High-entropy rare earth high-temperature thermistor material and preparation method thereof

By using a solid-state sintering method to prepare high-entropy rare earth materials, the problem of structural instability of traditional thermistors under high-temperature environments was solved, enabling high-precision temperature monitoring in the range of 550℃-1600℃, and producing high-temperature thermistor materials with stable performance and high sensitivity.

CN119049822APending Publication Date: 2024-11-29XINJIANG TECH INST OF PHYSICS & CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163772.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional spinel thermistor materials have unstable phase structures at high temperatures, which easily deteriorates their thermistor performance, limiting their application below 300℃ and failing to meet the temperature monitoring requirements in high-temperature environments.

Method used

High-entropy rare earth materials are used to prepare high-temperature thermistor materials with ferromanganese ore structure and monoclinic structure by mixing multiple rare earth elements and solid-state sintering. Platinum paste electrodes are coated and annealed to form a thermistor material with high stability and high sensitivity.

Benefits of technology

It exhibits a significant negative temperature coefficient and ultra-high linearity in the temperature range of 550℃-1600℃, with stable performance, and is suitable for high-precision high-temperature thermistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049822A_ABST
    Figure CN119049822A_ABST
Patent Text Reader

Abstract

The invention provides a high-entropy rare earth high-temperature thermistor material and a preparation method thereof. The material is prepared from any five of lanthanum trioxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, dysprosium oxide, holmium oxide, erbium oxide, terbium oxide, ytterbium oxide and lutetium oxide. The high-temperature thermistor material with a bixbyite structure and a monocline structure, a material constant B550 DEG C / 1600 DEG C = 17038-23648K, resistivity of 6.56 * 10 < 4 >-2.81 * 10 < 6 > omegacm at 750 DEG C and a sensitivity coefficient of-0.49--0.67% at 1600 DEG C is obtained by mixing, grinding, calcining, cold isostatic pressing, high-temperature sintering and electrode coating and burning. The high-temperature thermistor material with the bixbyite structure and the monoclinic structure is stable in performance and good in consistency. The material has obvious negative temperature coefficient characteristics in a temperature range of 550-1600 DEG C, has ultrahigh linearity, and is expected to be applied to high-precision high-temperature thermistors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high entropy rare earth high temperature thermistor material and a preparation method thereof. The thermistor material has good negative temperature coefficient characteristics in the temperature range of 550°C-1600°C and is a new type of thermistor material suitable for manufacturing ultra-high temperature thermistors. Background Art

[0002] In the rapidly developing field of electronics and sensor technology, thermistors occupy a pivotal position in many applications that require precise temperature monitoring and play a vital role in the progress of contemporary society. Compared with resistance temperature detectors and thermocouples, thermistors have extremely high sensitivity due to their high material constants and can accurately capture small fluctuations in temperature. Not only that, thermistors also have the dual advantages of low cost and simple preparation process, making them an ideal choice in the field of temperature monitoring. Especially in high temperature environments, its ultra-high sensitivity makes it have broad application prospects in high-precision temperature measurement in industry, defense and cutting-edge technology. With the continuous advancement of electronic information technology, scientific researchers have deepened their research on new NTC materials to meet increasingly complex application needs. However, the traditional spinel structure thermistor material has an unstable phase structure in a high temperature environment, and its thermal sensitivity is prone to deterioration, which limits its application in a higher temperature range, mainly limited to below 300°C.

[0003] In order to overcome this challenge, it is particularly important to carry out research on high-temperature thermistor materials with new structures. In this context, high-entropy rare earth materials have attracted widespread attention from scientific researchers due to their unique properties and structures. High-entropy rare earth materials are formed by mixing multiple rare earth elements in an equiatomic ratio or a near-equiatomic ratio. Their highly disordered atomic arrangement and complex chemical composition give them excellent thermal stability and antioxidant properties. As potential high-temperature NTCR materials, high-entropy rare earth materials have broad research prospects and application potential. By optimizing the elemental composition and preparation process, their thermosensitive properties can be further improved, and their stability and reliability at high temperatures can be improved. This will provide more efficient and safer temperature detection and control solutions for home appliances, medical devices, aerospace, automobile manufacturing and other fields.

[0004] The invention adopts a traditional solid phase sintering method to prepare a high entropy rare earth negative temperature coefficient thermistor, and adopts different sintering conditions to prepare a high temperature thermistor material with a temperature range of 550°C-1600°C. Summary of the invention

[0005] The object of the present invention is to provide a high entropy rare earth high temperature thermistor material and a preparation method thereof. The material is made of any five of lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide, erbium trioxide, terbium trioxide, ytterbium trioxide and lutetium trioxide as raw materials, and is subjected to mixed grinding, calcination, cold isostatic pressing, high temperature sintering, and coating and firing electrodes to obtain a material having a bixbyite structure and a monoclinic structure, and the material constant is B 550℃ / 1600℃ =17038K-23648K, temperature 750℃, resistivity is 6.56×10 4 Ωcm-2.81×10 6 Ωcm, and a high temperature thermistor material with a sensitivity coefficient of -0.49% to -0.67% at 1600°C. The bixbyite structure and monoclinic structure high temperature thermistor materials prepared by the method of the present invention have stable performance, good consistency, obvious negative temperature coefficient characteristics in the temperature range of 550°C-1600°C, and ultra-high linearity, and are expected to be applied to high-precision high temperature thermistors.

[0006] The high entropy rare earth high temperature thermistor material of the present invention has a chemical composition of R2O3, wherein R is any five of lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide, erbium trioxide, terbium trioxide, ytterbium trioxide, and lutetium trioxide as raw materials, and its structure belongs to the bixbyite structure and the monoclinic structure, and the space groups are Ia-3 and C2 / m respectively. The specific operation is carried out according to the following steps:

[0007] a. According to the composition of R2O3 and the chemical formula (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、(Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2)2O3: weigh lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide, erbium trioxide, terbium trioxide, ytterbium trioxide and lutetium trioxide respectively, mix them, grind the mixed raw materials in a ball mill for 6-10 hours to obtain powder;

[0008] b. Calcine the powder ground in step a at 1300-1400°C for 6-10 hours, and continue grinding in a ball mill for 5-10 hours to obtain (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、(Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3 powder;

[0009] c. The powder material obtained in step b is heated to 15-25 kg / cm 2 The block material is pressed at a pressure of 0.2-1 minute, and the formed block material is cold isostatically pressed at a pressure of 150-300 MPa for 2-5 minutes, and then sintered at a temperature of 1600°C-1700°C for 3-10 hours to obtain a high-temperature thermistor ceramic material;

[0010] d. The ceramic material sintered in step c is coated with platinum paste electrodes on both sides, and then annealed at a temperature of 1200°C for 120 minutes to obtain a negative temperature coefficient characteristic in the temperature range of 550°C-1600°C, and the material constant is B 550℃ / 1600℃ =17038K-23648K, the sensitivity coefficient is -0.49%--0.67% at 1600℃, and the resistivity is 6.56×10 4 -2.81×10 6 Ωcm high temperature thermistor material.

[0011] A method for preparing a high entropy rare earth high temperature thermistor material is carried out according to the following steps:

[0012] a. According to the chemical composition of R2O3, and according to the chemical formula (La0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、(Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3: weigh lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide, erbium trioxide, terbium trioxide, ytterbium trioxide and lutetium trioxide respectively, mix them, grind the mixed raw materials in a ball mill for 6-10 hours to obtain powder;

[0013] b. Calcine the powder ground in step a at 1300-1400°C for 6-10 hours, and continue grinding in a ball mill for 5-10 hours to obtain (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、(Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3 powder;

[0014] c. The powder material obtained in step b is heated to 15-25 kg / cm 2 The block material is pressed into a block at a pressure of 0.2-1 minute, and the formed block material is cold isostatically pressed at a pressure of 150-300 MPa for 2-5 minutes, and then sintered at a temperature of 1600-1700°C for 3-10 hours to obtain a high-temperature thermistor ceramic material;

[0015] d. Coat the ceramic material sintered in step c with platinum paste electrodes on both sides, and then anneal at 1200°C for 120 minutes to obtain a material with a negative temperature coefficient characteristic in the temperature range of 550-1600°C, with a material constant of B. 550℃ / 1600℃ =17038-23648K, the sensitivity coefficient is -0.49%--0.67% at 1600℃, and the resistivity is 6.56×10 4 -2.81×10 6 Ωcm high temperature thermistor material.

[0016] The high-entropy rare earth high-temperature thermistor material of the present invention is prepared by mixing and grinding any five oxides of lanthanum, neodymium, samarium, europium, gadolinium, dysprosium, holmium, erbium, terbium, ytterbium and lutetium by a solid phase method, calcining, mixing and grinding again to obtain a negative temperature coefficient thermistor powder material, and then cold isostatically pressing the powder material into a sheet, sintering at a high temperature, coating and firing platinum slurry electrodes on both sides to obtain a thermistor ceramic sheet, the ceramic sheet thermistor is a ceramic material with a bixbyite structure and a monoclinic structure R2O3 (R is a rare earth), and its material constant is B 550℃ / 1600℃ =17038K-23648K, the sensitivity coefficient is as high as -0.49%--0.67% at 1600℃, and the resistivity is 6.56×10 4 Ωcm-2.81×10 6 Ωcm high temperature thermistor material. The bixbyite structure and monoclinic structure high temperature thermistor materials prepared by the method have stable performance and good consistency. The thermistor material has obvious negative temperature coefficient characteristics in the temperature range of 550℃-1600℃ and has ultra-high linearity, and is expected to be applied to high-precision high temperature thermistors. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the XRD spectrum of the thermosensitive ceramic material sintered at a temperature of 1600-1700°C according to the present invention.

[0018] Figure 2 The figure is a temperature resistance curve of the thermosensitive ceramic material sintered at a temperature of 1600-1700°C according to the present invention. DETAILED DESCRIPTION

[0019] Example 1

[0020] a. First press (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2)2O3 composition, respectively weigh analytically pure lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide and gadolinium trioxide, mix them, grind the mixed raw materials in a ball mill for 6 hours to obtain powder;

[0021] b. The powder ground in step a was calcined at 1300°C for 6 hours and ground for 5 hours to obtain (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3 powder;

[0022] c. The powder material obtained in step b was heated to 15 kg / cm 2 The block material was pressed at a pressure of 150 MPa for 2 minutes, and then sintered at 1600°C for 3 hours to obtain a high-temperature thermistor ceramic material.

[0023] d. Coat the ceramic material sintered in step c with platinum paste electrodes on both sides, and then anneal at 1200°C for 120 minutes to obtain a material with a negative temperature coefficient in the temperature range of 750°C-1600°C. The material constant is B 750℃ / 1600℃ =18295K, the sensitivity coefficient is -0.52% at 1600℃, and the resistivity is 9.35×10 4 Ωcm high temperature thermistor material.

[0024] Example 2

[0025] a. First press (E 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3 composition, respectively weigh analytically pure europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide and erbium trioxide, mix them, grind the mixed raw materials in a ball mill for 8 hours to obtain powder;

[0026] b. The powder ground in step a was calcined at 1340°C for 7 hours and ground for 8 hours to obtain (Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3 powder;

[0027] c. The powder material obtained in step b was heated to 20 kg / cm 2The block material was pressed into a block under a pressure of 0.5 minutes, and the block material was cold isostatically pressed at a pressure of 200 MPa for 3 minutes, and then sintered at a temperature of 1650°C for 5 hours to obtain a high-temperature thermistor ceramic material.

[0028] d. Coat the ceramic material sintered in step c with platinum paste electrodes on both sides, and then anneal at 1200°C for 120 minutes to obtain a material with a negative temperature coefficient characteristic in the temperature range of 750°C-1600°C, and the material constant is B 750℃ / 1600℃ =21446K, the sensitivity coefficient is -0.661% at 1600℃, and the resistivity is 6.62×10 5 Ωcm high temperature thermistor material.

[0029] Example 3

[0030] a. First press (Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 composition, respectively weigh analytically pure dysprosium trioxide, holmium trioxide, terbium trioxide, ytterbium trioxide and lutetium trioxide, mix them, grind the mixed raw materials in a ball mill for 8 hours to obtain powder;

[0031] b. The powder ground in step a was calcined at 1360°C for 8 hours, and then (Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 powder;

[0032] c. The powder material obtained in step b was heated to 20 kg / cm 2 The block material was pressed into a block at a pressure of 0.5 minutes, and the block material was cold isostatically pressed at a pressure of 220 MPa for 4 minutes, and then sintered at a temperature of 16550°C for 5 hours to obtain a high-temperature thermistor ceramic material.

[0033] d. Coat the ceramic material sintered in step c with platinum paste electrodes on both sides, and then anneal at 1200°C for 120 minutes to obtain a material with a negative temperature coefficient in the temperature range of 750°C-1600°C. The material constant is B 750℃ / 1600℃ =23648K, the sensitivity coefficient is -0.67% at 1600℃, and the resistivity is 2.8×10 6 Ωcm high temperature thermistor material.

[0034] Example 4

[0035] a. First press (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3 composition, respectively weighing analytically pure neodymium trioxide, samarium trioxide, erbium trioxide, ytterbium trioxide and lutetium trioxide, mixing them, and grinding the mixed raw materials in a ball mill for 10 hours to obtain powder;

[0036] b. The powder ground in step a was calcined at 1400°C for 10 hours, and then ground for 10 hours to obtain (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3 powder;

[0037] c. The powder material obtained in step b was heated to 25 kg / cm 2 The block material was pressed into a block under a pressure of 100 MPa for 1 minute, and the block material was cold isostatically pressed at a pressure of 300 MPa for 5 minutes, and then sintered at a temperature of 1700°C for 10 hours to obtain a high-temperature thermistor ceramic material.

[0038] d. Coat the ceramic material sintered in step c with platinum paste electrodes on both sides, and then anneal at 1200°C for 120 minutes to obtain a material with a negative temperature coefficient in the temperature range of 550°C-1600°C. The material constant is B 550℃ / 1600℃ =17037K, the sensitivity coefficient is -0.49% at 1600℃, and the resistivity is 6.96×10 4 Ωcm high temperature thermistor material.

Claims

1. A high entropy rare earth high temperature thermistor material, characterized in that The chemical composition of the thermistor material is R2O3, wherein R is any five of lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide, erbium trioxide, terbium trioxide, ytterbium trioxide, and lutetium trioxide as raw materials, and its structure belongs to bixbyite structure and monoclinic structure, and the space groups are Ia-3 and C2 / m respectively. The specific operation is carried out according to the following steps: a. According to the composition of R2O3 and the chemical formula (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、 (Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3: weigh lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide, erbium trioxide, terbium trioxide, ytterbium trioxide and lutetium trioxide respectively, mix them, grind the mixed raw materials in a ball mill for 6-10 hours to obtain powder; b. Calcine the powder ground in step a at 1300-1400°C for 6-10 hours, and continue grinding in a ball mill for 5-10 hours to obtain (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、(Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3 powder; c. The powder material obtained in step b is heated to 15-25 kg / cm 2 The block material is pressed at a pressure of 0.2-1 minute, and the formed block material is cold isostatically pressed at a pressure of 150-300 MPa for 2-5 minutes, and then sintered at a temperature of 1600°C-1700°C for 3-10 hours to obtain a high-temperature thermistor ceramic material; d. The ceramic material sintered in step c is coated with platinum paste electrodes on both sides, and then annealed at a temperature of 1200°C for 120 minutes to obtain a negative temperature coefficient characteristic in the temperature range of 550°C-1600°C, and the material constant is B 550℃ / 1600℃ =17038K-23648K, the sensitivity coefficient at 1600℃ is -0.49%—-0.67%, and the resistivity at 750℃ is 6.56×10 4 -2.81×10 6 Ωcm high temperature thermistor material.

2. A method for preparing a high entropy rare earth high temperature thermistor material, characterized in that Follow these steps: a. According to the chemical composition of R2O3, and according to the chemical formula (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、 (Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3: weigh lanthanum trioxide, neodymium trioxide, samarium trioxide, europium trioxide, gadolinium trioxide, dysprosium trioxide, holmium trioxide, erbium trioxide, terbium trioxide, ytterbium trioxide and lutetium trioxide respectively, mix them, grind the mixed raw materials in a ball mill for 6-10 hours to obtain powder; b. Calcine the powder ground in step a at 1300-1400°C for 6-10 hours, and continue grinding in a ball mill for 5-10 hours to obtain (La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 Gd0 .2 )2O3、(Eu 0.2 G 0.2 Dy 0.2 Ho 0.2 Er 0.2 )2O3、(Dy 0.2 Ho 0.2 Tm 0.2 Yb 0.2 Lu 0.2 )2O3 and (Nd 0.2 Sm 0.2 Er 0.2 Yb 0.2 Lu 0.2 )2O3 powder; c. The powder material obtained in step b is heated to 15-25 kg / cm 2 The block material is pressed at a pressure of 0.2-1 minute, and the formed block material is cold isostatically pressed at a pressure of 150-300 MPa for 2-5 minutes, and then sintered at a temperature of 1600-1700°C for 3-10 hours to obtain a high-temperature thermistor ceramic material; d. The ceramic material sintered in step c is coated with platinum paste electrodes on both sides, and then annealed at a temperature of 1200°C for 120 minutes to obtain a negative temperature coefficient characteristic in the temperature range of 550-1600°C, and the material constant is B 550℃ / 1600℃ =17038-23648K, the sensitivity coefficient at 1600℃ is -0.49%—-0.67%, and the resistivity at 750℃ is 6.56×10 4 -2.81×10 6 Ωcm high temperature thermistor material.