Rapid activation method of fuel cell stack composed of low-platinum-loading membrane electrode
By performing a rapid activation method on the fuel cell stack composed of low-platinum load membrane electrodes, the specific operating conditions and current density changes are used to solve the problems of long activation time and consumption, and rapid activation within 48 minutes to 50 minutes and Performance improvement.
Patent Information
- Application Number
- CN202411182813.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The fuel cell stack composed of low-platinum load membrane electrodes has a long activation time, consumes more manpower and hydrogen, and has low activation efficiency, which goes against the original intention of reducing costs.
The rapid activation method is adopted, including purge the anode and cathode of the fuel cell stack composed of low-platinum load membrane electrodes, setting specific stack activation operating conditions, and changing the current density between primary and secondary pull loads , and after secondary pulling load, the current density increases slightly during multiple times, gradually reducing the cathode metering ratio and achieving rapid activation.
The rapid activation of a fuel cell composed of a low-platinum load membrane electrode is completed within 48 minutes to 50 minutes, significantly shortening the activation time and improving polarization performance. It is suitable for low-platinum load membrane electrodes with a platinum load of less than 0.3mg/cm2 A fuel cell composed of.
Smart Images

Figure CN119050409A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a rapid activation method for a fuel cell stack composed of a membrane electrode with a low platinum loading. Background Art
[0002] The core component of the proton exchange membrane fuel cell (PEMFC) is the membrane electrode, and the performance of the membrane electrode largely determines the performance of the fuel cell. The materials that make up the membrane electrode assembly (MEA) include catalysts, and the content of platinum, rhodium, palladium, etc. in the catalyst has a great influence on its performance. In order to enable the PEMFC to quickly reach its optimal state and working performance after starting to work, the MEA is usually activated before it is prepared and assembled into a fuel cell stack for normal test operation.
[0003] Activation is generally considered to include the following processes: (1) humidification of the proton exchange membrane; (2) establishment of material transfer channels; (3) optimization of the electrode structure; (4) improvement of the activity and utilization of the catalyst layer. PEMFC activation can enhance the hydration of the proton exchange membrane and improve the output performance of the fuel cell. Therefore, the choice of MEA activation method is very important for the performance of PEMFC. The traditional PEMFC activation process usually takes several hours or days, which not only consumes a large amount of hydrogen, but also delays the PEMFC production cycle. Reasonable activation methods can not only improve the performance of PEMFC, but also greatly reduce the activation time and reduce the amount of gas fuel used, thereby significantly reducing the activation cost.
[0004] At present, the platinum loading of conventional membrane electrode cathode is 0.4±0.05mg / cm 2 When the platinum loading reaches 0.3 mg / cm 2 The following is a low platinum loading. Reducing Pt / C reduces material costs to a certain extent and is the trend of future development.
[0005] However, for the stack composed of membrane electrodes with low platinum loading, rapid activation is a problem. The existing activation process takes more than 3 hours or several days to make the membrane electrode perform optimally, which consumes a lot of manpower and materials (hydrogen), resulting in the cost saved from reducing the platinum loading being invested in the activation process, which goes against the original intention of reducing costs. Summary of the invention
[0006] The purpose of the present invention is to provide a method for rapid activation of a fuel cell stack composed of a membrane electrode with a low platinum loading, aiming to solve the problems of long activation time, labor consumption, large amount of hydrogen materials and low activation efficiency of the existing fuel cell stack composed of a membrane electrode with a low platinum loading.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A method for rapidly activating a fuel cell stack composed of a membrane electrode with a low platinum loading, specifically comprising the following steps:
[0009] S01. Purging the anode and cathode of a fuel cell stack composed of a low platinum loading membrane electrode;
[0010] S02. Set the stack activation operating conditions: the stack temperature is 60-100°C, the anode / cathode pressure is 100-190 / 80-170 kPa, the anode / cathode humidity is 30-100 / 30-100%, and the anode / cathode stoichiometric ratio is 1.5-2.0 / 1.6-2.2;
[0011] S03. Pull load to 1.1-1.2A / cm 2 , maintain for 4-6 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.05-1.08, maintain for 18-22 seconds, and restore the flow rate for 50 seconds-1 minute;
[0012] S04. Secondary loading to 1.9-2.1A / cm 2 , maintain for 4-6 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10-1.3, maintain for 18-22 seconds, and restore the flow rate for 50 seconds-1 minute;
[0013] S05. According to 0.09-0.11A / cm 2 The increase in the amount of loading is gradually increased 5-7 times. After each loading, it is maintained for 4-6 minutes, the anode stoichiometric ratio is kept unchanged, the cathode stoichiometric ratio is reduced to 1.10-1.3, maintained for 18-22 seconds, and the recovery flow is maintained for 50 seconds to 1 minute;
[0014] S06. Reduce to the rated electrical density point and maintain for 4-6 minutes to complete activation.
[0015] Preferably, in step S01:
[0016] The low platinum loading is a platinum loading of 0.3 mg / cm 2 the following.
[0017] The gas used for the purge is nitrogen;
[0018] The purging is specifically: purging with nitrogen for 2-4 minutes.
[0019] Further preferably, before purging, the contaminants are washed away by washing with water.
[0020] Preferably, in step S02:
[0021] The stack activation operating conditions are as follows: stack temperature 60° C., anode / cathode pressure 190 / 170 kPa, anode / cathode humidity 100 / 100%, and anode / cathode stoichiometric ratio 1.7 / 2.2.
[0022] Preferably, in step S03:
[0023] Specifically: one pull load to 1.2A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.08, maintain for 20 seconds, and restore the flow rate to maintain for 1 minute.
[0024] Preferably, in step S04:
[0025] Specifically: Secondary pull to 2.0A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate to maintain for 1 minute.
[0026] Preferably, in step S05:
[0027] Specifically: according to 0.1A / cm 2 The load was pulled 6 times in succession with an increasing amount. After each loading, it was maintained for 5 minutes, keeping the anode stoichiometric ratio unchanged, and the cathode stoichiometric ratio was reduced to 1.10 and maintained for 20 seconds, and the flow was restored and maintained for 1 minute.
[0028] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0029] The rapid activation method of the patent application is used for a fuel cell composed of a membrane electrode with a low platinum loading. ... 2 The increase in the amount of anode stoichiometry is maintained unchanged, and the cathode stoichiometry is gradually reduced to a constant value (1.10-1.3), so that the rapid activation of the fuel cell composed of a low platinum loading membrane electrode can be completed within 48min-50min. It is suitable for a platinum loading of 0.3mg / cm 2 The following fuel cell composed of a low platinum loading membrane electrode; through a low potential activation method, the membrane electrode activation time can be effectively shortened, and the polarization performance of the fuel cell composed of a low platinum loading membrane electrode can be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a low potential activation flow chart provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In addition, if there are descriptions involving "once", "twice", etc. in the embodiments of the present invention, the descriptions of "once", "twice", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "once" and "twice" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0033] At present, the existing fuel cell stack composed of membrane electrode with low platinum loading has the problems of long activation time, labor consumption, more hydrogen materials and low activation efficiency. The embodiment of the present invention provides a method for rapid activation of a fuel cell stack composed of membrane electrode with low platinum loading.
[0034] Example 1
[0035] A method for rapidly activating a fuel cell stack composed of a membrane electrode with a low platinum loading, specifically comprising the following steps:
[0036] S01. The anode and cathode of the fuel cell stack composed of a low platinum loading membrane electrode are purged with nitrogen for 3 minutes;
[0037] S02. Set the stack activation operating conditions: stack temperature 60°C, anode / cathode pressure 190 / 170 kPa, anode / cathode humidity 100 / 100%, anode / cathode stoichiometric ratio 1.7 / 2.2;
[0038] S03. Load 1.2A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.08, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0039] S04. Load 2.0A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0040] S05. Load 2.1A / cm 2, maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0041] S06. Load 2.2A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0042] S07. Load 2.3A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0043] S08. Load 2.4A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0044] S09. Load 2.5A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0045] S10. Pulling load 2.6A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0046] S11. Reduce to the rated electrical density point and maintain for 5 minutes to complete activation.
[0047] The low potential activation flow chart of the rapid activation method of Example 1 is as follows Figure 1 As shown, activation is performed at a relatively low potential and the total activation time is 48 minutes, which is much shorter than the existing activation time for fuel cell stacks composed of membrane electrodes with low platinum loading.
[0048] Example 2
[0049] A method for rapidly activating a fuel cell stack composed of a membrane electrode with a low platinum loading, specifically comprising the following steps:
[0050] S01. The anode and cathode of the fuel cell stack composed of a low platinum loading membrane electrode were purged with nitrogen for 4 minutes;
[0051] S02. Set the stack activation operating conditions: stack temperature 100°C, anode / cathode pressure 100 / 80 kPa, anode / cathode humidity 30 / 30%, anode / cathode stoichiometric ratio 1.7 / 2.2;
[0052] S03. Load 1.1A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.05, maintain for 22 seconds, and restore the flow rate to maintain for 50 minutes;
[0053] S04. Load 1.9A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0054] S05. Load 2.0A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0055] S06. Load 2.1A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0056] S07. Load 2.2A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0057] S08. Load 2.3A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0058] S09. Load 2.4A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0059] S10. Pulling load 2.5A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate for 1 minute;
[0060] S11. The temperature is reduced to the rated electric density point and maintained for 5 minutes to complete the activation. The total activation time is 50 minutes, which is much shorter than the activation time of the existing fuel cell stack composed of low platinum loading membrane electrode.
[0061] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0062] The rapid activation method of the patent application is used for a fuel cell composed of a membrane electrode with a low platinum loading. ... 2 The increase in the amount of anode stoichiometry is maintained unchanged, and the cathode stoichiometry is gradually reduced to a constant value (1.10-1.3), so that the rapid activation of the fuel cell composed of a low platinum loading membrane electrode can be completed within 48min-50min. It is suitable for a platinum loading of 0.3mg / cm 2 The following fuel cell composed of a low platinum loading membrane electrode; through a low potential activation method, the membrane electrode activation time can be effectively shortened, and the polarization performance of the fuel cell composed of a low platinum loading membrane electrode can be significantly improved.
[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for rapid activation of a fuel cell stack composed of a low platinum loading membrane electrode, characterized in that: The specific steps include: S01. Purging the anode and cathode of a fuel cell stack composed of a low platinum loading membrane electrode; S02. Set the stack activation operating conditions: the stack temperature is 60-100°C, the anode / cathode pressure is 100-190 / 80-170 kPa, the anode / cathode humidity is 30-100 / 30-100%, and the anode / cathode stoichiometric ratio is 1.5-2.0 / 1.6-2.2; S03. Pull load to 1.1-1.2A / cm 2 , maintain for 4-6 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.05-1.08, maintain for 18-22 seconds, and restore the flow rate for 50 seconds-1 minute; S04. Secondary loading to 1.9-2.1A / cm 2 , maintain for 4-6 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10-1.3, maintain for 18-22 seconds, and restore the flow rate for 50 seconds-1 minute; S05. According to 0.09-0.11A / cm 2 The increase in the amount of loading is gradually increased 5-7 times. After each loading, it is maintained for 4-6 minutes, the anode stoichiometric ratio is kept unchanged, the cathode stoichiometric ratio is reduced to 1.10-1.3, maintained for 18-22 seconds, and the recovery flow is maintained for 50 seconds to 1 minute; S06. Reduce to the rated electrical density point and maintain for 4-6 minutes to complete activation.
2. The rapid activation method for a fuel cell stack composed of a membrane electrode with a low platinum loading according to claim 1, characterized in that: In step S01: the low platinum loading is a platinum loading of 0.3 mg / cm 2 the following.
3. The rapid activation method for a fuel cell stack composed of a membrane electrode with a low platinum loading according to claim 1, characterized in that: In step S01: the gas used for purging is nitrogen.
4. The rapid activation method for a fuel cell stack composed of a membrane electrode with a low platinum loading according to claim 1, characterized in that: The purging is specifically: purging with nitrogen for 2-4 minutes.
5. The rapid activation method for a fuel cell stack composed of a membrane electrode with a low platinum loading according to claim 1, characterized in that: In step S02: the stack activation operating conditions are: stack temperature 60°C, anode / cathode pressure 190 / 170 kPa, anode / cathode humidity 100 / 100%, anode / cathode stoichiometric ratio 1.7 / 2.
2.
6. The method for rapid activation of a fuel cell stack composed of a membrane electrode with a low platinum loading according to claim 1, characterized in that: In step S03: Specifically: pull the load to 1.2A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.08, maintain for 20 seconds, and restore the flow rate to maintain for 1 minute.
7. The rapid activation method for a fuel cell stack composed of a membrane electrode with a low platinum loading according to claim 1, characterized in that: In step S04: specifically: the secondary pull is increased to 2.0A / cm 2 , maintain for 5 minutes, keep the anode stoichiometric ratio unchanged, reduce the cathode stoichiometric ratio to 1.10, maintain for 20 seconds, and restore the flow rate to maintain for 1 minute.
8. The method for rapid activation of a fuel cell stack composed of a membrane electrode with a low platinum loading according to claim 1, characterized in that: In step S05: specifically: according to 0.1A / cm 2 The load was pulled 6 times in succession with an increasing amount. After each loading, it was maintained for 5 minutes, keeping the anode stoichiometric ratio unchanged, and the cathode stoichiometric ratio was reduced to 1.10 and maintained for 20 seconds, and the flow was restored and maintained for 1 minute.
Citation Information
Patent Citations
Universal fuel cell activation test method
CN110676485A
Rapid activation method of fuel cell stack
CN114447376A
Fuel cell system and activation method for fuel cell
US20100119887A1
Cited By
General rapid activation method for proton exchange membrane fuel cell stack