Preparation method of titanium-based oxide Magneril phase material

By melting Ti metal and titanium dioxide powder in alkali metal halide flux and controlling the reaction atmosphere and cooling speed, the problem of high synthesis temperature and low yield of titanium-based oxide margnelli phase in the prior art is solved, and the problem of high synthesis temperature and low yield of titanium-based oxide margnelli phase is achieved. It is prepared with high purity and high uniformity of margnelli phase materials, and has the ability to regulate the transition temperature and conductivity of metal insulators.

CN119020862APending Publication Date: 2024-11-26UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410984229.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to achieve the increase in volume synthesis of titanium-based oxide margnelli phase materials at one reaction under low reaction temperature and mild atmosphere conditions, resulting in large process energy consumption and low yield, which limits the industrial production application of this system materials. .

Method used

Ti metal and titanium dioxide powder are used as precursors to melt in alkali metal halide flux, and the reaction atmosphere and cooling rate are precisely controlled, so that the titanium oxide margnelli phase can nucleate on the crystalline surface of metal halide. A titanium-based oxide margnelli phase oxide powder material in an intermediate chemical valence state was obtained.

Benefits of technology

Reduces the material synthesis temperature and reaction time, improves product purity and uniformity, avoids high-risk reaction conditions such as harmful impurities and flammable and explosive, and achieves high purity and high uniformity of the titanium-based oxide margnelli phase. Preparation, with the ability to continuously regulate the transition temperature and conductivity of metal insulators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020862A_ABST
    Figure CN119020862A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a titanium-based oxide Magneril phase material, belongs to the field of electrochemical functional materials, and particularly relates to a method for preparing a titanium-based oxide Magneril phase material by using an additive with dual functions of a fluxing agent and a heterogeneous seed crystal and reducing the synthesis temperature limit through the lattice matching relationship between the fluxing agent and the specific crystal face of the titanium oxide Magneril phase. And the reaction speed is accelerated, harmful impurities and flammable and explosive high-risk synthesis conditions are avoided, and the method can be used for synthesizing the titanium-based oxide macageril phase material in a quantitative manner. The prepared titanium-based oxide Magneril phase material has high conductivity at room temperature, high thermal stability and high acid and alkali corrosion resistance, is non-toxic and harmless to a human body, and has considerable application value in the fields of photo-anodes, battery corrosion-resistant electrodes, catalytic protection electrodes and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of functional materials, electrocatalytic materials, and strongly correlated electronic devices, and specifically relates to a technical method for accurately synthesizing titanium-based oxide magneli phase materials under vacuum and protective atmosphere by using metal halides as flux to assist in controllable topological transformation of oxides. Background Art

[0002] The chemical formula is Ti n O 2n-1 The Magnéli phase of titanium oxide (1) has a shear oxygen-deficient lattice and Ti 3+ / Ti 4+ The charge is ordered, showing a rich intermediate valence structure, exhibiting high room temperature conductivity, high corrosion resistance and multi-level metal-insulator phase transition characteristics [2]. It can continuously undergo changes of more than 3 orders of magnitude and has broad application prospects in the fields of electrocatalysts [3], high-performance electrodes [4], and optoelectronic devices [5]. Compared with TiO2, which has no d-orbital electrons and exhibits insulating properties within a stable temperature range, the Magnelli phase Ti n O 2n-1 Some Ti sites contain localized d electrons, forming covalently bonded Ti 3+ -Ti 3+ Dimer, composed of Ti 4+ Ions and Ti2 6+ The ordered Ti chains with alternating dimers show an insulating state dominated by charge order at low temperatures. The electronic excitation caused by temperature and pressure fields gradually destroys the charge order, showing metal-insulator transition characteristics [6]. 11 (n=6), Ti7O 13 (n=7) can undergo the transition from low-temperature antiferromagnetic insulator to high-temperature paramagnetic metal, with the transition temperatures being 140 K, 130 K, and 120 K, respectively; the valence state of Ti4O7 (n=4) is Ti 3+ / Ti 4+ =1:1, with the strongest charge ordering phenomenon, and the transition from antiferromagnetic insulator to paramagnetic semiconductor and from paramagnetic semiconductor to paramagnetic metal occurs under the characteristic temperature triggering of 135 K and 150 K, respectively, with continuous resistance transition exceeding 5 orders of magnitude; when n is greater than 7, Ti 4+ The ions dominate the electronic structure and no longer show the metal-insulator transition characteristics. In addition to the strongest metal-insulator phase transition characteristics, the room temperature conductivity of Ti4O7 is as low as 10 -5Ω·m, high thermal and chemical stability, corrosion half-life in 4% sulfuric acid solution exceeds 50 years [7], has good dispersibility in water and organic solvents, shows better wear resistance under mechanical external force [8], is non-toxic and harmless to the human body, can be used as a protective electrode for acid-alkaline electrolyte batteries, cathode for lithium-sulfur batteries and zinc batteries [9], catalytic auxiliary electrode, photoanode, etc., can also be used for sewage treatment, photodegradation of organic wastes such as naphthalene

[10] , and selective organic synthesis catalyst

[11] .

[0003] At present, the common method for synthesizing titanium-based oxide magneli phase materials is solid phase reduction method, which mainly uses rutile phase TiO2 as raw material, fully grinds and mixes with reducing agent according to stoichiometric ratio, and synthesizes by multiple long-term solid phase reaction under high temperature conditions of 1100 ℃-1400 ℃. Common reducing agents include elemental carbon, hydrogen, mixed hydrogen, hydride, and elemental titanium. The reduction of elemental carbon easily forms carbon monoxide, carbon dioxide and incomplete carbides of titanium, which affects the purity of the product and has certain harm to the environment; hydrogen, mixed hydrogen and hydride have the risk of combustion and explosion under high temperature conditions, and the safety factor is low. In addition, elemental titanium can synthesize a variety of magneli phases under atmosphere controlled oxidation, but because titanium and TiO2 have a complex binary phase diagram, it is not easy to form a uniform solid phase reaction environment under mechanical mixing conditions, resulting in a relatively narrow stable phase region of the magneli phase, which requires strict atmosphere and temperature control, and the required reaction temperature is high (greater than or equal to 1200 ℃), the process energy consumption is large and the yield is low, which seriously limits the industrial production application of this system material.

[0004] In summary, the current art lacks an effective method that can achieve large-scale synthesis of titanium-based oxide magneli phase materials in a single reaction under low reaction temperature and mild gas atmosphere conditions, which limits the application of this system material.

[0005] 【1】Harada S, Tanaka K, Inui H. Thermoelectric properties and crystallographic shear structures in titanium oxides of the Magneli phases[J]. Journal of Applied Physics, 2010, 108(8). 【2】Xu B, Sohn HY, Mohassab Y, et al. Structures, preparation and applications of titanium suboxides [J]. RSC Advances, 2016, 6(83): 79706-22.

[0006] 【3】Luo M Q, Liu H J, Yang L X, et al. Precisely dominating oxygenvacancy of Magneli phase titanium suboxides to efficiently remove quinoloneantibiotics under visible light [J]. Separation and Purification Technology,2024, 341: 126626.

[0007] 【4】Smith J R, Walsh F C, Clarke R L. Electrodes based on Magnéliphase titanium oxides: the properties and applications of Ebonex® materials[J]. Journal of Applied Electrochemistry, 1998, 28(10): 1021-33. 【5】Yang B, Zhang Z, Liu P, et al. Flatband λ-Ti3O5 towardsextraordinary solar steam generation [J]. Nature, 2023, 622(7983): 499-506.

[0008] 【6】Lakkis S, Schlenker C, Chakraverty B K, et al. Metal-insulatortransitions in Ti4O7 single crystals: Crystal characterization, specific heat,and electron paramagnetic resonance [J]. Physical Review B, 1976, 14(4):1429-40.

[0009] 【7】Paunović P, Popovski O, Fidančevska E, et al. Co-Magneli phaseselectrocatalysts for hydrogen / oxygen evolution [J]. International Journal ofHydrogen Energy, 2010, 35(19): 10073-80.

[0010] 【8】Woydt M. Tribological characteristics of polycrystalline Magnéli-type titanium dioxides [J]. Tribology Letters, 2000, 8(2): 117-30.

[0011] 【9】Liu M, Jhulki S, Sun Z, et al. Atom-economic synthesis of Magnéliphase Ti4O7 microspheres for improved sulfur cathodes for Li–S batteries [J].Nano Energy, 2021, 79: 105428.

[0012]

[10] Kumar A, Barbhuiya N H, Singh S P. Magnéli phase titanium sub-oxides synthesis, fabrication and its application for environmentalremediation: Current status and prospect [J]. Chemosphere, 2022, 307: 135878.

[0013]

[11] Nagao M, Misu S, Hirayama J, et al. Magneli-Phase TitaniumSuboxide Nanocrystals as Highly Active Catalysts for Selective Acetalization of Furfural [J]. ACS Applied Materials & Interfaces, 2020, 12(2): 2539-47. Summary of the invention

[0014] The purpose of the present invention is to provide a method for preparing a titanium-based oxide magneli phase material. The main concept is: using Ti metal and titanium dioxide powder as precursors, effectively dissolving them in an alkali metal halide flux and accurately controlling the reaction atmosphere to achieve the purpose of effectively controlling the valence state of titanium and the stoichiometric ratio with oxygen; in the cooling process, based on the coherent matching relationship between the titanium suboxide magneli phase and the surface of the gradually precipitated metal halide crystal, the titanium suboxide magneli phase nucleates and grows on the surface of the metal halide crystal in a non-uniform heterogeneous nucleation manner, thereby obtaining a titanium-based oxide magneli phase oxide powder material with an intermediate chemical valence state.

[0015] A method for preparing a titanium-based oxide magneli phase material, the method comprising the following steps:

[0016] 1) According to the titanium-oxygen stoichiometric ratio of the fitted magneli phase titanium oxide, titanium and titanium oxide precursors are weighed and mixed stoichiometrically, and functional groups irrelevant to the final product are removed by pre-calcination;

[0017] 2) According to the phase stability zone temperature of the fitted magneli phase titanium oxide, a metal halide flux and a flux combination with a melting point adapted thereto are selected, and added to the above-mentioned precursor mixed powder in a certain proportion;

[0018] 3) The precursor mixed with flux is encapsulated in a quartz tube with a certain atmosphere, and heated to a certain temperature so that the precursor is fully dissolved in the molten halide flux; then, after being kept warm for a period of time, it is cooled to room temperature at a certain cooling rate, during which the magneli phase titanium oxide is precipitated together with the gradually solidified halide flux in a non-uniform nucleation process;

[0019] 4) The halide flux in the obtained powder product is removed by washing with water and ethanol solvents, and a pure phase magneli phase titanium oxide powder material is obtained after drying; the obtained powder is further added with a binder, cold-pressed and granulated, and then sintered to obtain a magneli phase titanium oxide ceramic material.

[0020] Furthermore, the chemical composition of the synthesized magneli phase titanium oxide in step 1) is Ti n O 2n-1 , where n=2-9, and when the precursor is TiO2 and titanium metal, the molar ratios are TiO2:Ti=3:1 (n=2), 5:1 (n=3), 7:1 (n=4), 9:1 (n=5), 11:1 (n=6), 13:1 (n=7), 15:1 (n=8), and 17:1 (n=9). The prepared Magnelli phase titanium oxide has a metal-insulator phase transition characteristic triggered by a characteristic temperature. The metal-insulator phase transition characteristic can be adjusted in a wide range of 120 K to 460 K by adjusting n, and a multi-level phase transition characteristic can also be achieved through a specific structure. In a preferred example, the synthesized pure phase Ti4O7 ceramic material exhibits a two-level electronic phase transition, namely, a semiconductor-semiconductor transition in the temperature range of 130-140 K and a semiconductor-metal transition at 150 K. In another preferred example, the synthesized pure phase β-Ti3O5 exhibits a low-temperature β insulator phase-high-temperature λ metal phase transition at 460 K, accompanied by a sudden change in conductivity. In another preferred embodiment, the synthesized pure phase γ-Ti3O5 exhibits a high temperature γ semiconductor phase-low temperature δ insulator phase transition at 237 K, accompanied by a sudden change in conductivity.

[0021] Further, the precursors described in step 1) include titanium dioxide, other titanium compounds and elemental titanium; the titanium dioxide used includes rutile phase titanium dioxide, anatase phase titanium dioxide, rutile / anatase mixed phase titanium dioxide and other titanium dioxide isomers; the other titanium compounds used are preferably titanium hydroxide; the elemental titanium used is preferably nano-metal titanium powder, micron-metal titanium powder, and metal titanium particles, with a particle size ranging from 200 nm to 2 mm. The precursors used can be directly mixed or pre-heated in the air to remove crystal water and surface grease before mixing; the degree of resistivity mutation, thermal stability and electrocatalytic performance of the synthesized powder metal insulator transition can be controlled by controlling the type, size and phase of the precursor. In a preferred example, the raw materials used are rutile phase TiO2 and nano-metal titanium powder, and pure phase Ti4O7 with two-stage phase transition is synthesized, and the continuous resistivity change exceeds 3 orders of magnitude. In another preferred embodiment, the raw materials used are anatase phase TiO2 and micron metal titanium powder, and pure phase Ti5O9 with a phase transition temperature of 140 K is synthesized, and the resistivity changes by more than 2 orders of magnitude.

[0022] Furthermore, the central metal ion Ti described in step 1) can be partially replaced by other transition metal ions to further control the basic resistivity of the material, the phase transition characteristics of the metal insulator, the oxidative thermal stability, and the catalytic characteristics in the acidic solution environment; the doping elements are preferably Fe, V, Co, Cr, Nb, Mo, and Mn, and their corresponding precursors are equivalent oxides of the corresponding transition metals, preferably Fe2O3, VO2, Co2O3, Cr2O3, Nb2O5, MoO2, and MnO2. The phase transition temperature of the doped magneli phase titanium oxide gradually decreases with the increase of the doping amount until it fully exhibits the metal electrical transport characteristics, and the room temperature conductivity can reach 10 -5 In a preferred embodiment, pure phase polycrystalline (V 0.02 Ti 0.98 )4O7, the first-order phase transition is completely suppressed and the second-order phase transition temperature is reduced to 130 K; doping can also significantly improve the thermal stability and electrochemical activity of magneli phase titanium oxide. In another preferred embodiment, pure phase polycrystalline β-(Fe 0.015 Ti 0.985 )3O5, achieving a thermal oxidation peak temperature 100°C higher than that of pure phase polycrystalline β-Ti3O5, and an electrochemical activity of catalyzing oxygen evolution reaction in 0.5 M H2SO4 solution increased by 65%.

[0023] Further, the melting point of the flux in step 2) is lower than the melting point required for the magneli phase titanium oxide, and it can dissolve and evenly disperse the precursor powder in a high temperature molten state to reduce its nucleation thermodynamic potential and realize the non-uniform nucleation of the product in the flux; the metal halide flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, CsI; a single flux can be used, or a binary and multi-component combination of the above flux systems can be used, preferably a KCl and LiCl eutectic system, a KCl and NaCl eutectic system, and a KCl and NaCl and LiCl eutectic system, so as to match the lattice parameters of the flux with the lattice parameters of the specific crystal plane of the magneli phase. The molar ratio of the metal halide flux to the titanium element in the precursor is 0.1-100.

[0024] Furthermore, the synthetic atmosphere in step 3) comprises a rough vacuum (10 -2 -10 -1 Pa), high vacuum (10 -4 -10 -3 Pa), ultra-high vacuum (less than or equal to 10-5 Pa), inert gas atmosphere, preferably nitrogen or argon atmosphere. Under different synthesis atmosphere conditions, the reference temperature is determined according to different magneli phase titanium oxide target products, so that the reaction process is located in the product equilibrium phase region corresponding to the oxygen partial pressure-temperature phase diagram, thereby avoiding the generation of impurity phases. Under the reaction conditions of 1100°C, Ti n O 2n-1 The oxygen partial pressure balance interval is 10 -20.7 -10 -17.5 Pa(n=2)、10 -17.5 -10 -14.6 Pa(n=3)、10 -14.6 -10 -12.9 Pa(n=4)、10 -12.9 -10 -12.6 Pa(n=5)、10 -12.6 -10 -12.2 Pa(n=6)、10 -12.2 -10 -12.1 Pa(n=7)、10 -12.1 -10 -12.0 Pa(n=8)、10 -12.0 -10 -11.9 Pa (n=9).

[0025] Furthermore, in step 3), the solid phase reaction heat treatment system is divided into two stages. The selection of the heat treatment system in the heating stage is determined by the stable phase region of the magneli phase titanium oxide under the selected synthesis atmosphere conditions, preferably 100-300 °C lower than the median temperature of the phase region, at which time the flux can fully melt and evenly disperse the precursor powder; the heat treatment system in the cooling stage selects a cooling rate of 0.1-10 °C / min, air cooling or quenching, and the quenching medium can be selected from water, oil, ice-water mixture and liquid nitrogen, so that the magneli phase titanium oxide and the flux are precipitated simultaneously in a non-uniform nucleation manner. In a preferred example, the raw materials selected are rutile phase TiO2 and micron metal titanium powder, the precursor molar ratio is 7:1, the flux is KCl, its melting point is 776 ° C, the heat treatment temperature in the heating stage is 1000 ° C, and the cooling rate in the cooling stage is 10 ° C / min to obtain pure phase Ti4O7; the directional control of the isomer ratio in the magneli phase titanium oxide product can also be achieved by precisely controlling the cooling rate. In another preferred embodiment, the raw materials are selected as rutile phase TiO2 and micron titanium metal powder, the precursor molar ratio is 5:1, the flux is selected as a mixture of KCl:NaCl=1:1, the heat treatment temperature in the heating stage is 1000°C, and the cooling rate is selected as 0.1°C / min to obtain β-Ti3O5 pure phase powder; in another preferred embodiment, the raw materials are selected as rutile phase TiO2 and micron titanium metal powder, the precursor molar ratio is 5:1, the flux is selected as a mixture of KCl:NaCl=1:1, the heat treatment temperature in the heating stage is 1000°C, and the cooling stage is quenched to room temperature to obtain γ-Ti3O5 pure phase powder; in another preferred embodiment, the raw materials are selected as rutile phase TiO2 and micron titanium metal powder, the precursor molar ratio is 5:1, the flux is selected as a mixture of KCl:NaCl=1:1, the heat treatment temperature in the heating stage is 1000°C, and the cooling rate is selected as 7 ℃ / min, and a powder with a ratio of β-Ti3O5 phase to γ-Ti3O5 phase of 1:10 was obtained.

[0026] Furthermore, by regulating the particle size of titanium oxide and titanium salt precursors, metallic titanium precursors, the proportion of flux, the holding temperature and time, the cooling rate, and the vacuum degree, the allotropic characteristics and particle size of the prepared titanium-based oxide magneli phase powder can be regulated; by selecting the type of flux, the surface crystal orientation of the prepared titanium-based oxide magneli phase powder can be regulated. In a preferred example, the precursors are selected as rutile phase TiO2 powder with a diameter of 100 microns and metal titanium powder with a diameter of 100 microns, KCl is selected as a flux, and the mixture is kept at 1000°C for 48 hours, and cooled at a rate of 5°C / min to obtain Ti4O7 pure phase powder with a powder particle size of 2 microns; in another preferred example, the precursors are selected as rutile phase TiO2 powder with a diameter of 10 microns and metal titanium powder with a diameter of 50 nanometers, the flux ratio KCl:LiCl=1:1 is selected, the mixture is kept at 950°C for 24 hours, and quenched and cooled to obtain Ti4O7 pure phase powder with a powder particle size of 200 nanometers.

[0027] The present invention proposes a method for mass production of magneli phase titanium oxide powder and ceramic material. Compared with other methods, the advantage of this method is that by introducing a metal halide flux with a lattice parameter similar to that of the synthesized material, thermodynamic conditions are provided for the growth of new phases, the reaction temperature required for material synthesis is reduced, the purity of the product is improved, the generation of harmful impurities is avoided, and flammable and explosive high-risk reaction conditions are avoided, so that the mass production of high-purity and high-uniformity materials can be achieved. By further regulating the size of n and the type of central metal ions, the metal-insulator transition temperature of the material can be continuously regulated in a wide range, and the room temperature conductivity can be as low as 10 -5 Ω·m, and has certain application prospects in the fields of mutation thermistors, photoanodes, and electrochemical auxiliary electrodes.

[0028] Compared with the traditional solid-phase reaction method and atmosphere reduction method of the system material, the technology provided by the present invention can greatly reduce the material synthesis temperature and reaction time, avoid the high-risk flammable and explosive gas environment, and improve the purity and uniformity of the prepared material, and can realize the mass production of the system material in air atmosphere, lower reaction temperature and shorter reaction time. The prepared material can be further sintered into a block or made into a slurry and applied to a photoanode, a highly corrosive electrolyte battery protective agent, a highly active catalyst auxiliary electrode, and a thermistor. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is an X-ray diffraction diagram of Ti4O7 powder prepared by the flux method proposed in the present invention. It can be seen that the prepared powder is a pure phase powder.

[0030] Figure 2The resistivity variation curve of Ti4O7 powder prepared by the flux method proposed in the present invention is as a function of temperature. It can be seen that the prepared powder undergoes a continuous transformation from a low-temperature insulator phase to a medium-temperature semiconductor phase, and from a medium-temperature semiconductor phase to a high-temperature metal phase near the characteristic temperature of the metal-insulator phase transition (135 K and 150 K).

[0031] Figure 3 This is an X-ray diffraction diagram of Ti3O5 powder prepared by the flux method proposed in the present invention. It can be seen that the prepared powder is a powder with a controlled phase ratio of β-Ti3O5 to γ-Ti3O5 of 1:10.

[0032] Figure 4 For the Ti6O planted using the flux method proposed by the present invention 11 The X-ray diffraction pattern of the powder shows that the prepared powder is a pure phase powder.

[0033] Figure 5 The linear current-overpotential curve of the oxygen evolution reaction catalyzed by the Ti4O7 powder prepared by the flux method proposed in the present invention in a 0.1 M KOH solution.

[0034] Figure 6 This is the oxygen partial pressure-temperature equilibrium phase diagram of Magnelli phase titanium oxide. DETAILED DESCRIPTION

[0035] Unless otherwise specified, the various raw materials used in the present invention can be obtained from the market or prepared according to conventional methods in the art. Unless otherwise defined or specified, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the method of the present invention.

[0036] Other aspects of the present invention will be apparent to those skilled in the art in view of the disclosure herein.

[0037] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0038] Example 1: Rutile phase TiO2 powder and 100 μm titanium metal powder were weighed at a precursor molar ratio of TiO2:Ti=7:1, and KCl was weighed at an element molar ratio of Ti:K=1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a rough vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -1Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 10 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti4O7 powder. A binder was added to the obtained powder and cold pressed and sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed into the medium-temperature semiconductor phase and the medium-temperature semiconductor phase transformed into the high-temperature metal phase at the phase transition characteristic temperatures of 135 K and 150 K, and the resistivity mutation degree triggered was 1000 times.

[0039] Example 2: Anatase phase TiO2 powder and titanium metal particles were weighed at a precursor molar ratio of TiO2:Ti=3:1, and KCl and LiCl were weighed at an element molar ratio of Ti:K:Li=2:1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a rough vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -2 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 5 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti2O3 powder. A binder was added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component. The transition from the low-temperature semiconductor phase to the high-temperature semi-metal phase occurred near the phase transition characteristic temperature of 450 K, and the resistivity mutation degree triggered was 50 times.

[0040] Example 3: Rutile TiO2 and 500 μm titanium metal powder were weighed at a precursor molar ratio of TiO2:Ti=5:1, and KCl and NaCl were weighed at an element molar ratio of Ti:K:Na=2:1:1. The precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press. The block was then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -3 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was quenched in a water medium and cooled to room temperature. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase γ-Ti3O5 powder. A binder was added to the obtained powder and cold pressed and sintered to obtain a ceramic material of this component. The transition from the low-temperature insulator phase to the high-temperature semiconductor phase occurred near the phase transition characteristic temperature of 237 K, and the resistivity mutation degree triggered was 50 times.

[0041] Example 4: Rutile TiO2 and 500 μm titanium metal powder were weighed at a precursor molar ratio of TiO2:Ti=5:1, and KCl and NaCl were weighed at an element molar ratio of Ti:K:Na=2:1:1. The precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press. The block was then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -3 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 0.1 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase β-Ti3O5 powder. A binder was added to the obtained powder and cold pressed and sintered to obtain a ceramic material of this component. The transition from the low-temperature insulator phase to the high-temperature metal phase occurred near the phase transition characteristic temperature of 460 K, and the resistivity mutation degree triggered was 100 times.

[0042] Example 5: Rutile TiO2 and 500 μm titanium metal powder were weighed at a precursor molar ratio of TiO2:Ti=5:1, and KCl and NaCl were weighed at an element molar ratio of Ti:K:Na=2:1:1. The precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press. The block was then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -3 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 7 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a powder with a ratio of β-Ti3O5 phase to γ-Ti3O5 phase of 1:10. A binder was added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component.

[0043] Example 6: Rutile phase TiO2 powder and titanium metal particles were weighed at a precursor molar ratio of TiO2:Ti=9:1, and KBr was weighed at an element molar ratio of Ti:K=1:1. The above precursors were placed in an agate mortar and ground evenly, and cold pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -4Pa. The quartz tube was placed in a muffle furnace and kept at 950 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 5 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti5O9 powder. A binder was added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component. The transition from the low-temperature insulator phase to the high-temperature metal phase occurred near the phase transition characteristic temperature of 140 K, and the resistivity mutation degree triggered was 100 times.

[0044] Example 7: According to the precursor molar ratio of TiO2:Ti=11:1, brookite phase TiO2 powder and 200 nanometer titanium metal powder were weighed, and LiCl was weighed according to the element molar ratio of Ti:Li=1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in an ultra-high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -5 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 48 hours. After the reaction was completed, it was quenched in an ice-water mixture and cooled to room temperature. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti6O 11 Powder, a binder is added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component. The transformation from low-temperature insulator phase to high-temperature metal phase occurs near the phase transition characteristic temperature of 130 K, and the resistivity mutation degree triggered is 100 times.

[0045] Example 8: Rutile / anatase mixed phase TiO2 powder and titanium foil were weighed at a precursor molar ratio of TiO2:Ti=13:1, KCl, NaCl and LiCl were weighed at an element molar ratio of Ti:K:Na:Li=6:3:1:2, the above precursors were placed in an agate mortar and ground evenly, and cold pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -4 Pa. The quartz tube was placed in a muffle furnace and kept at 1100 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 5 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti7O 13 Powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, at the phase transition characteristic temperature of 120 K, the transition from low-temperature insulator phase to medium-temperature semiconductor phase and from medium-temperature semiconductor phase to high-temperature metal phase occurs, and the resistivity mutation degree triggered is 20 times.

[0046] Example 9: 100 μm diameter rutile phase TiO2 powder and 100 μm diameter titanium metal powder were weighed at a precursor molar ratio of TiO2:Ti=7:1, and KCl was weighed at an element molar ratio of Ti:K=1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -3 Pa. The quartz tube was placed in a muffle furnace and kept at 950 °C for 48 hours. After the reaction was completed, it was cooled to room temperature at a rate of 5 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase Ti4O7 powder with a particle size of 2 microns. A binder was added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component. The low-temperature insulator phase transformed into the medium-temperature semiconductor phase and the medium-temperature semiconductor phase transformed into the high-temperature metal phase at the phase transition characteristic temperatures of 135 K and 150 K, and the resistivity mutation degree triggered was 500 times.

[0047] Example 10: According to the precursor molar ratio of TiO2:Ti=7:1, 10 micron rutile phase TiO2 powder and 50 nanometer titanium metal powder were weighed, and KCl and LiCl were weighed according to the element molar ratio of Ti:K:Li=2:1:1. The above precursors were placed in an agate mortar and ground evenly, and cold pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -3 Pa. The quartz tube was placed in a muffle furnace and kept at 950 °C for 24 hours. After the reaction was completed, it was quenched in a water medium and cooled to room temperature. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase Ti4O7 powder with a particle size of 200 nanometers. A binder was added to the obtained powder and cold pressed and sintered to obtain a ceramic material of this component. The low-temperature insulator phase transformed into the medium-temperature semiconductor phase and the medium-temperature semiconductor phase transformed into the high-temperature metal phase at the phase transition characteristic temperatures of 135 K and 150 K, and the resistivity mutation degree triggered was 3000 times.

[0048] Example 11: According to the precursor molar ratio of TiO2:Ti=17:1, brookite phase TiO2 powder and 50 nanometers titanium metal powder were weighed, and KI and Na1 were weighed according to the element molar ratio of Ti:K:Na=2:1:1. The above precursors were placed in an agate mortar and fully ground evenly, and cold pressed into a block with a diameter of 6 mm by a press, and then sealed in a quartz tube with a nitrogen protective atmosphere with the assistance of argon purge, and the pressure was 5 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 ° C for 48 hours. After the reaction was completed, it was quenched and cooled to room temperature in a liquid nitrogen medium. The block sample was taken out of the quartz tube and ground, and the powder sample was washed three times with deionized water, and the powder sample was washed once with anhydrous ethanol and dried to obtain a pure phase Ti9O 17 Powder, adding a binder to the obtained powder, cold pressing and sintering to obtain the ceramic material of the component.

[0049] Example 12: Rutile phase TiO2 powder, titanium metal particles and M1 phase VO2 powder were weighed at a precursor molar ratio of TiO2:Ti:VO2=175:21:4, and NaBr was weighed at an element molar ratio of Ti:Na=1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in an ultra-high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -5 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 10 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase (V 0.02 Ti 0.98 )4O7 powder, added binder to the obtained powder, cold pressed and sintered to obtain the ceramic material of this component. The transformation from low-temperature insulator phase to high-temperature metal phase occurred near the phase transition characteristic temperature of 140 K, and the resistivity mutation degree triggered was 100 times; the electrochemical activity of catalyzing oxygen evolution reaction in 0.5 M H2SO4 solution was increased by 10%.

[0050] Example 13: Rutile phase TiO2 powder, titanium metal particles and Fe2O3 powder were weighed according to the precursor molar ratio of TiO2:Ti:Fe2O3=100:182:9, and NaCl and RbCl were weighed according to the element molar ratio of Ti:Na:Rb=3:2:1. The above precursors were placed in an agate mortar and fully ground evenly, and cold pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -4Pa. The quartz tube was placed in a muffle furnace and kept at 1050 °C for 24 hours. After the reaction was completed, it was quenched in an oil medium and cooled to room temperature. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase β-(Fe 0.015 Ti 0.985 )3O5 powder, adding a binder to the obtained powder and cold pressing and sintering to obtain the ceramic material of this component, the low-temperature insulator phase changes to the high-temperature metal phase at the phase transition characteristic temperature of 350 K; compared with β-Fe3O5 synthesized under the same conditions, β-(Fe 0.015 Ti 0.985 The electrochemical activity of )3O5 in 0.5 M H2SO4 solution for catalytic oxygen evolution reaction was increased by 60%; the peak temperature of thermal decomposition was increased by 100℃.

[0051] Example 14: According to the precursor molar ratio of TiO2:Ti:VO2:Cr2O3=550:541:6:3, brookite phase TiO2 powder, nano-titanium metal powder, M1 phase VO2 powder, Cr2O3 powder were weighed, and KI and CsI were weighed according to the element molar ratio of Ti:K:Cs=7:4:3. The above precursors were placed in an agate mortar and fully ground evenly. They were cold pressed into blocks with a diameter of 6 mm using a press, and then sealed in a quartz tube with an argon protective atmosphere with the assistance of argon purge, and the air pressure was 15 Pa. The quartz tube was placed in a muffle furnace and kept at 1100 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 5 °C / min. The block sample was taken out of the quartz tube and ground, and the powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase (V 0.01 Cr 0.01 Ti 0.98 )6O 11 The powder has a particle size of 500 nanometers. The ceramic material of this component is obtained by adding a binder to the obtained powder and cold pressing and sintering. The low-temperature semiconductor phase transforms to the high-temperature semi-metal phase at the phase transition characteristic temperature of 110 K, and the resistivity mutation degree triggered by it is 5 times. The electrochemical activity of catalyzing oxygen evolution reaction in 0.1 M HCl solution is higher than that of Ti6O synthesized under the same conditions. 11 An increase of 37%.

[0052] Example 17: Anatase phase TiO2 powder and titanium foil were weighed at a precursor molar ratio of TiO2:Ti=17:1, and KF and NaF were weighed at an element molar ratio of Ti:K:Na=2:1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in an ultra-high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -5Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature in air. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti9O 17 Powder, particle size 5 microns.

[0053] Example 18: Titanium hydroxide powder and 5-micron titanium metal powder were weighed at a precursor molar ratio of Ti(OH)4:Ti=7:9, and RbCl was weighed at an element molar ratio of Ti:Rb=1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press. Then, the block was sealed in a quartz tube in a rough vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -1 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 7 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase Ti4O7 powder with a particle size of 500 nanometers. A binder was added to the obtained powder and cold pressed and sintered to obtain a ceramic material of this component. The low-temperature insulator phase transformed into the medium-temperature semiconductor phase and the medium-temperature semiconductor phase transformed into the high-temperature metal phase at the phase transition characteristic temperatures of 135 K and 150 K, and the resistivity mutation degree triggered was 1500 times.

[0054] Example 17: Titanium hydroxide powder and titanium metal particles were weighed at a precursor molar ratio of Ti(OH)4:Ti=9:11, and KCl was weighed at an element molar ratio of Ti:K=1:10. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a rough vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -2 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 5 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti5O9 powder. A binder was added to the obtained powder, cold pressed and sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 140 K, and the resistivity mutation degree triggered was 30 times.

[0055] Example 18: Titanium hydroxide powder and 200 nanometer titanium metal powder were weighed at a precursor molar ratio of Ti(OH)4:Ti=11:13, and LiCl, KCl, and NaCl were weighed at an element molar ratio of Ti:Li:Na:K=15:8:6:1. The precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press. The block was then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -3 Pa. The quartz tube was placed in a muffle furnace and kept at 900 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at 0.5 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti6O 11 Powder, a binder is added to the obtained powder, cold pressed and sintered to obtain a ceramic material of this component. The transformation from low-temperature insulator phase to high-temperature metal phase occurs near the phase transition characteristic temperature of 130 K, and the resistivity mutation degree triggered is 20 times.

[0056] Example 19: Rutile phase TiO2 powder and 100 μm titanium metal powder were weighed at a precursor molar ratio of TiO2:Ti=7:1, and KCl was weighed at an element molar ratio of Ti:K=1:100. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a high vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -4 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 °C for 24 hours. After the reaction was completed, it was cooled to room temperature at a rate of 1 °C / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain pure phase Ti4O7 powder. A binder was added to the obtained powder and cold pressed and sintered to obtain the ceramic material of this component. The low-temperature insulator phase transformed into the medium-temperature semiconductor phase and the medium-temperature semiconductor phase transformed into the high-temperature metal phase at the phase transition characteristic temperatures of 135 K and 150 K, and the resistivity mutation degree triggered was 2000 times.

[0057] Example 20: Titanium hydroxide powder, 5000 nanometer diameter rutile phase TiO2 powder and 10 micrometer diameter titanium metal powder were weighed according to the precursor molar ratio of Ti(OH)4:TiO2:Ti=3:3:4, and KCl was weighed according to the element molar ratio of Ti:K=1:1. The above precursors were placed in an agate mortar and ground evenly, and cold-pressed into a block with a diameter of 6 mm using a press, and then sealed in a quartz tube in a rough vacuum environment with the assistance of argon purge, and the vacuum degree was 10 -1Pa. The quartz tube was placed in a muffle furnace and kept at 1000℃ for 48 hours. After the reaction was completed, it was cooled to room temperature at a rate of 0.1℃ / min. The bulk sample was taken out of the quartz tube and ground. The powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase Ti5O9 powder with a particle size of 500 nanometers. A binder was added to the obtained powder and cold pressed and sintered to obtain a ceramic material of this component. The low-temperature insulator phase transformed to the high-temperature metal phase near the phase transition characteristic temperature of 140 K, and the resistivity mutation degree triggered was 50 times.

[0058] Example 21: Titanium hydroxide powder, titanium metal particles and Cr2O3 powder were weighed according to the precursor molar ratio of Ti(OH)4:Ti:Co2O3=175:221:2, and KCl was weighed according to the element molar ratio of Ti:K=1:50. The above precursors were placed in an agate mortar and ground evenly. They were cold pressed into blocks with a diameter of 6 mm using a press, and then sealed in a quartz tube in a nitrogen environment with the assistance of argon purge, and the air pressure was 3 Pa. The quartz tube was placed in a muffle furnace and kept at 950 °C for 24 hours. After the reaction was completed, it was quenched in an oil medium and cooled to room temperature. The block sample was removed from the quartz tube and ground, and the powder sample was washed three times with deionized water, washed once with anhydrous ethanol and dried to obtain a pure phase (Co 0.01 Ti 0.99 )4O7 powder, a binder was added to the obtained powder, cold pressed and sintered to obtain the ceramic material of this component. The transformation from low-temperature insulator phase to high-temperature metal phase occurred near the phase transition characteristic temperature of 125 K, and the resistivity mutation degree triggered was 100 times; the electrochemical activity of catalyzing oxygen evolution reaction in 0.1 M KOH solution was 10% higher than that of Ti4O7 synthesized under the same conditions.

[0059] Example 22: According to the precursor molar ratio of TiO2:Ti=5:1, brookite phase TiO2 powder and 50 nanometers titanium metal powder were weighed, and KBr and NaBr were weighed according to the element molar ratio of Ti:K:Na=1:25:25. The above precursors were placed in an agate mortar and fully ground evenly, and cold pressed into a block with a diameter of 6 mm by a press, and then sealed in a quartz tube with argon protective atmosphere with the assistance of argon purge, and the pressure was 15 Pa. The quartz tube was placed in a muffle furnace and kept at 1000 ° C for 24 hours. After the reaction was completed, it was quenched and cooled to room temperature in an ice-water mixture medium. The block sample was taken out of the quartz tube and ground, and the powder sample was washed three times with deionized water, and the powder sample was washed once with anhydrous ethanol and dried to obtain a pure phase λ-Ti3O5 powder with a particle size of 100 nanometers and a high solar light absorption efficiency of 96.4%.

[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of the substantial technical content of the present invention. The substantial technical content of the present invention is broadly defined in the scope of the claims of the application. Any technical entity or method completed by others, if it is exactly the same as that defined in the scope of the claims of the application or an equivalent variation, will be deemed to be included in the scope of the claims.

Claims

1. A method for preparing a titanium-based oxide magneli phase material, characterized in that: The following steps are involved: 1) According to the titanium-oxygen stoichiometric ratio of the fitted magneli phase titanium oxide, titanium and titanium oxide precursors are weighed and mixed stoichiometrically, and functional groups irrelevant to the final product are removed by pre-calcination; 2) According to the phase stability zone temperature of the fitted magneli phase titanium oxide, a metal halide flux and a flux combination with a melting point adapted thereto are selected, and added to the above-mentioned precursor mixed powder in a certain proportion; 3) The precursor mixed with flux is encapsulated in a quartz tube with a certain atmosphere and heated to a certain temperature so that the precursor is fully dissolved in the molten halide flux; Then, the mixture is kept at this temperature for a period of time and then cooled to room temperature at a certain cooling rate. During this process, the magneli phase titanium oxide is precipitated together with the gradually solidified halide flux in a non-uniform nucleation process. 4) The halide flux in the obtained powder product is removed by washing with water and ethanol solvents, and a pure phase magneli phase titanium oxide powder material is obtained after drying; the obtained powder is further added with a binder, cold-pressed and granulated, and then sintered to obtain a magneli phase titanium oxide ceramic material.

2. A method for preparing a titanium-based oxide magneli phase material according to claim 1, characterized in that: Step 1) The chemical composition of the synthesized magneli phase titanium oxide is Ti n O 2n-1 , where n=2-9, and when the precursors are TiO2 and titanium metal, the molar ratios are TiO2:Ti=3:1 (n=2), 5:1 (n=3), 7:1 (n=4), 9:1 (n=5), 11:1 (n=6), 13:1 (n=7), 15:1 (n=8), and 17:1 (n=9), respectively; the prepared magneli phase titanium oxide has metal-insulator phase transition characteristics under characteristic temperature triggering; the metal-insulator phase transition characteristics can be adjusted in a wide range of 120 K to 460 K by adjusting n, or multi-level phase transition characteristics can be achieved through specific structures.

3. The method for preparing a titanium-based oxide magneli phase material according to claim 1, characterized in that: The precursors described in step 1) include titanium dioxide, other titanium compounds and elemental titanium; the titanium dioxide used includes rutile phase titanium dioxide, anatase phase titanium dioxide, rutile / anatase mixed phase titanium dioxide and other titanium dioxide isomers; the other titanium compound used is titanium hydroxide; the elemental titanium used is nano-metal titanium powder, micron-metal titanium powder, and metal titanium particles, with a particle size ranging from 200 nm to 2 mm; the precursors used are directly mixed or pre-heated in air to remove crystal water and surface grease before mixing; by controlling the type, size, and phase of the precursors, the degree of sudden change in resistivity of the synthesized powder metal insulator transition, thermal stability, and electrocatalytic performance can be regulated.

4. The method for preparing a titanium-based oxide magneli phase material according to claim 1, characterized in that: The central metal ion Ti in step 1) can be partially replaced by other transition metal ions to further control the basic resistivity of the material, the phase transition characteristics of the metal insulator, the oxidative thermal stability, and the catalytic properties in the acidic solution environment; the doping elements include Fe, V, Co, Cr, Nb, Mo, and Mn, and their corresponding precursors are equivalent oxides of the corresponding transition metals, including Fe2O3, VO2, Co2O3, Cr2O3, Nb2O5, MoO2, and MnO2; the phase transition temperature of the doped magneli phase titanium oxide gradually decreases with the increase of the doping amount until it fully exhibits the metal electrical transport characteristics, and the room temperature conductivity can reach 10 -5 Ω·m quantity; doping can also significantly improve the thermal stability and electrochemical activity of magneli phase titanium oxide.

5. The method for preparing a titanium-based oxide magneli phase material according to claim 1, characterized in that: The flux described in step 2) has a melting point lower than the melting point required for the magneli phase titanium oxide, and can dissolve and uniformly disperse the precursor powder in a high-temperature molten state to reduce its nucleation thermodynamic potential and achieve non-uniform nucleation of the product in the flux; the metal halide flux includes LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, CsI; a single flux can be used, or a binary or multi-component combination of the above flux systems can be used, preferably a KCl and LiCl eutectic system, a KCl and NaCl eutectic system, and a KCl and NaCl and LiCl eutectic system, so as to match the lattice parameters of the flux with the lattice parameters of the specific crystal planes of the magneli phase; the molar ratio of the metal halide flux to the titanium element in the precursor is 0.1-100.

6. A method for preparing a titanium-based oxide magneli phase material as claimed in claim 1, characterized in that: Step 3) The synthetic atmosphere includes a rough vacuum (10 -2 -10 -1 Pa), high vacuum (10 -4 -10 -3 Pa), ultra-high vacuum (less than or equal to 10 -5 Pa), inert gas atmosphere, preferably nitrogen or argon atmosphere; under different synthesis atmosphere conditions, the reference temperature is determined according to different magneli phase titanium oxide target products, so that the reaction process is located in the product equilibrium phase region corresponding to the oxygen partial pressure-temperature phase diagram, thereby avoiding the generation of impurity phases; under the reaction condition of 1100 °C, Ti n O 2n-1 The oxygen partial pressure balance interval is 10 -20.7 -10. -17.5 Pa(n=2)、10 -17.5 -10 -14.6 Pa(n=3)、10 -14.6 -10 -12.9 Pa(n=4)、10 -12.9 -10 -12.6 Pa(n=5)、10 -12.6 -10 -12.2 Pa(n=6)、10 -12.2 -10 -12.1 Pa(n=7)、10 -12.1 -10 -12.0 Pa(n=8)、10 -12.0 -10 -11.9 Pa (n=9).

7. A method for preparing a titanium-based oxide magneli phase material according to claim 1, characterized in that: Step 3) The solid phase reaction heat treatment system is divided into two stages. The selection of the heat treatment system in the heating stage is determined by the stable phase region of the magneli phase titanium oxide under the selected synthesis atmosphere conditions, and the temperature is selected to be 100-300 °C lower than the median temperature of the phase region, at which the flux can fully melt and evenly disperse the precursor powder; the heat treatment system in the cooling stage selects a cooling rate of 0.1-10 °C / min, air cooling or quenching, and the quenching medium is selected from water, oil, ice-water mixture and liquid nitrogen, so that the magneli phase titanium oxide and the flux are precipitated simultaneously in a non-uniform nucleation manner; the directional regulation of the isomer ratio in the magneli phase titanium oxide product can also be achieved by precisely controlling the cooling rate.

8. The method for preparing a titanium-based oxide magneli phase material according to claim 1, characterized in that: By regulating the particle size of titanium oxide and titanium salt precursors, metallic titanium precursors, the proportion of flux, the holding temperature and time, the cooling rate, and the vacuum degree, the particle size of the prepared titanium-based oxide magneli phase powder can be regulated; by selecting the type of flux, the surface crystal orientation of the prepared titanium-based oxide magneli phase powder can be regulated.