained in step (2) was mixed with 150 mL of 0.1 mol·L -1 The mixture was mixed with sodium acetate buffer solution, adjusted to pH 6.2, and 0.45 g of cellulase and 0.15 g of hemicellulase were added. The mixture was reacted in a water bath shaker at 45 °C and 200 r / min for 72 h, and then centrifuged at 4000 r / min for 10 min, and washed with distilled water until neutral;

[0093] (4) The material obtained in step (3) was mixed with 135 mL of a 90 wt% glycerol / water solution, and 2 g of sodium hydroxide was added as a catalyst. The mixture was heated to 60° C. for reaction for 3 h, and then centrifuged to obtain a supernatant. An acetic acid aqueous solution was added to adjust the pH value of the supernatant to 2.3, and the mixture was allowed to stand for 24 h to obtain a white lignin precipitate.

[0094] (5) The lignin precipitate obtained in step (4) was washed with 0.5wt% citric acid solution to remove excess acid and salt, and 10mL 0.2wt% ascorbic acid and polyethylene glycol 200 solution were added to obtain a white slurry, which was freeze-dried to obtain the white lignin. The white lignin extracted in this example was tested for whiteness, and the detection method was the same as that in Example 1. The color data is shown in Table 1. The test results showed that the whiteness value of the lignin was 80.11.

[0095] Comparative Example 1

[0096] The commercial lignin product is alkaline lignin, purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number L832292-100g.

[0097] The whiteness test of commercial lignin was carried out in the same manner as in Example 1. The color data is shown in Table 1.

[0098] Comparative Example 2

[0099] The pistachio shells were crushed and passed through a 150-mesh sieve. Then, 10 g of pistachio shell powder was added to 200 mL of pyruvic acid solution (50% by mass), and treated at 100° C. for 1 h to obtain light-colored lignin.

[0100] The whiteness test of the light-colored lignin was carried out in the same manner as in Example 1. The color data is shown in Table 1.

[0101] Comparative Example 3

[0102] The camellia oleifera shell was crushed and passed through a 150-mesh sieve. Then 10 g of the camellia oleifera shell powder was added to 200 mL of a pyruvic acid solution (50% by mass) and treated at 100° C. for 1 h to obtain light yellow lignin.

[0103] The light yellow lignin was tested for whiteness, and the testing steps were the same as in Example 1. The color data is shown in Table 1.

[0104] Comparative Example 4

[0105] (1) Wash the oil tea fruit shells, dry them in a hot air oven at 50°C for 8 hours, crush them mechanically with a household mixer, continue to ball mill them in a planetary ball mill for 8 hours, and then pass them through a 150-mesh sieve to obtain a crushed material;

[0106] (2) Weigh 20 g of the material obtained in step (1), mix with 300 mL of 5 wt% sodium hydroxide solution, stir at -6 °C for 3 h, put into a refrigerator for 10 h, stir at room temperature for 12 h after the material is thawed, and then filter and wash to obtain a residue;

[0107] (3) The filter residue obtained in step (2) was mixed with 150 mL of 0.1 mol·L -1 The mixture was mixed with sodium acetate buffer solution, adjusted to pH 6.4, and 0.45 g of cellulase and 0.15 g of hemicellulase (Novozyme enzyme) were added. The mixture was reacted in a water bath shaker at 45°C and 200 r / min for 72 h, and then centrifuged at 4000 r / min for 10 min, and washed with distilled water until neutral;

[0108] (4) The material obtained in step (3) was mixed with 135 mL of a 90 wt% glycerol / water solution, and 2 g of sodium hydroxide was added as a catalyst. The mixture was heated to 60° C. for reaction for 3 h, and then centrifuged to obtain a supernatant. An acetic acid aqueous solution was added to adjust the pH value of the supernatant to 2.3, and the mixture was allowed to stand for 24 h to obtain a light brown lignin precipitate.

[0109] (5) The lignin precipitate obtained in step (4) was washed with 0.5 wt% acetic acid solution to remove excess acid and salt, and 10 mL 0.2 wt% ascorbic acid and polyvinyl alcohol solution were added to obtain a light brown precipitate, which was freeze-dried to obtain light brown lignin. The measurement results showed that the whiteness value of the lignin was 44.85.

[0110] Comparative Example 5

[0111] (1) Wash the peanut shells, dry them in a hot air oven at 50°C for 8 hours, crush them mechanically with a household mixer, continue to ball mill them in a planetary ball mill for 8 hours, and then pass them through a 150-mesh sieve to obtain a crushed material;

[0112] (2) Weigh 20 g of the material obtained in step (1), mix with 300 mL of 5 wt% sodium hydroxide solution, stir at -6 °C for 3 h, put into a refrigerator for 10 h, stir at room temperature for 12 h after the material is thawed, and then filter and wash to obtain a residue;

[0113] (3) The filter residue obtained in step (2) was mixed with 150 mL of 0.1 mol·L -1 The mixture was mixed with sodium acetate buffer solution, adjusted to pH 6.4, and 0.45 g of cellulase and 0.15 g of hemicellulase (Novozyme enzyme) were added. The mixture was reacted in a water bath shaker at 45°C and 200 r / min for 72 h, and then centrifuged at 4000 r / min for 10 min, and washed with distilled water until neutral;

[0114] (4) The material obtained in step (3) was mixed with 135 mL of a 90 wt% glycerol / water solution, and 2 g of sodium hydroxide was added as a catalyst. The mixture was heated to 60° C. for reaction for 3 h, and then centrifuged to obtain a supernatant. An acetic acid aqueous solution was added to adjust the pH value of the supernatant to 2.3, and the mixture was allowed to stand for 24 h to precipitate yellow lignin.

[0115] (5) The lignin precipitate obtained in step (4) was washed with 0.5 wt% acetic acid solution to remove excess acid and salt, and 10 mL of 0.2 wt% ascorbic acid and polyvinyl alcohol solution was added to obtain yellow floccules, which were freeze-dried to obtain yellow lignin. The measurement results showed that the whiteness value of the lignin was 42.94.

[0116] Table 1

[0117]

[0118] Table 1 is the color data of each embodiment. The data comparison analysis of Example 1 and Comparative Example 1 shows that the white lignin extracted by this method is significantly better than the commercial lignin on the market in terms of whiteness. By comparing Example 1 with Comparative Examples 2 and 3, it can be seen that the lignin extracted by the acid method is darker in color. By comparing Example 1 with Comparative Examples 4 and 5, it can be seen that the whiteness obtained by treating different biomass raw materials with the same method is different, and white lignin is not present in all types of lignin. Therefore, the present invention is highly efficient in improving the whiteness of lignin, providing an important basis for further application development.

[0119] Figure 2 The color comparison diagram of the commercial lignin in Comparative Example 1 and the white lignin in Example 1 is shown in FIG. Figure 2 It can be seen that the color of commercial lignin is darker, showing black-brown, while the lignin extracted by the method of the present invention is white, indicating that the extraction method proposed in the present invention can effectively improve the whiteness of lignin, and its whiteness value is as high as 90.40.

[0120] Figure 3 The infrared absorption spectra of the white lignin in Example 1 and the commercial lignin in Comparative Example 1 are shown in the figure. As can be seen from the figure, 3358 cm -1 The characteristic peak of OH on the benzene ring and side chain of lignin, 2940cm -1 and 2872cm -1 It is the characteristic peak of CH in methyl and methylene. 1653cm -1 、1503cm -1 and 1462cm -1 It is the characteristic peak of the aromatic ring skeleton of lignin. 1329cm -1 、1225cm -1 、1126cm -1 and 1051cm-1 It is the characteristic peak of the basic structural unit of lignin, indicating that white lignin has a typical lignin compound structure. In addition, it can be seen from the figure that the peak intensity of commercial lignin increases with the increase of chromophore or auxochrome, which may be the reason for the blackening of lignin.

[0121] Figure 4 The UV absorption spectra of the commercial lignin in Comparative Example 1 and the white lignin in Example 1 illustrate that the white lignin can effectively absorb ultraviolet radiation and can be applied to the sun protection field of cosmetics.

[0122] The above specific implementation modes are preferred embodiments of the present invention and cannot be used to limit the present invention. Any other changes or other equivalent replacement methods that do not deviate from the technical solution of the present invention are included in the protection scope of the present invention.

Claims

1. A method for extracting white lignin, characterized in that: The following steps are involved: (1) Wash and dry the white fruit shells, crush and sieve them to obtain crushed materials of different sizes; (2) preparing a sodium hydroxide solution, mixing the crushed material in step (1) with the sodium hydroxide solution to obtain a mixed solution, reacting the mixed solution under low temperature conditions, neutralizing it with acid, filtering it with suction, and washing it to obtain a filter residue; (3) preparing a buffer solution, mixing the filter residue in step (2) with the buffer solution, adding cellulase and hemicellulase, reacting in a water bath shaker for 72 hours, and then centrifuging and washing until neutral to obtain a lignin-rich residue; (4) mixing the lignin-rich residue in step (3) with an alcohol organic solvent, adding an inorganic base, heating and centrifuging to obtain a supernatant, adjusting the pH value of the supernatant, standing for 2 to 12 hours, and precipitating a white lignin precipitate; (5) The white lignin precipitate in step (4) is washed with an acidic aqueous solution to remove excess acid and salt, an antioxidant and a polyol are added to obtain a white slurry, and the white slurry is freeze-dried to obtain white lignin.

2. The method for extracting white lignin according to claim 1, characterized in that: The white husks include one or more of ginkgo husks, pumpkin seed husks, pistachio husks, white kidney bean husks, white lima bean husks, safflower seed husks and white toothpick melon seed husks.

3. The method for extracting white lignin according to claim 1, characterized in that: The specific steps of reacting the mixed solution under low temperature conditions in step (2) are: The mixture is stirred at -15 to 0°C for 1 to 5 hours, then frozen for 10 to 24 hours, and finally placed at room temperature to thaw, and the thawed mixture is stirred at room temperature.

4. The method for extracting white lignin according to claim 1, characterized in that: The mass ratio of the filter residue to the buffer in step (3) is 1:1 to 20.

5. The method for extracting white lignin according to claim 1, characterized in that: In step (3), the amount of the cellulase used is 1-10 wt %, and the amount of the hemicellulase used is 0.1-3 wt %.

6. The method for extracting white lignin according to claim 1, characterized in that: The alcohol organic solvent in step (4) includes one or more of 1,4-butanediol, 1,3-butanediol, glycerol, ethylene glycol, propylene glycol and isopropanol.

7. The method for extracting white lignin according to claim 1, characterized in that: The solid-to-liquid ratio of the lignin residue to the alcohol organic solvent in step (4) is 1 g: 10-20 mL.

8. The method for extracting white lignin according to claim 1, characterized in that: The specific step of heating in step (4) is to heat to 60-100° C. in an oil bath or a water bath and keep the reaction for 1-3 hours.

9. A white lignin, characterized in that The white lignin is extracted by the extraction method of any one of claims 1 to 8.

10. The use of white lignin according to claim 9, characterized in that: Used in cosmetics, 3D printing and thin film manufacturing industries.

Citation Information

Patent Citations

  • Production methods for solubilized lignin, saccharide raw material and monosaccharide raw material, and solubilized lignin

    CN101848920A

  • Method for producing lignin degradation product

    CN103998617A

  • Method for extracting high-activity lignin from biomass and lignin extracted by same

    CN105860090A

  • Method for extracting light-colored lignin from camellia oleifera meal and application of light-colored lignin in sunscreen cream

    CN114920951A

  • Light-color lignin as well as preparation method and application thereof

    CN115838482A