Gel electrolyte composition, gel electrolyte, preparation method of gel electrolyte and magnesium ion battery
By using a gel electrolyte composition of ether compounds, magnesium salts, and Lewis acid catalysts in magnesium-ion batteries, a gel polymer is formed through in-situ ring-opening polymerization, which solves the problem of poor electrolyte-electrode interface stability in magnesium-ion batteries, improves battery conductivity and cycle stability, and enhances high-voltage stability and rate performance.
Patent Information
- Application Number
- CN202411462555.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-29
AI Technical Summary
Magnesium-ion batteries have poor interfacial stability between the electrolyte and the electrode, resulting in low ionic conductivity and poor battery charge-discharge performance.
A gel electrolyte composition comprising an ether compound, a magnesium salt, and a Lewis acid catalyst is used to form a gel polymer through an in-situ ring-opening polymerization reaction, thereby improving the interfacial stability between the magnesium metal anode and the electrolyte. The conductivity and electrochemical window are optimized by controlling the component ratio and polymerization reaction conditions.
It improves the room temperature conductivity, electrochemical window, and cycle stability of magnesium-ion batteries, enhances the deposition and dissolution uniformity of magnesium metal anodes, reduces the dissolution and shuttle effect of polysulfides, and improves the high voltage stability and rate performance of batteries.
Smart Images

Figure CN119050469A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of magnesium ion batteries, and in particular to a gel electrolyte composition, a gel electrolyte and a preparation method thereof, and a magnesium ion battery. Background Art
[0002] Traditional batteries mostly use electrolytes because they have high ionic conductivity and charge and discharge efficiency, but electrolytes are easy to leak, highly corrosive, flammable and explosive, which poses a great safety hazard to the battery. So people turned their attention to all-solid-state batteries. Therefore, all-solid-state batteries have high safety stability and long cycle life, but the interface compatibility of all-solid-state electrolytes is poor, the impedance is high, and the room temperature ionic conductivity is low, which makes it difficult to meet the battery requirements. Gel electrolyte (GPE) has the advantages of both electrolytes and all-solid-state electrolytes. While improving safety, the interface compatibility is better than that of all-solid-state electrolytes, and the ionic conductivity is also improved accordingly. Therefore, gel electrolyte solid-state batteries are one of the most promising new generation of high-performance energy storage devices. However, the gel electrolyte supported by polypropylene diaphragms prepared by traditional methods (such as extraction method, phase transfer method, etc.) has poor interface contact with positive and negative electrodes, low ionic conductivity of the battery, and poor thermal stability, and has poor battery charge and discharge performance in high energy density battery systems. Compared with the defects of liquid electrolytes, such as volatility, flammability and unsafety, polymer electrolytes have higher safety performance, so that magnesium batteries assembled with polymer electrolytes have both high energy density and safety performance.
[0003] In order to improve a series of problems such as poor contact between polymer electrolyte and electrode interface, many researchers currently use in-situ polymerization electrolyte preparation methods, which are simple to operate, easy to control, and have great experimental controllability. The preparation of polymer gel electrolytes by in-situ polymerization can effectively reduce the interface impedance between electrolyte and electrode, thereby helping to improve ionic conductivity and battery cycle stability.
[0004] In addition, in the post-lithium-ion battery era, rechargeable magnesium batteries have attracted widespread attention due to their potential for high energy density, abundant raw material sources, and safe use of metal negative electrodes. Therefore, the development of in-situ polymerized gel electrolytes based on magnesium batteries is of great significance to battery development and application. Summary of the invention
[0005] The main purpose of the present invention is to provide a gel electrolyte composition, a gel electrolyte and a preparation method thereof, and a magnesium ion battery, so as to solve the problem of poor interface stability between the electrolyte and the electrode in the magnesium ion battery in the prior art.
[0006] To achieve the above object, according to one aspect of the present invention, a gel electrolyte composition is provided, which comprises, by weight, 25 to 75 parts of an ether compound, 15 to 45 parts of a magnesium salt and 0.1 to 15 parts of a Lewis acid catalyst.
[0007] Furthermore, the gel electrolyte composition comprises 67 to 72 parts of an ether compound, 17 to 31 parts of a magnesium salt and 2 to 6 parts of a Lewis acid catalyst.
[0008] Further, the ether compound is selected from any one or more of tetrahydrofuran, 1,3-dioxane, tetrahydropyran, 1,3-dioxane, 1,4-dioxane and 1,3,5-trioxane; and / or the magnesium salt is selected from any one or more of bis(trifluoromethanesulfonylimide)magnesium, phenylmagnesium chloride, magnesium tetrakis(hexafluoroisopropyloxy)borate, magnesium perfluoropinacol borate, magnesium borohydride and magnesium tetrachloroaluminate; and / or the Lewis acid catalyst is selected from any one or more of boron trifluoride, magnesium chloride, aluminum chloride, trimethylaluminum, magnesium trifluoromethanesulfonate and tris(hexafluoroisopropyl)borate.
[0009] Furthermore, the ether compound is tetrahydrofuran, the magnesium salt is magnesium tetrakis(hexafluoroisopropyloxy)borate, the Lewis acid catalyst is tris(hexafluoroisopropyl)borate, and the mass ratio of tetrahydrofuran, magnesium tetrakis(hexafluoroisopropyloxy)borate and tris(hexafluoroisopropyl)borate is 65-75:25-30:1-5.
[0010] According to another aspect of the present invention, a method for preparing a gel electrolyte is provided, the method comprising: mixing a gel electrolyte composition and injecting the mixture into a dry battery cell to perform an in-situ ring-opening polymerization reaction to obtain a gel electrolyte; wherein the gel electrolyte composition is the aforementioned gel electrolyte composition.
[0011] Furthermore, the temperature of the in-situ ring-opening polymerization reaction is 20 to 120° C.; and / or, the time of the in-situ ring-opening polymerization reaction is 1 to 24 h; and / or, the pressure of the in-situ ring-opening polymerization reaction is 0.1 to 60 MPa.
[0012] Furthermore, the temperature of the in-situ ring-opening polymerization reaction is 25 to 75° C.; and / or, the time of the in-situ ring-opening polymerization reaction is 6 to 16 hours; and / or, the pressure of the in-situ ring-opening polymerization reaction is 10 to 15 MPa; preferably, the in-situ ring-opening polymerization reaction is carried out in a static state.
[0013] According to another aspect of the present invention, a gel electrolyte is provided. The gel electrolyte is prepared by the above-mentioned preparation method.
[0014] Further, the thickness of the gel electrolyte is 70 to 700 μm; and / or the ionic conductivity of the gel electrolyte at 25° C. is 3.58×10 -3 ~5.28×10 -3 S / cm; and / or, the electrochemical window of the gel electrolyte is not less than 3.5V.
[0015] According to another aspect of the present invention, a magnesium ion battery is provided, comprising a positive electrode sheet, an electrolyte and a negative electrode sheet, wherein the electrolyte is the aforementioned gel electrolyte.
[0016] By applying the technical solution of the present invention, the Lewis acid catalyst in the gel electrolyte composition attacks the multi-electron oxygen in the ether compound due to the lack of electrons, thereby catalyzing the ring-opening polymerization reaction of the ether compound to form a gel polymer, and the gel polymer can help the magnesium salt dissociate, thereby helping to improve the room temperature conductivity of the gel electrolyte. The gel electrolyte is applied to the magnesium ion battery, which is conducive to uniform deposition and dissolution of the magnesium metal negative electrode, thereby helping to improve the stability of the interface between the magnesium metal negative electrode and the gel electrolyte. In addition, since the free solvent in the gel polymer is reduced, it is helpful to improve the electrochemical window of the gel electrolyte, and then help to improve the high voltage stability of the magnesium ion battery. At the same time, the semi-solid property of the gel polymer electrolyte alleviates the severe dissolution and shuttling of polysulfides in the liquid electrolyte, causing a large loss of active substances, thereby helping to improve the rate performance and cycle stability of the magnesium ion battery. It is preferred to control the weight of each component in the gel electrolyte composition within the above range, which helps to improve the synergistic effect between the components, thereby helping to further improve the room temperature conductivity and electrochemical window of the gel electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0018] Figure 1 An optical photograph of the gel polymer electrolyte in Example 1 of the present application is shown;
[0019] Figure 2 The LSV curve of the magnesium ion battery assembled by the gel polymer electrolyte in Example 1 of the present application is shown;
[0020] Figure 3 The long cycle curve of the magnesium ion battery assembled with the gel polymer electrolyte in Example 2 of the present application at 30°C is shown;
[0021] Figure 4The figure shows the morphology of the magnesium sheet surface after the magnesium ion battery assembled with the gel polymer electrolyte in Example 2 of the present application has been cycled for 1000 times;
[0022] Figure 5 The long cycle curve of the magnesium ion battery assembled with the gel polymer electrolyte in Example 3 of the present application at 30° C. is shown. DETAILED DESCRIPTION
[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0024] As analyzed in the background technology of the present application, magnesium ion batteries in the prior art have the problem of poor interface stability between the electrolyte and the electrode. In order to solve the above problem, the present application provides a gel electrolyte composition, a gel electrolyte and a preparation method thereof, and a magnesium ion battery.
[0025] In a typical embodiment of the present application, a gel electrolyte composition is provided, which includes, by weight, 25 to 75 parts of an ether compound, 15 to 45 parts of a magnesium salt, and 0.1 to 15 parts of a Lewis acid catalyst.
[0026] The Lewis acid catalyst in the gel electrolyte composition attacks the multi-electron oxygen in the ether compound due to the lack of electrons, thereby catalyzing the ring-opening polymerization reaction of the ether compound to form a gel polymer. The gel polymer can help the magnesium salt dissociate, thereby helping to improve the room temperature conductivity of the gel electrolyte. The gel electrolyte is applied to the magnesium ion battery, which is conducive to uniform deposition and dissolution of the magnesium metal negative electrode, thereby helping to improve the stability of the interface between the magnesium metal negative electrode and the gel electrolyte. In addition, since the free solvent in the gel polymer is reduced, it helps to improve the electrochemical window of the gel electrolyte, and then helps to improve the high voltage stability of the magnesium ion battery. At the same time, the semi-solid property of the gel polymer electrolyte alleviates the severe dissolution and shuttling of polysulfides in the liquid electrolyte, causing a large loss of active substances, thereby helping to improve the rate performance and cycle stability of the magnesium ion battery. It is preferred to control the weight of each component in the gel electrolyte composition within the above range, which helps to improve the synergistic effect between the components, thereby helping to further improve the room temperature conductivity and electrochemical window of the gel electrolyte.
[0027] In order to further improve the room temperature conductivity and electrochemical window of the gel electrolyte, in one embodiment of the present application, the gel electrolyte composition preferably includes 67 to 72 parts of an ether compound, 17 to 31 parts of a magnesium salt and 2 to 6 parts of a Lewis acid catalyst.
[0028] In one embodiment of the present application, the ether compound is selected from any one or more of tetrahydrofuran, 1,3-dioxolane, tetrahydropyran, 1,3-dioxane, 1,4-dioxane and 1,3,5-trioxane; and / or the magnesium salt is selected from any one or more of bis(trifluoromethanesulfonylimide)magnesium, phenylmagnesium chloride, magnesium tetrakis(hexafluoroisopropyloxy)borate, magnesium perfluoropinacol borate, magnesium borohydride and magnesium tetrachloroaluminate; and / or the Lewis acid catalyst is selected from any one or more of boron trifluoride, magnesium chloride, aluminum chloride, trimethylaluminum, magnesium trifluoromethanesulfonate and tris(hexafluoroisopropyl)borate.
[0029] It is preferred to control the type of ether compound within the above range, which helps to improve the efficiency of the ring-opening polymerization. It is preferred to control the type of magnesium salt within the above range, which helps to obtain higher ion conductivity. It is preferred to control the type of Lewis acid catalyst within the above range, which helps to control the ring-opening polymerization time.
[0030] In one embodiment of the present application, the ether compound is tetrahydrofuran, the magnesium salt is magnesium tetrakis(hexafluoroisopropyloxy)borate, the Lewis acid catalyst is tris(hexafluoroisopropyl)borate, and the mass ratio of tetrahydrofuran, magnesium tetrakis(hexafluoroisopropyloxy)borate and tris(hexafluoroisopropyl)borate is 65-75:25-30:1-5.
[0031] Preferably, the mass ratio of tetrahydrofuran, magnesium tetrakis(hexafluoroisopropyloxy)borate and tris(hexafluoroisopropyl)borate is controlled within the above range, which helps tris(hexafluoroisopropyl)borate to effectively catalyze the ring-opening polymerization of tetrahydrofuran, thereby helping to obtain a stable gel polymer electrolyte.
[0032] In another typical embodiment of the present application, a method for preparing a gel electrolyte is provided, the method comprising: mixing a gel electrolyte composition and injecting the mixture into a dry battery cell to perform an in-situ ring-opening polymerization reaction to obtain a gel electrolyte; wherein the gel electrolyte composition is the aforementioned gel electrolyte composition.
[0033] After the gel electrolyte composition is mixed, it is injected into the dry battery cell for in-situ ring-opening polymerization, which helps to improve the interaction between the gel electrolyte and the electrode, thereby helping to regulate the interface of the magnesium metal negative electrode in the magnesium ion battery and the solubility of polysulfides, thereby helping to improve the rate performance and cycle stability of the magnesium ion battery. In addition, the preparation method of the gel polymer electrolyte of the present application has the advantages of simple process and low cost.
[0034] In one embodiment of the present application, the temperature of the in-situ ring-opening polymerization reaction is 20-120° C.; and / or, the time of the in-situ ring-opening polymerization reaction is 1-24 h; and / or, the pressure of the in-situ ring-opening polymerization reaction is 0.1-60 MPa.
[0035] Too high a polymerization reaction temperature is not conducive to improving the stability of the gel electrolyte, too low a polymerization reaction temperature is not conducive to accelerating the polymerization reaction rate, too high an in-situ ring-opening polymerization reaction pressure is likely to lead to excessively large polymer molecular weight, which is not conducive to improving the ionic conductivity of the polymer, and too low an in-situ ring-opening polymerization reaction pressure is not conducive to uniform polymerization. It is preferred to control the polymerization reaction temperature, time and pressure within the above range, which helps to improve the efficiency of forming the gel electrolyte and the comprehensive performance of the gel electrolyte.
[0036] In order to further improve the efficiency of forming the gel electrolyte, in one embodiment of the present application, the temperature of the in-situ ring-opening polymerization reaction is preferably 25 to 75° C.; and / or the time of the in-situ ring-opening polymerization reaction is 6 to 16 h; and / or the pressure of the in-situ ring-opening polymerization reaction is 10 to 15 MPa; preferably, the in-situ ring-opening polymerization reaction is carried out in a static state.
[0037] In another typical embodiment of the present application, a gel electrolyte is provided. The gel electrolyte is prepared by the aforementioned preparation method.
[0038] The gel electrolyte prepared by the preparation method has higher room temperature conductivity and electrochemical window.
[0039] In one embodiment of the present application, the thickness of the gel electrolyte is 70-700 μm; and / or the ionic conductivity of the gel electrolyte at 25° C. is 3.58×10 -3 ~5.28×10 -3 S / cm; and / or, the electrochemical window of the gel electrolyte is not less than 3.5V.
[0040] Applying the gel electrolyte having the above-mentioned thickness, ionic conductivity and electrochemical window range to a magnesium ion battery is beneficial for uniform deposition and dissolution of the magnesium metal negative electrode, thereby helping to improve the stability of the interface between the magnesium metal negative electrode and the gel electrolyte, and helping to reduce the dissolution and shuttle effect of polysulfides, thereby helping to improve the rate performance and cycle stability of the magnesium ion battery.
[0041] In another typical embodiment of the present application, a magnesium ion battery is provided, comprising a positive electrode sheet, an electrolyte and a negative electrode sheet, wherein the electrolyte is the aforementioned gel electrolyte.
[0042] Since the magnesium ion battery contains the gel electrolyte of the present application, the magnesium ion battery has higher rate performance and cycle stability.
[0043] The negative electrode sheet includes metal magnesium; wherein the purity of the metal magnesium is greater than 99% and the thickness of the metal magnesium is between 100 and 500 μm. The magnesium ion battery also includes a diaphragm, which is selected from any one or more of a polyethylene (PE) diaphragm, a polypropylene (PP) diaphragm and a glass fiber (GF) diaphragm. The positive active material in the positive electrode sheet is sulfur and / or a copper sulfur compound; wherein the sulfur or copper sulfur compound has a particle size between 100 nm and 10 μm.
[0044] The preparation method of the above-mentioned magnesium ion battery comprises the following steps: in an argon atmosphere, stacking in sequence according to the positive electrode shell-positive electrode sheet-gel polymer electrolyte-negative electrode sheet-steel sheet-shrapnel-negative electrode shell, encapsulating to obtain a magnesium ion battery; or, in an argon atmosphere, stacking in sequence according to the positive electrode shell-positive electrode sheet-diaphragm-negative electrode sheet-steel sheet-shrapnel-negative electrode shell, loading a gel electrolyte precursor solution on the diaphragm, performing in-situ polymerization, and encapsulating to obtain a magnesium ion battery.
[0045] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0046] Example 1
[0047] In an argon glove box, 27 parts of magnesium tetrakis(hexafluoroisopropyloxy)borate and 4 parts of tris(hexafluoroisopropyl)borate were dissolved in 69 parts of tetrahydrofuran by weight to form an in-situ polymerized electrolyte precursor solution. The in-situ polymerized electrolyte precursor solution was injected into the dry battery cell for infiltration, and allowed to react for 16 hours under heating conditions of 25°C. The reaction pressure was 10MPa, and in-situ ring-opening polymerization occurred to form an integrated gel polymer electrolyte in close contact with the battery pole piece, wherein the thickness of the electrolyte was 630μm and the electrochemical window was 3.5V.
[0048] Example 2
[0049] The difference from Example 1 is that, by weight, 31 parts of magnesium bis(trifluoromethanesulfonyl imide) and 2 parts of magnesium chloride are dissolved in 67 parts of 1,3-dioxolane in an argon glove box to form an in-situ polymerized electrolyte precursor solution. The in-situ polymerized electrolyte precursor solution is injected into the dry battery cell for infiltration, and allowed to react for 12 hours at a heating condition of 40°C and a reaction pressure of 10 MPa, and in-situ ring-opening polymerization occurs to form an integrated gel polymer electrolyte in close contact with the battery pole piece.
[0050] Example 3
[0051] The difference from Example 1 is that, by weight, 25 parts of phenylmagnesium chloride and 3 parts of aluminum chloride are dissolved in 72 parts of 1,3-dioxane in an argon glove box to form an in-situ polymerized electrolyte precursor solution. The in-situ polymerized electrolyte precursor solution is injected into the dry battery cell for infiltration, and allowed to react for 10 hours at a heating condition of 60°C and a reaction pressure of 10 MPa, and in-situ ring-opening polymerization occurs to form an integrated gel polymer electrolyte in close contact with the battery pole piece.
[0052] Example 4
[0053] The difference from Example 1 is that, by weight, 17 parts of magnesium perfluoropinacol borate and 6 parts of magnesium trifluoromethanesulfonate are dissolved in 75 parts of 1,4-dioxane in an argon glove box to form an in-situ polymerized electrolyte precursor solution. The in-situ polymerized electrolyte precursor solution is injected into the dry battery cell for infiltration, and allowed to stand for reaction at 35°C for 15 hours under a heating condition of 12 MPa, and in-situ ring-opening polymerization occurs to form an integrated gel polymer electrolyte in close contact with the battery pole piece.
[0054] Example 5
[0055] The difference from Example 1 is that, by weight, 21 parts of magnesium tetrachloroaluminate and 5 parts of boron trifluoride are dissolved in 74 parts of tetrahydropyran in an argon glove box to form an in-situ polymerized electrolyte precursor solution. The in-situ polymerized electrolyte precursor solution is injected into the dry battery cell for infiltration, and allowed to react for 6 hours at a heating condition of 75° C. The reaction pressure is 12 MPa, and in-situ ring-opening polymerization occurs to form an integrated gel polymer electrolyte in close contact with the battery pole piece.
[0056] Example 6
[0057] The difference from Example 1 is that the total weight proportions of tetrahydrofuran, tetrakis(hexafluoroisopropyloxy)magnesium borate and tris(hexafluoroisopropyl)borate remain unchanged, and the mass ratio of tetrahydrofuran, tetrakis(hexafluoroisopropyloxy)magnesium borate and tris(hexafluoroisopropyl)borate is 65:30:1, and a gel electrolyte is finally obtained.
[0058] Example 7
[0059] The difference from Example 1 is that the total weight proportions of tetrahydrofuran, tetrakis(hexafluoroisopropyloxy)magnesium borate and tris(hexafluoroisopropyl)borate remain unchanged, and the mass ratio of tetrahydrofuran, tetrakis(hexafluoroisopropyloxy)magnesium borate and tris(hexafluoroisopropyl)borate is 75:25:5, and a gel electrolyte is finally obtained.
[0060] Example 8
[0061] The difference from Example 1 is that the temperature of the in-situ ring-opening polymerization reaction is 75° C., the time of the in-situ ring-opening polymerization reaction is 6 h, the pressure of the in-situ ring-opening polymerization reaction is 15 MPa, and finally a gel electrolyte is obtained.
[0062] Example 9
[0063] The difference from Example 1 is that the temperature of the in-situ ring-opening polymerization reaction is 20° C., the time of the in-situ ring-opening polymerization reaction is 24 h, the pressure of the in-situ ring-opening polymerization reaction is 60 MPa, and finally a gel electrolyte is obtained.
[0064] Example 10
[0065] The difference from Example 1 is that the temperature of the in-situ ring-opening polymerization reaction is 120° C., the time of the in-situ ring-opening polymerization reaction is 1 h, the pressure of the in-situ ring-opening polymerization reaction is 0.1 MPa, and finally a gel electrolyte is obtained.
[0066] Embodiment 11
[0067] The difference from Example 1 is that the temperature of the in-situ ring-opening polymerization reaction is 130° C., the time of the in-situ ring-opening polymerization reaction is 0.5 h, the pressure of the in-situ ring-opening polymerization reaction is 0.05 MPa, and finally a gel electrolyte is obtained.
[0068] Comparative Example 1
[0069] The difference from Example 1 is that tris(hexafluoroisopropyl) borate is not added, and the electrolyte is finally obtained.
[0070] Comparative Example 2
[0071] The difference from Example 1 is that the weight parts of tetrakis(hexafluoroisopropyloxy)magnesium borate are 10 parts, the weight parts of tris(hexafluoroisopropyl) borate are 10 parts, and the weight parts of tetrahydrofuran are 80 parts, and finally a gel electrolyte is obtained.
[0072] Performance Testing
[0073] The thickness, electrochemical oxidation window and ionic conductivity of the electrolyte prepared in the above embodiments and comparative examples were tested at 25°C. The electrolyte prepared in the above embodiments and comparative examples was assembled into a magnesium ion battery together with a positive electrode sheet and a negative electrode sheet, wherein the positive electrode active material of the positive electrode sheet is a sulfur-containing compound, and the negative electrode active material of the negative electrode sheet is metallic magnesium. The magnesium ion battery was subjected to a constant current charge and discharge test at 30°C, with a battery rate of 0.5C and 100 cycles. The capacity retention rate and coulomb efficiency of the magnesium ion battery after 100 cycles, as well as the thickness, electrochemical oxidation window and ionic conductivity of the electrolyte are shown in Table 1.
[0074] Table 1
[0075]
[0076]
[0077] Figure 1 is an optical photograph of the gel polymer electrolyte in Example 1, from which it can be seen that the electrolyte is in a colorless gel state;
[0078] Figure 2 The LSV curve of the magnesium ion battery assembled with the gel polymer electrolyte in Example 1, wherein the counter electrode in the magnesium ion battery is stainless steel and the negative electrode active material is metal magnesium. From the figure, it can be concluded that the electrochemical oxidation window of the gel polymer electrolyte is 3.5V;
[0079] Figure 3 This is a long cycle curve of the magnesium ion battery assembled with the gel polymer electrolyte in Example 2 at 30°C, wherein the positive electrode in the magnesium ion battery is a copper current collector, the negative electrode active material is metallic magnesium, and the coulomb efficiency of the magnesium ion battery for reversible deposition / dissolution of magnesium for 800 cycles is still above 90%, indicating that the gel electrolyte exhibits a good ability to reversibly deposit / dissolve magnesium.
[0080] Figure 4 The morphology of the magnesium sheet surface after the magnesium ion battery assembled with the gel polymer electrolyte in Example 2 was cycled for 1000 times at 30°C. (a) and (b) represent the surface morphology of the magnesium sheet at different magnifications. The positive electrode in the magnesium ion battery is a copper current collector, and the negative electrode active material is metallic magnesium. It can be seen from the figure that the surface morphology of the magnesium sheet is uniform after a long cycle.
[0081] Figure 5 This is a long cycle curve of the magnesium ion battery assembled with the gel polymer electrolyte in Example 3 at 30°C, wherein the positive electrode active material in the magnesium ion battery is a sulfur-containing compound, and the negative electrode active material is metallic magnesium. The specific capacity of the battery after 100 cycles at 30°C is still above 200mAh / g, indicating that the electrolyte can effectively inhibit the shuttling of polysulfides and improve the interface stability, long cycle performance, safety performance and energy density of the magnesium ion battery.
[0082] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0083] The Lewis acid catalyst in the gel electrolyte composition attacks the multi-electron oxygen in the ether compound due to the lack of electrons, thereby catalyzing the ring-opening polymerization reaction of the ether compound to form a gel polymer. The gel polymer can help the magnesium salt dissociate, thereby helping to improve the room temperature conductivity of the gel electrolyte. The gel electrolyte is applied to the magnesium ion battery, which is conducive to uniform deposition and dissolution of the magnesium metal negative electrode, thereby helping to improve the stability of the interface between the magnesium metal negative electrode and the gel electrolyte. In addition, since the free solvent in the gel polymer is reduced, it helps to improve the electrochemical window of the gel electrolyte, and then helps to improve the high voltage stability of the magnesium ion battery. At the same time, the semi-solid property of the gel polymer electrolyte alleviates the severe dissolution and shuttling of polysulfides in the liquid electrolyte, causing a large loss of active substances, thereby helping to improve the rate performance and cycle stability of the magnesium ion battery. It is preferred to control the weight of each component in the gel electrolyte composition within the above range, which helps to improve the synergistic effect between the components, thereby helping to further improve the room temperature conductivity and electrochemical window of the gel electrolyte.
[0084] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A gel electrolyte composition, characterized in that: In parts by weight, the gel electrolyte composition comprises: 25 to 75 parts of an ether compound; 15 to 45 parts of a magnesium salt; and 0.1 to 15 parts of Lewis acid catalyst.
2. The gel electrolyte composition according to claim 1, characterized in that The gel electrolyte composition comprises: 67-72 parts of an ether compound; 17 to 31 parts of a magnesium salt; and 2 to 6 parts of Lewis acid catalyst.
3. The gel electrolyte composition according to claim 1 or 2, characterized in that: The ether compound is selected from any one or more of tetrahydrofuran, 1,3-dioxolane, tetrahydropyran, 1,3-dioxane, 1,4-dioxane and 1,3,5-trioxane; And / or, the magnesium salt is selected from any one or more of bis(trifluoromethanesulfonyl imide) magnesium, phenylmagnesium chloride, magnesium tetrakis(hexafluoroisopropyloxy)borate, perfluoropinacol magnesium borate, magnesium borohydride and magnesium tetrachloroaluminate; And / or, the Lewis acid catalyst is selected from any one or more of boron trifluoride, magnesium chloride, aluminum chloride, trimethylaluminum, magnesium trifluoromethanesulfonate and tris(hexafluoroisopropyl)borate.
4. The gel electrolyte composition according to claim 3, characterized in that: The ether compound is tetrahydrofuran, the magnesium salt is magnesium tetrakis(hexafluoroisopropyloxy)borate, the Lewis acid catalyst is tris(hexafluoroisopropyl)borate, and the mass ratio of the tetrahydrofuran, the magnesium tetrakis(hexafluoroisopropyloxy)borate and the tris(hexafluoroisopropyl)borate is 65-75:25-30:1-5.
5. A method for preparing a gel electrolyte, characterized in that: The preparation method comprises: mixing a gel electrolyte composition and injecting it into a dry battery cell to perform an in-situ ring-opening polymerization reaction to obtain the gel electrolyte; wherein the gel electrolyte composition is the gel electrolyte composition according to any one of claims 1 to 4.
6. The preparation method according to claim 5, characterized in that: The temperature of the in-situ ring-opening polymerization reaction is 20 to 120° C.; and / or, the time of the in-situ ring-opening polymerization reaction is 1 to 24 hours; and / or, the pressure of the in-situ ring-opening polymerization reaction is 0.1 to 60 MPa.
7. The preparation method according to claim 6, characterized in that: The temperature of the in-situ ring-opening polymerization reaction is 25 to 75° C.; and / or, the time of the in-situ ring-opening polymerization reaction is 6 to 16 hours; and / or, the pressure of the in-situ ring-opening polymerization reaction is 10 to 15 MPa; preferably, the in-situ ring-opening polymerization reaction is carried out in a static state.
8. A gel electrolyte, characterized in that: The gel electrolyte is prepared by the preparation method according to any one of claims 5 to 7.
9. The gel electrolyte according to claim 8, characterized in that The thickness of the gel electrolyte is 70 to 700 μm; and / or the ionic conductivity of the gel electrolyte at 25° C. is 3.58×10 -3 ~5.28×10 -3 S / cm; and / or, the electrochemical window of the gel electrolyte is not less than 3.5V.
10. A magnesium ion battery, comprising a positive electrode sheet, an electrolyte and a negative electrode sheet, characterized in that: The electrolyte is the gel electrolyte according to claim 8 or 9.