Vanadium oxychloride-based vanadium trichloride and preparation method thereof

Through the chlorination reaction between vanadium source and chlorinating agent and the low-temperature solid-liquid separation, the problems of environmental pollution and high energy consumption in the preparation of vanadium trichloride are solved, and low-cost, high-purity vanadium trichloride preparation is achieved, with environmental Friendly, low cost, short time and low energy consumption.

CN119059560APending Publication Date: 2024-12-03WUHAN UNIV OF SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411057631.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing vanadium trichloride preparation methods have problems such as environmental pollution, high cost, long time consumption, large energy consumption and high impurity content.

Method used

The chlorination reaction of vanadium source and chlorinating agent is used to form vanadyl oxychloride, and then the solid-liquid separation is added at low temperatures, avoiding additional heating and protective gases. , the preparation of vanadium trichloride was achieved.

Benefits of technology

It achieves environmentally friendly low cost, low energy consumption, and preparation of high-purity vanadium trichloride in a short time, reducing impurity content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059560A_ABST
    Figure CN119059560A_ABST
Patent Text Reader

Abstract

The invention relates to vanadium oxytrichloride-based vanadium trichloride and a preparation method thereof. According to the technical scheme, a vanadium source and a chlorinating agent are mixed to obtain a chlorination rectification raw material; placing the chlorination rectification raw material in a distillation device, introducing a protective atmosphere, carrying out a chlorination reaction, and condensing to obtain a vanadium oxytrichloride liquid; adding an additive into the vanadium oxytrichloride liquid, and stirring to obtain a vanadium oxytrichloride mixed liquid; adding a reducing agent into the vanadium oxytrichloride mixed solution, stirring at 0-40 DEG C, standing, and carrying out solid-liquid separation to obtain a vanadium trichloride solution and waste residues; and drying the vanadium trichloride solution in a vacuum drying oven to obtain the vanadium oxytrichloride-based vanadium trichloride. The method has the characteristics of environmental friendliness, low cost, short time consumption, low energy consumption and simple process, and the impurity content of the vanadium oxychloride-based vanadium trichloride prepared by the method is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vanadium trichloride, and specifically relates to vanadium trichloride based on vanadium oxytrichloride and a preparation method thereof. Background Art

[0002] Vanadium trichloride is an inorganic compound widely used in the production of various alloys and catalysts. In recent years, with the continuous development of steel, chemical industry, biology and other fields, the market demand for vanadium trichloride has shown a rapid growth trend. At present, vanadium trichloride is usually prepared by thermal decomposition of vanadium tetrachloride or reaction of vanadium trioxide with disulfur dichloride, but there are problems such as complex process and high cost of raw material preparation. Therefore, the development of a new preparation method of vanadium trichloride is of concern to those skilled in the art.

[0003] The patented technology of "Method for preparing metallic vanadium powder" (CN111266597B) uses vanadium-containing powder as vanadium source, including high-grade vanadium-containing intermediate alloy powder such as FeV80 and AlV85, and chlorine as chlorination medium, and performs boiling chlorination to obtain the initial vanadium trichloride. The initial vanadium trichloride is subjected to two-step distillation at 160-180°C to obtain vanadium trichloride. The purity of vanadium trichloride prepared by this method is above 99.5%, but this technology introduces chlorine as the chlorination medium, which causes great pollution to the environment, and the reaction is heated and distilled, and the reaction temperature is relatively high.

[0004] The patented technology of "A method for recycling vanadium resources" (CN113737024A) adds activated carbon to vanadium-containing refined titanium tetrachloride to reduce vanadium trichloride in titanium tetrachloride to vanadium trichloride, and the obtained vanadium-containing solution is subjected to sedimentation and solid-liquid separation to obtain the product. Although this method can prepare vanadium trichloride products, the activated carbon solid used cannot react well with the vanadium trichloride liquid, and the obtained product has a high impurity content, and the activated carbon has a low reduction strength, a large amount of addition, and a high cost.

[0005] The patented technology of "A vanadium trichloride and preparation method based on vanadium trichloride, a product of vanadium shale chlorination distillation" (2024108714836) adds mineral oil to the vanadium trichloride raw material of chlorination distillation, stirs at 50-100°C for more than 30 minutes to reduce the vanadium trichloride to vanadium trichloride, then adds alcohol to the solution, lets it stand for more than 18 hours, takes the supernatant and dries it to obtain the vanadium trichloride product. In the process of preparing vanadium trichloride by this method, mineral oil and alcohol cannot be separated well, the standing time is long, the temperature is high during the reaction, and the energy consumption is high.

[0006] In summary, the existing vanadium trichloride preparation method has the disadvantages of being environmentally unfriendly, high cost, time-consuming, high energy consumption and high impurity content. Summary of the invention

[0007] The present invention aims to overcome the defects of the prior art and aims to provide a method for preparing vanadium trichloride based on vanadium oxychloride which has simple process, low cost and is environmentally friendly. The vanadium trichloride based on vanadium oxychloride prepared by the method has low impurity content.

[0008] To achieve the above purpose, the specific steps of the technical solution adopted by the present invention are:

[0009] Step 1: Chlorination distillation

[0010] Step 1.1, according to the molar ratio of vanadium in the vanadium source: chlorinating agent being 1: (1-4), the vanadium source and the chlorinating agent are mixed to obtain a chlorination distillation raw material.

[0011] Step 1.2, placing the chlorination distillation raw material in a distillation device, introducing a protective atmosphere, and carrying out a chlorination reaction at 150-190° C. for 1-3 hours to obtain vanadium trichloride gas; condensing to obtain vanadium trichloride liquid.

[0012] Step 2, preparation of vanadium trichloride

[0013] Step 2.1, adding the additive to the vanadium oxychloride liquid at a volume ratio of the vanadium oxychloride liquid to the additive of 1:(1-20), stirring, and obtaining a vanadium oxychloride mixed liquid.

[0014] Step 2.2, according to the mass ratio of the vanadium trichloride mixed solution: reducing agent being 40: (0.5-1), adding the reducing agent to the vanadium trichloride mixed solution, stirring for 5-15 minutes at a temperature of 0-40° C., standing, and solid-liquid separation to obtain a vanadium trichloride solution and waste residue.

[0015] Step 2.3: placing the vanadium trichloride solution in a vacuum drying oven and drying it at 80-120° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

[0016] The vanadium source is sodium vanadate or potassium vanadate.

[0017] The chlorinating agent is aluminum chloride, or a mixture of zinc chloride and aluminum chloride.

[0018] The protective atmosphere is nitrogen or argon.

[0019] The additive is anhydrous ethanol or acetic acid.

[0020] The reducing agent is aluminum powder or zinc powder.

[0021] The vacuum degree of the vacuum drying oven is -0.08 to -0.1 MPa.

[0022] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:

[0023] 1. The present invention uses aluminum powder or zinc powder as a reducing agent to reduce vanadium trichloride to prepare vanadium trichloride. Compared with the existing process of preparing vanadium tetrachloride by introducing a large amount of chlorine into vanadium oxide and then pyrolyzing to prepare vanadium trichloride, or converting vanadium master alloy into vanadium trichloride under chlorine and 160-180°C, the present invention does not need to introduce additional protective gas, avoids the problem of chlorine pollution, and is environmentally friendly. Compared with the existing vanadium trichloride preparation process, the present invention is an exothermic reaction, has no heating process, reacts at room temperature, has a low reaction temperature, has low energy consumption, and has a simple process.

[0024] 2. The present invention adds anhydrous ethanol or acetic acid as an additive to vanadium trichloride, and reacts with a reducing agent to prepare vanadium trichloride based on vanadium trichloride. Compared with the use of organic solvents to prepare vanadium trichloride, the reaction is carried out in anhydrous ethanol or acetic acid medium, and aluminum powder or zinc powder is combined with oxygen in vanadium trichloride to generate metal oxides to achieve the effect of reduction. It can react with liquid vanadium trichloride quickly and fully, requires less raw materials, and has low cost. The metal oxide generated by the reaction forms a precipitate in anhydrous ethanol or acetic acid medium. Compared with the standing time used for liquid-liquid separation used in the existing organic solvent preparation process, the solid-liquid separation used in the present invention is not only time-consuming, but also does not introduce other impurities into the supernatant, and the impurity content is low.

[0025] Therefore, the present invention has the characteristics of being environmentally friendly, low cost, short time consumption, low energy consumption and simple process. The vanadium trichloride prepared by the method has low impurity content. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention discloses a Fourier transform infrared absorption spectrum of vanadium trichloride based on vanadium oxychloride prepared by the present invention. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but is not intended to limit the scope of protection thereof.

[0028] A vanadium trichloride based on vanadium oxychloride and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:

[0029] Step 1: Chlorination distillation

[0030] Step 1.1, according to the molar ratio of vanadium in the vanadium source: chlorinating agent being 1: (1-4), the vanadium source and the chlorinating agent are mixed to obtain a chlorination distillation raw material.

[0031] Step 1.2, placing the chlorination distillation raw material in a distillation device, introducing a protective atmosphere, and carrying out a chlorination reaction at 150-190° C. for 1-3 hours to obtain vanadium trichloride gas; condensing to obtain vanadium trichloride liquid.

[0032] Step 2, preparation of vanadium trichloride

[0033] Step 2.1, adding the additive to the vanadium oxychloride liquid according to the volume ratio of the vanadium oxychloride liquid additive of 1:(1-20), stirring, and obtaining a vanadium oxychloride mixed liquid.

[0034] Step 2.2, according to the mass ratio of the vanadium trichloride mixed solution to the reducing agent being 40: (0.5-1), adding the reducing agent to the vanadium trichloride mixed solution, stirring for 5-15 minutes at a temperature of 20-30° C., standing, and solid-liquid separation to obtain a vanadium trichloride solution and waste residue.

[0035] Step 2.3: placing the vanadium trichloride solution in a vacuum drying oven and drying it at 80-120° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

[0036] The vanadium source is sodium vanadate or potassium vanadate.

[0037] The chlorinating agent is aluminum chloride, or a mixture of zinc chloride and aluminum chloride.

[0038] The protective atmosphere is nitrogen or argon.

[0039] The additive is anhydrous ethanol or acetic acid.

[0040] The reducing agent is aluminum powder or zinc powder.

[0041] The vacuum degree of the vacuum drying oven is -0.08 to -0.1 MPa.

[0042] Example 1

[0043] A vanadium trichloride based on vanadium oxychloride and a preparation method thereof. The steps of the preparation method described in this embodiment are:

[0044] Step 1: Chlorination distillation

[0045] Step 1.1, according to the molar ratio of vanadium in the vanadium source: chlorinating agent being 1:4, the vanadium source and the chlorinating agent are mixed to obtain a chlorination distillation raw material.

[0046] Step 1.2, placing the chlorination distillation raw material in a distillation apparatus, introducing a protective atmosphere, and carrying out a chlorination reaction at 190° C. for 1 hour to obtain vanadium trichloride gas; and condensing to obtain vanadium trichloride liquid.

[0047] Step 2, preparation of vanadium trichloride

[0048] Step 2.1, adding the additive to the vanadium oxychloride liquid at a volume ratio of vanadium oxychloride liquid to additive of 1:5, stirring to obtain a vanadium oxychloride mixed liquid.

[0049] Step 2.2, according to the mass ratio of the vanadium trichloride mixed solution: reducing agent being 40:0.8, adding the reducing agent to the vanadium trichloride mixed solution, placing in a heating magnetic stirrer, stirring at a temperature of 0°C for 15 minutes, standing, solid-liquid separation, and obtaining a vanadium trichloride solution and waste residue.

[0050] Step 2.4: placing the supernatant in a vacuum drying oven and drying it at 100° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

[0051] The vanadium source is sodium vanadate.

[0052] The chlorinating agent is a mixture of zinc chloride and aluminum chloride.

[0053] The protective atmosphere is nitrogen.

[0054] The additive is anhydrous ethanol.

[0055] The reducing agent is aluminum powder.

[0056] The vacuum degree of the vacuum drying oven is -0.08MPa.

[0057] Example 2

[0058] A vanadium trichloride based on vanadium oxychloride and a preparation method thereof. The steps of the preparation method described in this embodiment are:

[0059] Step 1: Chlorination distillation

[0060] Step 1.1, according to the molar ratio of vanadium in the vanadium source: chlorinating agent being 1:3, the vanadium source and the chlorinating agent are mixed to obtain a chlorination distillation raw material.

[0061] Step 1.2, placing the chlorination distillation raw material in a distillation apparatus, introducing a protective atmosphere, and carrying out a chlorination reaction at 180° C. for 2 hours to obtain vanadium trichloride gas; and condensing to obtain vanadium trichloride liquid.

[0062] Step 2, preparation of vanadium trichloride

[0063] Step 2.1, adding the additive to the vanadium oxychloride liquid at a volume ratio of vanadium oxychloride liquid to additive of 1:10, stirring to obtain a vanadium oxychloride mixed liquid.

[0064] Step 2.2, adding the reducing agent to the vanadium trichloride mixed solution according to the mass ratio of the vanadium trichloride mixed solution to the reducing agent being 40:0.7, stirring for 13 minutes at a temperature of 10° C., to obtain a vanadium trichloride solution and waste residue.

[0065] Step 2.4: placing the supernatant in a vacuum drying oven and drying at 90° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

[0066] The vanadium source is potassium vanadate.

[0067] The chlorinating agent is a mixture of zinc chloride and aluminum chloride.

[0068] The protective atmosphere is nitrogen.

[0069] The additive is acetic acid.

[0070] The reducing agent is aluminum powder.

[0071] The vacuum degree of the vacuum drying oven is -0.1 MPa.

[0072] Example 3

[0073] A vanadium trichloride based on vanadium oxychloride and a preparation method thereof. The steps of the preparation method described in this embodiment are:

[0074] Step 1: Chlorination distillation

[0075] Step 1.1, according to the molar ratio of vanadium in the vanadium source: chlorinating agent being 1:2, the vanadium source and the chlorinating agent are mixed to obtain a chlorination distillation raw material.

[0076] Step 1.2, placing the chlorination distillation raw material in a distillation apparatus, introducing a protective atmosphere, and carrying out a chlorination reaction at 170° C. for 1 hour to obtain vanadium trichloride gas; and condensing to obtain vanadium trichloride liquid.

[0077] Step 2, preparation of vanadium trichloride

[0078] Step 2.1, adding the additive to the vanadium oxychloride liquid at a volume ratio of vanadium oxychloride liquid to additive of 1:20, stirring to obtain a vanadium oxychloride mixed liquid.

[0079] Step 2.2, adding the reducing agent to the vanadium trichloride mixed solution according to the mass ratio of the vanadium trichloride mixed solution to the reducing agent being 40:0.5, stirring for 5 minutes at a temperature of 40° C., to obtain a vanadium trichloride solution and waste residue.

[0080] Step 2.4: placing the supernatant in a vacuum drying oven and drying at 120° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

[0081] The vanadium source is sodium vanadate.

[0082] The chlorinating agent is a mixture of zinc chloride and aluminum chloride.

[0083] The protective atmosphere is nitrogen.

[0084] The additive is anhydrous ethanol.

[0085] The reducing agent is zinc powder.

[0086] The vacuum degree of the vacuum drying oven is -0.08MPa.

[0087] Example 4

[0088] A vanadium trichloride based on vanadium oxychloride and a preparation method thereof. The steps of the preparation method described in this embodiment are:

[0089] Step 1: Chlorination distillation

[0090] Step 1.1, mixing the vanadium source with the chlorinating agent at a molar ratio of vanadium in the vanadium source to the chlorinating agent of 1:1 to obtain a chlorination distillation raw material.

[0091] Step 1.2, placing the chlorination distillation raw material in a distillation device, passing a protective atmosphere, and carrying out a chlorination reaction at 150° C. for 3 hours to obtain vanadium trichloride gas; condensing to obtain vanadium trichloride liquid.

[0092] Step 2, preparation of vanadium trichloride

[0093] Step 2.1, adding the additive to the vanadium oxychloride liquid at a volume ratio of vanadium oxychloride liquid to additive of 1:1, stirring to obtain a vanadium oxychloride mixed liquid.

[0094] Step 2.2, adding the reducing agent to the vanadium trichloride mixed solution according to the mass ratio of the vanadium trichloride mixed solution to the reducing agent being 40:1, stirring for 8 minutes at a temperature of 30° C. to obtain a vanadium trichloride solution and waste residue.

[0095] Step 2.4: placing the supernatant in a vacuum drying oven and drying at 80° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

[0096] The vanadium source is sodium vanadate.

[0097] The chlorinating agent is aluminum chloride.

[0098] The protective atmosphere is argon.

[0099] The additive is acetic acid.

[0100] The reducing agent is zinc powder.

[0101] The vacuum degree of the vacuum drying oven is -0.09 MPa.

[0102] Example 5

[0103] A vanadium trichloride based on vanadium oxychloride and a preparation method thereof. The steps of the preparation method described in this embodiment are:

[0104] Step 1: Chlorination distillation

[0105] Step 1.1, according to the molar ratio of vanadium in the vanadium source: chlorinating agent being 1:2, the vanadium source and the chlorinating agent are mixed to obtain a chlorination distillation raw material.

[0106] Step 1.2, placing the chlorination distillation raw material in a distillation apparatus, introducing a protective atmosphere, and carrying out a chlorination reaction at 160° C. for 2 hours to obtain vanadium trichloride gas; and condensing to obtain vanadium trichloride liquid.

[0107] Step 2, preparation of vanadium trichloride

[0108] Step 2.1, adding the additive to the vanadium oxychloride liquid at a volume ratio of vanadium oxychloride liquid to additive of 1:15, stirring to obtain a vanadium oxychloride mixed liquid.

[0109] Step 2.2, adding the reducing agent to the vanadium trichloride mixed solution according to the mass ratio of the vanadium trichloride mixed solution to the reducing agent being 40:0.6, stirring for 11 minutes at a temperature of 20° C. to obtain a vanadium trichloride solution and waste residue.

[0110] Step 2.4: placing the supernatant in a vacuum drying oven and drying at 110° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

[0111] The vanadium source is potassium vanadate.

[0112] The chlorinating agent is aluminum chloride.

[0113] The protective atmosphere is argon.

[0114] The additive is anhydrous ethanol.

[0115] The reducing agent is zinc powder.

[0116] The vacuum degree of the vacuum drying oven is -0.1 MPa.

[0117] Compared with the prior art, this specific implementation has the following positive effects:

[0118] 1. This specific embodiment uses aluminum powder or zinc powder as a reducing agent to reduce vanadium trichloride to prepare vanadium trichloride. Compared with the existing process of preparing vanadium tetrachloride by introducing a large amount of chlorine into vanadium oxide and then pyrolyzing to prepare vanadium trichloride, or converting vanadium intermediate alloy into vanadium trichloride under chlorine and 160-180°C, this specific embodiment does not need to introduce additional protective gas, avoids the problem of chlorine environmental pollution, and is environmentally friendly. Compared with the traditional vanadium trichloride preparation process, this specific embodiment is an exothermic reaction, without a heating process, and reacts at room temperature, with a low reaction temperature and low energy consumption.

[0119] 2. In this specific embodiment, anhydrous ethanol or acetic acid is added as an additive to vanadium trichloride, and reacted with a reducing agent to prepare vanadium trichloride. Compared with the use of organic solvents to prepare vanadium trichloride, the reaction is carried out in anhydrous ethanol or acetic acid medium, and aluminum powder or zinc powder is combined with oxygen in vanadium trichloride to form metal oxides, thereby achieving the effect of reduction. It can react quickly and fully with liquid vanadium trichloride, and the corresponding raw materials required are less and the cost is low. The metal oxide generated by the reaction forms a precipitate in the anhydrous ethanol or acetic acid medium. Compared with the standing time used for liquid-liquid separation used in the existing organic solvent preparation process, the solid-liquid separation used in this specific embodiment is not only time-consuming, but also does not introduce other impurities into the supernatant, and the impurity content is low. The method for preparing vanadium trichloride based on vanadium trichloride in this specific embodiment is shown in the accompanying drawings. Figure 1 is the Fourier transform infrared absorption spectrum of vanadium trichloride based on vanadium oxychloride prepared in Example 1; Figure 1 It can be seen that the prepared vanadium trichloride based on vanadium oxychloride has basically no impurity peaks, low impurity content, and good matching degree with the standard sample.

[0120] Therefore, the present specific implementation mode has the characteristics of being environmentally friendly, low cost, short time consumption, low energy consumption and simple process. The vanadium trichloride prepared by the method has a low impurity content based on vanadium oxychloride.

Claims

1. A method for preparing vanadium trichloride based on vanadium oxychloride, characterized in that The specific steps of the preparation method are: Step 1: Chlorination distillation Step 1.1, mixing the vanadium source and the chlorinating agent according to the molar ratio of vanadium in the vanadium source to the chlorinating agent being 1:(1-4) to obtain a chlorination distillation raw material; Step 1.2, placing the chlorination rectification raw material in a distillation device, introducing a protective atmosphere, and performing a chlorination reaction at 150-190° C. for 1-3 hours to obtain vanadium trichloride gas; condensing to obtain vanadium trichloride liquid; Step 2, preparation of vanadium trichloride Step 2.1, adding the additive to the vanadium oxychloride liquid at a volume ratio of vanadium oxychloride liquid to additive of 1:(1-20), stirring to obtain a vanadium oxychloride mixed solution; Step 2.2, according to the mass ratio of the vanadium trichloride mixed solution: the reducing agent being 40: (0.5-1), adding the reducing agent to the vanadium trichloride mixed solution, stirring for 5-15 minutes at a temperature of 0-40° C., standing, and solid-liquid separation to obtain a vanadium trichloride solution and waste residue; Step 2.3: placing the vanadium trichloride solution in a vacuum drying oven and drying it at 80-120° C. to obtain vanadium trichloride based on vanadium oxytrichloride.

2. The method for preparing vanadium trichloride based on vanadium oxychloride according to claim 1, characterized in that The vanadium source is sodium vanadate or potassium vanadate.

3. The method for preparing vanadium trichloride based on vanadium oxychloride according to claim 1, characterized in that The chlorinating agent is aluminum chloride, or a mixture of zinc chloride and aluminum chloride.

4. The method for preparing vanadium trichloride based on vanadium oxychloride according to claim 1, characterized in that The protective atmosphere is nitrogen or argon.

5. The method for preparing vanadium trichloride based on vanadium oxychloride according to claim 1, characterized in that The additive is anhydrous ethanol or acetic acid.

6. The method for preparing vanadium trichloride based on vanadium oxychloride according to claim 1, characterized in that The reducing agent is aluminum powder or zinc powder.

7. The method for preparing vanadium trichloride based on vanadium oxychloride according to claim 1, characterized in that The vacuum degree of the vacuum drying oven is -0.08 to -0.1 MPa.

8. A vanadium trichloride based on vanadium oxychloride, characterized in that The vanadium trichloride-based vanadium trichloride is a vanadium trichloride-based vanadium trichloride prepared according to the method for preparing vanadium trichloride-based vanadium trichloride according to any one of claims 1 to 7.

Citation Information

Cited By

  • Method for enriching and purifying vanadium through fused salt chlorination rectification

    CN119800116A

  • A method for enriching and purifying vanadium by molten salt chlorination distillation

    CN119800116B