Asphalt-based spherical hard carbon negative electrode material and preparation method and application thereof

Through cross-linking polymerization and melt spray granulation technology, combined with plasma oxidation treatment, high-density asphalt-based spherical hard carbon materials were prepared, which solved the problem of low specific capacity and density of existing asphalt-based hard carbon materials, significantly improving its content and Electrochemical and safety performance in lithium-ion and sodium-ion batteries.

CN119050351APending Publication Date: 2024-11-29HUNAN XINGFEIYUE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411147672.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The low specific capacity and low tap density of existing bituminous hard carbon materials limit their application in lithium-ion batteries and sodium-ion batteries, especially in fast charging and high safety performance.

Method used

Asphalt with high softening points was obtained by cross-linking polymerization, spherical particles were prepared by melt spray granulation method, combined with plasma oxidation treatment, and finally carbonization was carried out under low and high temperature conditions to prepare asphalt-based spherical hard carbon material.

Benefits of technology

The tap density and electrochemical performance of the material are improved. The reversible capacity of lithium-ion batteries exceeds 400mAh/g, the first Coulomb efficiency of sodium-ion batteries exceeds 90%, and the capacity retention rate of 1,000 cycles is above 90%, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050351A_ABST
    Figure CN119050351A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of carbon materials and battery materials, and particularly relates to an asphalt-based spherical hard carbon negative electrode material as well as a preparation method and application thereof. Cheap asphalt is used as a raw material, modified asphalt with a high softening point is obtained through cross-linking polymerization, then spherical asphalt particles are obtained through fusion spray granulation, pre-oxidized asphalt spheres are obtained in combination with plasma oxidation treatment, and finally the asphalt-based spherical hard carbon material is obtained through low-temperature carbonization and high-temperature carbonization treatment. The material is used as a negative electrode material of a lithium ion battery and / or a sodium ion battery. The synthesis process is simple, easy to control, safe, reliable, low in production cost, high in yield and suitable for industrial batch production. The material is a lithium ion battery negative electrode material, the reversible capacity exceeds 400mAh / g, and the capacity retention rate of 0.1 C / 5C is more than 70%. As a sodium ion battery negative electrode material, the reversible capacity reaches 310 mAh / g or above, the first coulombic efficiency exceeds 90%, and the capacity retention rate is 90% or above after 1000 cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of carbon materials and battery materials, and particularly relates to a pitch-based spherical hard carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] Graphite material is currently the most widely used negative electrode material for lithium-ion batteries, but the theoretical lithium insertion capacity of graphite is only 372mAh / g. In addition, the interlayer spacing of graphite is small, which causes the slow kinetic diffusion of lithium ions during the insertion and removal process, resulting in poor rate performance, limiting the application of lithium-ion batteries in the field of fast charging. Hard carbon materials have a highly disordered isotropic structure and a large interlayer spacing, which can meet the rapid insertion and removal of lithium ions and are suitable for large current charging and discharging. Moreover, hard carbon has good compatibility with the electrolyte, can prevent the precipitation of dendrite lithium, and has more stable cycle performance and better safety performance. Therefore, hard carbon has become the most promising negative electrode material for automotive lithium-ion power batteries that focus on output power.

[0003] Compared with lithium, sodium has more abundant reserves, more even distribution, similar chemical properties, lower cost, and sodium-ion batteries have the same working principle as lithium-ion batteries. Sodium-ion batteries can meet the requirements of low cost, long life, and high safety performance in the field of new energy, and to a certain extent alleviate the shortage of lithium resources, making them a beneficial supplement to lithium-ion batteries. In the research of sodium-ion battery electrode materials, asphalt has the advantages of high carbon yield and low cost, and is an ideal carbon source for preparing sodium-ion battery negative electrode materials, but its specific capacity is low, generally <100mAh g -1 If its sodium storage performance is improved, asphalt will be an excellent negative electrode material for sodium ion batteries. The low sodium storage capacity of asphalt is because the molecules of asphalt undergo orderly rearrangement to form a graphite-like layer structure during the high-temperature pyrolysis and carbonization process, which is not conducive to the storage of sodium ions. To realize the application of asphalt-based carbon materials in the negative electrode of sodium ion batteries, the key is to limit graphitization during the high-temperature carbonization process and introduce more sodium ion storage defect sites in the carbon skeleton.

[0004] In recent years, researchers have studied a large number of different synthetic methods to prepare asphalt-based hard carbon materials. However, the prepared hard carbon negative electrode materials still face the problems of low specific capacity and low tap density. Therefore, using a simple and feasible method to prepare high-capacity and high-tap density hard carbon negative electrode materials is an urgent problem to be solved in the industrialization of lithium-ion batteries and sodium-ion batteries. Summary of the invention

[0005] In response to the problems existing in the current preparation methods of asphalt-based hard carbon materials, cheap asphalt is used as raw material, and modified asphalt with a high softening point is obtained through cross-linking polymerization. Subsequently, melt spray granulation is used to obtain spherical asphalt particles, which are then combined with plasma oxidation treatment to obtain pre-oxidized asphalt balls. Finally, asphalt-based spherical hard carbon materials are obtained through low-temperature carbonization and high-temperature carbonization treatment as negative electrode materials for lithium-ion batteries and / or sodium-ion batteries.

[0006] The technical solution of the present invention is as follows:

[0007] A pitch-based spherical hard carbon negative electrode material, comprising the following raw materials: asphalt, a cross-linking agent, and a catalyst;

[0008] The cross-linking agent is one or more of terephthalaldehyde, terephthalic alcohol, p-tolualdehyde, p-toluyl alcohol, benzaldehyde, and trioxymethylene;

[0009] The catalyst is one or more of p-toluenesulfonic acid, concentrated sulfuric acid, benzenesulfonic acid and chlorosulfonic acid.

[0010] Preferably, the mass ratio of asphalt to cross-linking agent is 100:10-40, and the mass ratio of asphalt to catalyst is 100:5-15.

[0011] Preferably, the asphalt has a softening point of 50 to 150°C.

[0012] Another object of the present invention is to protect the preparation method of the above-mentioned asphalt-based spherical hard carbon negative electrode material, characterized in that it comprises the following steps:

[0013] (1) Cross-linking polymerization: The asphalt, cross-linking agent and catalyst are mixed evenly and reacted while stirring to obtain a cross-linked high softening point asphalt;

[0014] (2) Melt spray granulation: The high softening point asphalt is heated to obtain a molten liquid, and the molten liquid is spray granulated to obtain asphalt microspheres with controllable particle size;

[0015] (3) Pre-oxidation treatment: The asphalt microspheres are heated and oxidized in an oxidizing atmosphere to obtain pre-oxidized asphalt microspheres;

[0016] (4) Carbonization treatment: Pre-oxidized asphalt microspheres are carbonized to obtain asphalt-based spherical hard carbon particles.

[0017] Preferably, the reaction in step (1) is carried out under the protection of an inert gas;

[0018] And / or, the reaction conditions are: temperature 120-250° C., time 1-10 h.

[0019] Preferably, the oxidizing atmosphere in step (3) is one or more of oxygen, ozone, air, nitrogen dioxide, and sulfur trioxide;

[0020] And / or, the heating oxidation treatment conditions are: temperature of 150-350° C. and time of 3-15 hours.

[0021] Preferably, the carbonization process in step (4) is: heating to 450-800° C. for carbonization treatment for 0.5-4 h under the protection of inert gas, and then heating to 1200-1600° C. for carbonization treatment for 2-6 h.

[0022] Preferably, the carbonization in step (3) is carried out in a furnace equipped with a plasma treatment device; preferably, it is carried out in a rotary kiln.

[0023] Another object of the present invention is to protect the use of the above-mentioned asphalt-based spherical hard carbon negative electrode material or the asphalt-based spherical hard carbon negative electrode material prepared by the above-mentioned method in lithium-ion batteries and / or sodium-ion batteries.

[0024] Furthermore, it is used as a negative electrode material.

[0025] Beneficial effects of the present invention:

[0026] (1) By cross-linking and polymerizing the asphalt molecules to increase its softening point, combined with melt spray granulation, spherical particles are obtained. Spherical particles help to increase the tap density of the material, and the tap density is >0.9g / cm 3 .

[0027] (2) In the traditional heating oxidation method, oxygen molecules react with the asphalt surface to form a dense oxidative cross-linking layer, which hinders the further diffusion of oxygen molecules into the interior. The present invention uses plasma-assisted oxidation, and the oxygen molecules are highly active, which helps the asphalt microspheres to be evenly and fully oxidized, and greatly shortens the oxidation time, thereby improving production efficiency.

[0028] (3) The pitch-based spherical hard carbon material of the present invention can exhibit excellent electrochemical properties. As a negative electrode material for lithium-ion batteries, the reversible capacity exceeds 400 mAh / g, and the capacity retention rate at 0.1C / 5C is more than 70%. As a negative electrode material for sodium-ion batteries, the reversible capacity is more than 310 mAh / g, the first coulombic efficiency exceeds 90%, and the capacity retention rate is more than 90% after 1,000 cycles.

[0029] (4) The synthesis process of the present invention is simple, easy to control, safe and reliable, has low production cost and high yield, and is suitable for industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a scanning electron microscope image of the hard carbon material of Example 1;

[0031] Figure 2 This is a scanning electron microscope image of the hard carbon material of Comparative Example 1;

[0032] Figure 3 The charge and discharge curve of the hard carbon material of Example 1 as the negative electrode of a sodium ion battery at 0.1C.

[0033] Figure 4 This is a rate performance diagram of the hard carbon materials of Example 1 and Comparative Example 1 as negative electrodes of lithium-ion batteries. Specific implementation methods

[0034] The present invention is further described in detail below by way of examples so that those skilled in the art can better understand the present invention, but the present invention is not limited to the following examples.

[0035] Example 1

[0036] A method for preparing a pitch-based spherical hard carbon negative electrode material comprises the following steps:

[0037] (1) Cross-linking polymerization: Grind coal tar pitch raw material with a softening point of 80°C through a 100-mesh sieve, then use terephthalaldehyde as a cross-linking agent, the cross-linking agent accounts for 10% of the asphalt mass ratio, and use p-toluenesulfonic acid as a catalyst, the catalyst accounts for 15% of the asphalt mass ratio, mix the three evenly, heat to 160°C under N2 protection, and react for 8 hours while stirring to obtain a cross-linked high softening point asphalt;

[0038] (2) Melt spray granulation: The high softening point asphalt is heated to 300°C to obtain a melt, and the melt is spray-cooled and granulated to obtain asphalt microspheres with a D50 of 8 to 12 μm;

[0039] (3) Pre-oxidation reaction: The asphalt microspheres are added to a rotary kiln equipped with a plasma treatment device, heated to 280°C in an oxygen atmosphere for oxidation treatment for 5 hours to obtain pre-oxidized asphalt microspheres;

[0040] (4) Carbonization treatment: The pre-oxidized asphalt microspheres were added into a carbonization furnace and heated to 700°C for carbonization treatment for 2 h under nitrogen gas protection, and then heated to 1300°C for carbonization treatment for 4 h to obtain asphalt-based spherical hard carbon particles.

[0041] The SEM results show that Figure 1 The hard carbon material has a regular spherical morphology, a smooth surface and no obvious holes. Electrochemical tests show that as a negative electrode material for sodium ion batteries, the first charge and discharge efficiency of the hard carbon material is 93%, and the first charge specific capacity is 326mAh / g. As a negative electrode material for lithium ion batteries, the reversible specific capacity is 435mAh / g, and the capacity at 5C rate is 75% of the capacity at 0.1C rate, with good fast charging performance.

[0042] Example 2

[0043] A method for preparing a pitch-based spherical hard carbon negative electrode material comprises the following steps:

[0044] (1) Cross-linking polymerization: Grind the ethylene tar asphalt raw material with a softening point of 60°C through a 100-mesh sieve, then use terephthalic acid as a cross-linking agent, the cross-linking agent accounts for 30% of the asphalt mass ratio, and use concentrated sulfuric acid as a catalyst, the catalyst accounts for 5% of the asphalt mass ratio, mix the three together, heat to 120°C under N2 protection, and react for 10 hours while stirring to obtain a cross-linked high softening point asphalt;

[0045] (2) Melt spray granulation: The high softening point asphalt is heated to 250°C to obtain a molten liquid, and the molten liquid is spray-cooled and granulated to obtain asphalt microspheres with a D50 of 5 to 8 μm;

[0046] (3) Pre-oxidation reaction: The asphalt microspheres are added to a rotary kiln equipped with a plasma treatment device, heated to 150°C for oxidation treatment for 15 hours in an ozone atmosphere to obtain pre-oxidized asphalt microspheres;

[0047] (4) Carbonization treatment: The pre-oxidized asphalt microspheres were added into a carbonization furnace and heated to 450°C for carbonization treatment for 4 h under argon gas protection, and then heated to 1400°C for carbonization treatment for 6 h to obtain asphalt-based spherical hard carbon particles.

[0048] Example 3

[0049] A method for preparing a pitch-based spherical hard carbon negative electrode material comprises the following steps:

[0050] (1) Cross-linking polymerization: a petroleum asphalt raw material with a softening point of 150°C is ground through a 100-mesh sieve, and then p-methylbenzaldehyde is used as a cross-linking agent, the cross-linking agent accounts for 20% of the asphalt mass ratio, and benzenesulfonic acid is used as a catalyst, the catalyst accounts for 10% of the asphalt mass ratio. The three are mixed evenly, heated to 250°C under N2 protection, and reacted for 1 hour while stirring to obtain a cross-linked high softening point asphalt;

[0051] (2) Melt spray granulation: The high softening point asphalt is heated to 380°C to obtain a melt, and the melt is spray-cooled and granulated to obtain asphalt microspheres with a D50 of 13 to 18 μm;

[0052] (3) Pre-oxidation reaction: the asphalt microspheres are added into a rotary kiln equipped with a plasma treatment device, heated to 350°C for oxidation treatment for 3 h in a nitrogen dioxide atmosphere to obtain pre-oxidized asphalt microspheres;

[0053] (4) Carbonization treatment: The pre-oxidized asphalt microspheres are added into a carbonization furnace and heated to 800°C for carbonization treatment for 0.5 h under the protection of an inert gas, and then the temperature is raised to 1600°C for carbonization treatment for 2 h to obtain asphalt-based spherical hard carbon particles.

[0054] Example 4

[0055] A method for preparing a pitch-based spherical hard carbon negative electrode material comprises the following steps:

[0056] (1) Cross-linking polymerization: A heavy aromatic hydrocarbon asphalt raw material with a softening point of about 100°C is ground through a 100-mesh sieve, and then trioxymethylene is used as a cross-linking agent, the cross-linking agent accounts for 30% of the asphalt mass ratio, and chlorosulfonic acid is used as a catalyst, the catalyst accounts for 8% of the asphalt mass ratio. The three are mixed evenly, heated to 180°C under N2 protection, and reacted for 6 hours while stirring to obtain a cross-linked high softening point asphalt;

[0057] (2) Melt spray granulation: The high softening point asphalt is heated to 280°C to obtain a molten liquid, and the molten liquid is spray-cooled and granulated to obtain asphalt microspheres with a D50 of 10 to 15 μm;

[0058] (3) Pre-oxidation reaction: The asphalt microspheres are added to a rotary kiln equipped with a plasma treatment device, heated to 250°C in a sulfur trioxide atmosphere for oxidation treatment for 8 hours to obtain pre-oxidized asphalt microspheres;

[0059] (4) Carbonization treatment: The pre-oxidized asphalt microspheres are added into a carbonization furnace and heated to 600°C for carbonization treatment for 2 h under the protection of an inert gas, and then the temperature is raised to 1200°C for carbonization treatment for 6 h to obtain asphalt-based spherical hard carbon particles.

[0060] Comparative Example 1

[0061] A method for preparing a pitch-based hard carbon negative electrode material comprises the following steps:

[0062] (1) Melt spray granulation: Coal tar pitch is heated to 300°C to obtain a molten liquid, and the molten liquid is spray-cooled and granulated to obtain pitch microspheres with a D50 of 8 to 12 μm;

[0063] (2) Pre-oxidation reaction: The asphalt microspheres are added to a rotary kiln equipped with a plasma treatment device, heated to 280°C in an oxygen atmosphere for oxidation treatment for 5 hours to obtain pre-oxidized asphalt particles;

[0064] (3) Carbonization treatment: The pre-oxidized asphalt microspheres were added into a carbonization furnace and heated to 700 °C for carbonization treatment for 2 h under the protection of inert gas, and then heated to 1300 °C for carbonization treatment for 4 h to obtain asphalt-based hard carbon particles.

[0065] Asphalt that has not been cross-linked and polymerized can be spray-granulated into spherical particles, but during the pre-oxidation process, due to the low softening point, oxygen cannot diffuse into the material, resulting in insufficient oxidation, and the asphalt particles melt and agglomerate, making it difficult to maintain a spherical shape. The tap density is only 0.75g / cm3 , the sodium storage capacity is about 185mAh / g.

[0066] Comparative Example 2

[0067] A method for preparing a pitch-based hard carbon negative electrode material comprises the following steps:

[0068] (1) Cross-linking polymerization: Grind coal tar pitch raw material with a softening point of 80 degrees through a 100-mesh sieve, then use terephthalaldehyde as a cross-linking agent, the cross-linking agent accounts for 10% of the asphalt mass ratio, and use p-toluenesulfonic acid as a catalyst, the catalyst accounts for 15% of the asphalt mass ratio, mix the three together, heat to 160°C under N2 protection, and react for 8 hours while stirring to obtain a cross-linked high softening point asphalt;

[0069] (2) Pre-oxidation reaction: After the asphalt is crushed into powder, it is added to a rotary kiln equipped with a plasma treatment device and heated to 280°C for oxidation treatment for 5 hours in an oxygen atmosphere to obtain pre-oxidized asphalt powder;

[0070] (3) Carbonization treatment: The pre-oxidized asphalt microspheres were added into a carbonization furnace and heated to 700 °C for carbonization treatment for 2 h under the protection of inert gas, and then heated to 1300 °C for carbonization treatment for 4 h to obtain asphalt-based hard carbon material.

[0071] There is no melt spray granulation step, the asphalt particles are not spherical, the oxidation process is not uniform and sufficient, and the tap density and capacity are low. The tap density is only 0.82g / cm 3 , the sodium storage capacity is about 260mAh / g.

[0072] Comparative Example 3

[0073] A method for preparing a pitch-based hard carbon negative electrode material comprises the following steps:

[0074] (1) Cross-linking polymerization: Grind coal tar pitch raw material with a softening point of 80 degrees through a 100-mesh sieve, then use terephthalaldehyde as a cross-linking agent, the cross-linking agent accounts for 10% of the asphalt mass ratio, and use p-toluenesulfonic acid as a catalyst, the catalyst accounts for 15% of the asphalt mass ratio, mix the three together, heat to 160°C under N2 protection, and react for 8 hours while stirring to obtain a cross-linked high softening point asphalt;

[0075] (2) Melt spray granulation: The high softening point asphalt is heated to 300°C to obtain a melt, and the melt is spray-cooled and granulated to obtain asphalt microspheres with a D50 of 8 to 12 μm;

[0076] (3) Pre-oxidation reaction: The asphalt microspheres are added into a rotary kiln and heated to 280°C for oxidation treatment for 5 h in an oxygen atmosphere to obtain pre-oxidized asphalt microspheres;

[0077] (4) Carbonization treatment: The pre-oxidized asphalt microspheres are added into a carbonization furnace and heated to 700°C for carbonization treatment for 2 h under the protection of an inert gas, and then the temperature is raised to 1300°C for carbonization treatment for 4 h to obtain asphalt-based spherical hard carbon particles.

[0078] There is no plasma treatment device in the pre-oxidation process, and the oxygen activity is not high, which makes it difficult to diffuse into the asphalt particles, resulting in insufficient oxidation and easy formation of skin-core structure, resulting in low tap density and capacity. The tap density is only 0.73g / cm 3 , the sodium storage capacity is about 225mAh / g.

[0079] Implementation effect example

[0080] The carbon materials prepared in Examples 1-4 and Comparative Examples 1-3 were used as negative electrode materials for sodium batteries and lithium batteries to compare electrochemical performance. The specific experimental process was as follows: carbon materials prepared in Examples 1-4 and Comparative Examples 1-3: carbon nanotubes: CMC binder = 90:5:5; sodium sheets or lithium sheets were used as counter electrodes and reference electrodes; the electrolyte was 1M NaPF6-EC / DMC (volume ratio 1:1) or 1M LiPF6-EC / DMC (volume ratio 1:1), and the charge and discharge rate was 0.1C. The experimental results are shown in Table 1.

[0081] Table 1 Comparison of the performance of the negative electrode materials prepared in Examples 1-4 and Comparative Examples 1-3

[0082]

Claims

1. A pitch-based spherical hard carbon negative electrode material, characterized in that: Includes the following raw materials: asphalt, cross-linking agent, catalyst; The cross-linking agent is one or more of terephthalaldehyde, terephthalic alcohol, p-tolualdehyde, p-toluyl alcohol, benzaldehyde, and trioxymethylene; The catalyst is one or more of p-toluenesulfonic acid, concentrated sulfuric acid, benzenesulfonic acid and chlorosulfonic acid.

2. The pitch-based spherical hard carbon negative electrode material according to claim 1, characterized in that: The mass ratio of asphalt to cross-linking agent is 100:10-40, and the mass ratio of asphalt to catalyst is 100:5-15.

3. The pitch-based spherical hard carbon negative electrode material according to claim 1 or 2, characterized in that: The asphalt has a softening point of 50 to 150°C.

4. The method for preparing the pitch-based spherical hard carbon negative electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Cross-linking polymerization: The asphalt, cross-linking agent and catalyst are mixed evenly and reacted while stirring to obtain a cross-linked high softening point asphalt; (2) Melt spray granulation: The high softening point asphalt is heated to obtain a molten liquid, and the molten liquid is spray granulated to obtain asphalt microspheres with controllable particle size; (3) Pre-oxidation treatment: The asphalt microspheres are heated and oxidized in an oxidizing atmosphere to obtain pre-oxidized asphalt microspheres; (4) Carbonization treatment: Pre-oxidized asphalt microspheres are carbonized to obtain asphalt-based spherical hard carbon particles.

5. The preparation method according to claim 4, characterized in that: The reaction in step (1) is carried out under the protection of an inert gas; And / or, the reaction conditions are: temperature 120-250° C., time 1-10 h.

6. The preparation method according to claim 4, characterized in that: The oxidizing atmosphere in step (3) is one or more of oxygen, ozone, air, nitrogen dioxide, and sulfur trioxide; And / or, the heating oxidation treatment conditions are: temperature of 150-350° C. and time of 3-15 hours.

7. The preparation method according to claim 4, characterized in that: The carbonization process of step (4) is as follows: heating to 450-800° C. for carbonization treatment for 0.5-4 h under the protection of inert gas, and then heating to 1200-1600° C. for carbonization treatment for 2-6 h.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The carbonization in step (3) is carried out in a furnace equipped with a plasma treatment device; preferably, in a rotary furnace.

9. Use of the asphalt-based spherical hard carbon negative electrode material described in any one of claims 1 to 3 or the asphalt-based spherical hard carbon negative electrode material prepared by the method described in any one of claims 4 to 8 in lithium-ion batteries and / or sodium-ion batteries.

10. The use according to claim 9, characterized in that: Used as negative electrode material.

Citation Information

Cited By

  • Method for preparing hard carbon microspheres by utilizing solvothermal catalytic crosslinking of coal pitch and application

    CN119735199A

  • Carbon material, method for producing the same, and method for using the same

    CN119873795B

  • Asphalt-based hard carbon negative electrode material for sodium-ion battery and preparation method of asphalt-based hard carbon negative electrode material

    CN120081362A

  • Hard carbon material and preparation method thereof, negative pole piece and battery

    CN120483095A

  • Preparation method of hard carbon negative electrode material

    CN120483106A