Preparation method of sodium ion battery negative electrode material

Through amidation and zinc doping treatment of modified biomass materials, nitrogen-doped porous hard carbon was prepared, which solved the problems of low specific capacity and poor stability of the negative electrode material of sodium ion battery, and achieved high capacity and high efficiency battery performance. And reduce costs.

CN119079970APending Publication Date: 2024-12-06SUZHOU GUONA ZHICHUANG TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311787631.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing sodium ion battery hard carbon anode materials have low specific capacity, poor cycle stability, poor rate performance and high cost.

Method used

Modify the biomass material through amidation reaction, add it to zinc salt solution and heat it and stir it with magnetic stirring, and then freeze-dry it and carbide it to prepare the negative electrode material of nitrogen-doped zinc pore-making sodium ion battery, and use the chelation of EDTA to promote Zn ion uniformity. Dispersion and pore formation.

Benefits of technology

It improves the reversible capacity of the negative electrode material of sodium ion battery and the first week of Coulomb efficiency, reduces costs, and has industrial advantages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079970A_ABST
    Figure CN119079970A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sodium-ion batteries, and discloses a preparation method of a sodium-ion battery negative electrode material, which comprises the following steps: S1, amidation reaction: in an organic solvent, carrying out amidation reaction on a biomass material and a catalyst to obtain an EDTA modified biomass material; s2, mixing and stirring: adding a pyridine compound after the reaction of the EDTA modified biomass material is completed, performing ultrasonic treatment after uniform stirring, and performing centrifugal treatment after baking in an oven; s3, preparing a precursor: adding the modified biomass material into a zinc salt solution, uniformly dispersing the modified biomass material by using a constant-temperature heating magnetic stirrer, heating in a water bath, and then freeze-drying to obtain a zinc ion doped biomass precursor; and S4, carrying out carbonization treatment. The sodium-ion battery negative electrode material is large in reversible capacity and high in first-week coulombic efficiency, and compared with the same type, the sodium-ion battery negative electrode material is simple in step and low in cost and has considerable industrial advantages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for preparing a negative electrode material for a sodium ion battery. Background Art

[0002] As the second largest alkali metal after lithium in the periodic table, sodium has similar physical and chemical properties to lithium. It is widely distributed in the earth's crust and has abundant reserves. Therefore, the cost of sodium is much lower than that of lithium. In addition, sodium ions do not react with aluminum, so aluminum can be used as a current collector in sodium-ion batteries, replacing copper used in traditional lithium-ion batteries, further reducing the overall cost of the battery. Sustainable sodium-ion batteries (SIBs), as an energy storage system, are widely regarded as a promising solution to replace market-dominant lithium-ion batteries to alleviate the shortage of lithium resources.

[0003] In recent years, many sodium ion battery positive electrode materials with excellent performance have been successfully developed based on lithium ion battery positive electrode materials. Commercial graphite has shown excellent performance as a negative electrode material for lithium ion batteries. Ethylenediaminetetraacetic acid (EDTA) is a commonly used chelating agent that has the ability to form stable complexes with metal ions. It can regulate the adsorption behavior and dispersion state of metal ions by forming complexes with metal ions, thereby regulating the preparation and performance of nanoparticles. By changing the charge properties of the surface of the object, EDTA can affect the adsorption behavior of metal ions and form stable complexes with metal ions, thereby affecting their distribution at the solid-liquid interface.

[0004] Carbonized biomass materials refer to biomass materials that are treated at high temperatures to undergo a carbonization reaction and be converted into carbon materials. There are many natural organic substances in nature, such as biomass, which have unique advantages in the preparation of hard carbon materials. These natural organic substances, as good precursors of hard carbon materials, have unique intrinsic morphology and structure, as well as excellent thermal stability and conductivity. However, these natural organic substances, as hard carbon materials, have many irreversible sodium storage structures and defects, resulting in the specific capacity of most hard carbon materials being less than 300.0 mAh / g, and their rate performance also has some problems. Therefore, a method for preparing a negative electrode material for a sodium ion battery is proposed. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing a negative electrode material for a sodium ion battery, which solves the problems of low specific capacity, poor cycle stability, poor rate performance and high cost of the existing hard carbon negative electrode materials for sodium ion batteries.

[0007] (II) Technical solution

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A method for preparing a negative electrode material for a sodium ion battery comprises the following steps:

[0010] S1: amidation reaction, in an organic solvent, the biomass material is subjected to an amidation reaction with a catalyst to obtain an EDTA-modified biomass material;

[0011] S2: mixing and stirring, adding a pyridine compound after the EDTA-modified biomass material has completed the reaction, stirring evenly, ultrasonicating, baking in an oven, and then centrifuging;

[0012] S3: preparing a precursor, adding the modified biomass material to a zinc salt solution, uniformly dispersing it using a constant temperature heating magnetic stirrer, heating it in a water bath, and then freeze-drying it to obtain a zinc ion-doped biomass precursor;

[0013] S4: Carbonization treatment, carbonizing the biomass material under the protection of an inert gas to obtain the corresponding nitrogen-doped zinc pore-forming sodium ion battery negative electrode material.

[0014] Furthermore, the biomass material in S1 is one of basswood, cellulose, lignin and chitin.

[0015] Based on the above, the organic solvent in S1 is one of DMF, DMSO, DMA and HMPT.

[0016] As a further solution of the present invention, the water bath heating temperature in S3 is between 50 degrees and 90 degrees, and the carbonization treatment time in S4 is between 1 hour and 5 hours.

[0017] Furthermore, the pyridine compound in S2 is one of pyridine, 2-hydroxymethylpyridine, 3,5-dichloropyridine, and aminopyridine.

[0018] Based on the above, the inert gas in S4 is one of argon, nitrogen, and hydrogen argon (5% hydrogen).

[0019] As a further solution of the present invention, the carbonization treatment temperature in S4 is between 500 degrees and 1400 degrees, and the carbonization treatment time is between 2 hours and 8 hours.

[0020] Furthermore, the catalyst in S1 includes one or more of dipyridine, 1,0-phenanthroline, ethylenediaminetetraacetic acid, ethylenediamine, nitrosodiacetic acid, oxalate, dithizone, 8-hydroxyquinoline, o-phenanthroline (C12H8N2), and potassium sodium tartrate.

[0021] Based on the above, the zinc salt in S3 is one or more of ZnCl2, ZnSO4, Zn(NO3)2, Zn(ClO4)2, and Zn(BF4)2.

[0022] (III) Beneficial effects

[0023] Compared with the prior art, the present invention provides a method for preparing a negative electrode material for a sodium ion battery, which has the following beneficial effects:

[0024] The present invention has strong universality, simple process and obvious performance improvement. A large amount of uniformly dispersed Zn activator is introduced into basswood. EDTA (ethylenediaminetetraacetic acid) and its derivatives (such as EDTAD) usually have a chelating effect. They are grafted onto fibers to promote the uniform dispersion of Zn ions in wood fibers, and uniform pores are formed in the subsequent pyrolysis process. The EDTAD with chelating effect is introduced into the structure of basswood by a swelling method. The combination of EDTAD introduces carboxyl groups into wood cellulose, which enhances the coordination binding between cellulose macromolecules and Zn metal ions. While successfully fixing Zn ions in the structure of basswood fibers, nitrogen doping is introduced to obtain a hard carbon precursor containing uniformly dispersed Zn ions. Then, high-temperature pyrolysis is performed to evaporate Zn species, leaving a rich pore structure, and a nitrogen-doped porous hard carbon material with rich defect sites and a large interlayer spacing is prepared. The negative electrode material of the sodium ion battery of the present invention has a large reversible capacity and a high first-week coulomb efficiency. Compared with the same type of inventions, the steps are simple and the cost is low, and it has considerable industrial advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The infrared spectra of the untreated biomass material and the chemically modified biomass material in Example 1 of the present invention;

[0026] Figure 2 TEM image of the sodium ion battery negative electrode material prepared in Example 1 of the present invention;

[0027] Figure 3 The charge and discharge curve of the negative electrode of the sodium ion battery prepared in Example 1 of the present invention;

[0028] Figure 4 This is the charge and discharge curve of the first five cycles of the untreated sodium ion battery negative electrode;

[0029] Figure 5 The present invention is a schematic flow chart of a method for preparing a negative electrode material for a sodium ion battery. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] Reference Figure 1-5 , a method for preparing a negative electrode material for a sodium ion battery, comprising the following steps:

[0033] Take 500 mg of EDTAD and dissolve it in 80 ml of DMF, and add 1.5 ml of pyridine to stably disperse the EDTAD in the solution. Add 800 mg of basswood pretreated by ball milling to the above solution, ultrasonicate for 1 hour, and then place the mixture in a 90-degree oven for 24 hours. Centrifuge the mixture, pour off the supernatant, and obtain EDTAD-modified basswood chips.

[0034] Preparation of Zn-rich sawdust: Add EDTAD-modified basswood to 30 ml of 0.5 M ZnAc2 DMF solution, disperse it evenly using a constant temperature heating magnetic stirrer, and heat it in a water bath at 75°C for 2 hours; centrifuge the mixture to remove excess liquid, wash it once with acetone, once with alcohol, and twice with water in turn to clean the excess Zn ions attached to the surface of the material, and freeze-dry it to obtain a Zn-doped basswood precursor; place the above-mentioned Zn-doped basswood precursor in a high-temperature tubular furnace for carbonization; in an Ar atmosphere, heat it to 800°C at a rate of 10°C / min, then to 1100°C at a rate of 5°C / min, and finally to 1300°C at a rate of 2°C / min, and maintain it for 4 hours. After cooling to room temperature, take it out to obtain a basswood-derived N-doped porous carbon material that has been pretreated by ball milling.

[0035] Scanning electron microscope photos Figure 2 As shown, it can be seen from a scanning electron microscope that the surface of the obtained carbon material is rough. The hard carbon material prepared as above is used as an active material for the battery negative electrode material in the preparation of sodium ion batteries.

[0036] The prepared electrode material was uniformly mixed with a conductive agent (Ketjen black) and a binder (sodium alginate) in a mass ratio of 7:2:1. Deionized water was used as the solvent and the mixture was ground into a uniform slurry using a mortar. The slurry was applied on a flat copper foil current collector and the surface of the slurry was made uniform and flat using a 100 μm coater. The slurry was then dried in an oven at 60°C for 30 minutes and then taken out and cut into circular electrodes with a diameter of 12 mm. The electrodes were placed in a vacuum oven at 80°C and dried for 12 hours. After the moisture in the electrodes was fully dried, the electrodes were taken out and quickly placed in a glove box for use.

[0037] Secondly, button cells were assembled in a glove box filled with argon: high-purity sodium sheets (99.97%) were used as counter electrodes, glass fiber films (GF / A) were used as diaphragms, the electrolyte was 1.0 mol / L lithium hexafluorophosphate (NaPF6), and the solvent was ethylene glycol dimethyl ether (DME). 2032 button cells were assembled and sealed with a sealing press (pressure of 50 MPa). The excess electrolyte on the outer shell was wiped off with a paper towel and then put into a No. 4 sealed bag. The cells were taken out of the glove box and placed in a 25°C thermostat for 12 hours to allow the electrolyte to fully infiltrate the electrode. The test results are shown in the figure. Figure 3 It can be seen that its reversible capacity is 391.4 mAh / g and the first-week coulombic efficiency is 87.89%.

[0038] Comparative Example 1

[0039] Take 800 mg of basswood that has not been pretreated by ball milling and put it into a high-temperature tubular furnace for carbonization. Under Ar atmosphere, the temperature is raised to 800°C at a rate of 10°C / min, then to 1100°C at a rate of 5°C / min, and finally to 1300°C at a rate of 2°C / min and maintained for 4 hours. After cooling to room temperature, take out and obtain a comparative carbon material.

[0040] The prepared electrode material was uniformly mixed with the conductive agent (Ketjen black) and the binder (sodium alginate) in a mass ratio of 7:2:1, deionized water was used as the solvent, and the slurry was ground into a uniform slurry with a mortar, which was applied on the flat copper foil current collector, and the slurry surface was evenly flattened using a 100μm coater, and then dried in an oven at 60°C for 30 minutes, and then taken out, cut into circular pole pieces with a diameter of 12mm, and placed in a vacuum oven at 80°C for 12 hours to fully dry the moisture therein. After that, the pole piece was taken out and quickly placed in a glove box for standby use.

[0041] Secondly, button cells were assembled in a glove box filled with argon: high-purity sodium sheets (99.97%) were used as counter electrodes, glass fiber films (GF / A) were used as diaphragms, the electrolyte was 1.0 mol / L lithium hexafluorophosphate (NaPF6), and the solvent was ethylene glycol dimethyl ether (DME). 2032 button cells were assembled and sealed with a sealing press (pressure of 50 MPa). The excess electrolyte on the outer shell was wiped off with a paper towel and then put into a No. 4 sealed bag. The cells were taken out of the glove box and placed in a 25°C thermostat for 12 hours to allow the electrolyte to fully infiltrate the electrode. The test results are shown in the figure. Figure 4 It can be seen that its reversible capacity is 251.6 mAh / g and the first-week coulombic efficiency is 87.94%.

[0042] Example 2

[0043] Take 500mg EDTAD and dissolve it in 80ml DMSO, and add 1.5ml pyridine to make EDTAD stably dispersed in the solution. Add 800mg of cellulose pretreated by ball milling to the above solution and ultrasonicate for 1h. Then put the mixture together in a 90-degree oven and keep it for 24h. Centrifuge the mixture, pour off the supernatant, and obtain EDTAD-modified basswood chips. Preparation of Zn-rich sawdust: Add EDTAD-modified basswood to 30ml 0.5MZnAc2 DMF solution, use a constant temperature heating magnetic stirrer to evenly disperse it, and heat it in a water bath at 50°C for 2 hours. Centrifuge the mixture to remove excess liquid, wash it once with acetone, once with alcohol, and twice with water in turn to clean the excess Zn ions attached to the surface of the material, and freeze-dry to obtain a Zn-doped basswood precursor. The above Zn-doped basswood precursor is placed in a high-temperature tubular furnace for carbonization. In an Ar atmosphere, the temperature was raised to 800°C at a rate of 10°C / min, then to 1100°C at a rate of 5°C / min, and finally to 1300°C at a rate of 2°C / min, and maintained for 4 hours. After cooling to room temperature, the ball-milled pre-treated basswood-derived N-doped porous carbon material was obtained. The test results showed that its reversible capacity was 361.9mAh / g and the first-week coulomb efficiency was 88.09%.

[0044] Example 3

[0045] Take 500mg EDTAD and dissolve it in 80ml DMA, and add 1.5ml pyridine to make EDTAD stably dispersed in the solution. Add 800mg chitin pre-treated by ball milling to the above solution and ultrasonicate for 1h. Then put the mixture together in a 90-degree oven and keep it for 24h. Centrifuge the mixture, pour off the supernatant, and obtain EDTAD-modified basswood chips. Preparation of Zn-rich sawdust: Add EDTAD-modified basswood to 30ml 0.5M ZnAc2 DMF solution, use a constant temperature heating magnetic stirrer to evenly disperse it, and heat it in a water bath at 50°C for 2 hours. Centrifuge the mixture to remove excess liquid, wash it once with acetone, once with alcohol, and twice with water in turn to clean the excess Zn ions attached to the surface of the material, and freeze-dry to obtain a Zn-doped basswood precursor. The above Zn-doped basswood precursor is placed in a high-temperature tube furnace for carbonization. In an Ar atmosphere, the temperature was raised to 800°C at a rate of 10°C / min, then to 1200°C at a rate of 2°C / min, and maintained for 4 hours. After cooling to room temperature, the ball-milled basswood-derived N-doped porous carbon material was obtained. The test results showed that its reversible capacity was 380.9mAh / g and the first-week coulomb efficiency was 87.25%.

[0046] Example 4

[0047] Take 500mg EDTAD and dissolve it in 80ml DMA, and add 1.5ml pyridine to make EDTAD stably dispersed in the solution. Add 800mg chitin pre-treated by ball milling to the above solution and ultrasonicate for 1h. Then put the mixture together in a 90-degree oven and keep it for 24h. Centrifuge the mixture, pour off the supernatant, and obtain EDTAD-modified basswood chips. Preparation of Zn-rich sawdust: Add EDTAD-modified basswood to 30ml 0.5M ZnAc2 DMF solution, use a constant temperature heating magnetic stirrer to evenly disperse it, and heat it in a water bath at 50°C for 2 hours. Centrifuge the mixture to remove excess liquid, wash it once with acetone, once with alcohol, and twice with water in turn to clean the excess Zn ions attached to the surface of the material, and freeze-dry to obtain a Zn-doped basswood precursor. The above Zn-doped basswood precursor is placed in a high-temperature tube furnace for carbonization. In a nitrogen atmosphere, the temperature was raised to 800°C at a rate of 10°C / min, then to 1200°C at a rate of 2°C / min, and maintained for 8 hours. After cooling to room temperature, the ball-milled basswood-derived N-doped porous carbon material was obtained. The test results showed that its reversible capacity was 361.5mAh / g and the first-week coulomb efficiency was 89.12%.

[0048] Example 5

[0049] Take 500mg EDTAD and dissolve it in 80ml DMA, and add 1.5ml 3,5-dichloropyridine to make EDTAD stably dispersed in the solution. Add 800mg chitin pre-treated by ball milling to the above solution and ultrasonicate for 1h. Then put the mixture together in a 90-degree oven and keep it for 24h. Centrifuge the mixture, pour off the supernatant, and obtain EDTAD-modified basswood chips. Preparation of Zn-rich sawdust: Add EDTAD-modified basswood to 30ml 0.5M ZnAc2 DMF solution, use a constant temperature heating magnetic stirrer to evenly disperse it, and heat it in a water bath at 50°C for 2 hours. Centrifuge the mixture to remove excess liquid, wash it once with acetone, once with alcohol, and twice with water in turn, wash off the excess Zn ions attached to the surface of the material, and freeze-dry to obtain a Zn-doped basswood precursor. The above Zn-doped basswood precursor is placed in a high-temperature tube furnace for carbonization. In a nitrogen atmosphere, the temperature was raised to 800°C at a rate of 10°C / min, then to 1200°C at a rate of 2°C / min, and maintained for 2 hours. After cooling to room temperature, the ball-milled basswood-derived N-doped porous carbon material was obtained. The test results showed that its reversible capacity was 370.1mAh / g and the first-week coulomb efficiency was 87.66%.

[0050] Example 6

[0051] Take 500mg EDTAD and dissolve it in 80ml HMPT, and add 1.5ml aminopyridine to make EDTAD stably dispersed in the solution. Add 800mg chitin pre-treated by ball milling to the above solution and ultrasonicate for 1h. Then put the mixture together in a 90-degree oven and keep it for 24h. Centrifuge the mixture, pour off the supernatant, and obtain EDTAD-modified basswood chips. Preparation of Zn-rich sawdust: Add EDTAD-modified basswood to 30ml 0.5M ZnAc2 DMF solution, use a constant temperature heating magnetic stirrer to evenly disperse it, and heat it in a water bath at 50°C for 2 hours. Centrifuge the mixture to remove excess liquid, wash it once with acetone, once with alcohol, and twice with water in turn, wash off the excess Zn ions attached to the surface of the material, and freeze-dry to obtain a Zn-doped basswood precursor. The above Zn-doped basswood precursor is placed in a high-temperature tube furnace for carbonization. In a nitrogen atmosphere, the temperature was raised to 800°C at a rate of 10°C / min, then to 1200°C at a rate of 2°C / min, and maintained for 2 hours. After cooling to room temperature, the ball-milled basswood-derived N-doped porous carbon material was obtained. The test results showed that its reversible capacity was 365.4mAh / g and the first-week coulomb efficiency was 88.44%.

[0052] The present invention introduces carboxyl groups into wood cellulose through the combination of EDTAD, thereby enhancing the coordination binding between cellulose macromolecules and Zn metal ions. While successfully fixing Zn ions in the structure of basswood fibers, nitrogen doping is introduced to obtain a hard carbon precursor containing evenly dispersed Zn ions. The Zn species is then evaporated by high-temperature pyrolysis, leaving a rich pore structure, and a nitrogen-doped porous hard carbon material with rich defect sites and a large interlayer spacing is prepared. The reversible capacity of the sodium ion battery negative electrode material of the present invention is greater than 360.0mAh / g, and the first-week coulomb efficiency is greater than 85.0%. Compared with similar inventions, it has simple steps and low costs, and has considerable industrial advantages.

[0053] In the description of this article, it should be noted that relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a negative electrode material for a sodium ion battery, characterized in that: The following steps are involved: S1: amidation reaction, in an organic solvent, the biomass material is subjected to an amidation reaction with a catalyst to obtain an EDTA-modified biomass material; S2: mixing and stirring, adding a pyridine compound after the EDTA-modified biomass material has completed the reaction, stirring evenly, ultrasonicating, placing in an oven for baking, and then centrifuging; S3: preparing a precursor, adding the modified biomass material to a zinc salt solution, uniformly dispersing it using a constant temperature heating magnetic stirrer, heating it in a water bath, and then freeze-drying it to obtain a zinc ion-doped biomass precursor; S4: Carbonization treatment, carbonizing the biomass material under the protection of an inert gas to obtain the corresponding nitrogen-doped zinc pore-forming sodium ion battery negative electrode material.

2. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The biomass material in S1 is one of basswood, cellulose, lignin and chitin.

3. The method for preparing a negative electrode material for a sodium ion battery according to claim 2, characterized in that: The organic solvent in S1 is one of DMF, DMSO, DMA and HMPT.

4. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The water bath heating temperature in S3 is between 50 degrees and 90 degrees, and the carbonization treatment time in S4 is between 1 hour and 5 hours.

5. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The pyridine compound in S2 is one of pyridine, 2-hydroxymethylpyridine, 3,5-dichloropyridine and aminopyridine.

6. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The inert gas in S4 is one of argon, nitrogen, and hydrogen argon (5% hydrogen).

7. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The carbonization treatment temperature in S4 is between 500 and 1400 degrees, and the carbonization treatment time is between 2 and 8 hours.

8. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The catalyst in S1 includes one or more of dipyridine, 1,0-phenanthroline, ethylenediaminetetraacetic acid, ethylenediamine, nitrosodiacetic acid, oxalate, dithizone, 8-hydroxyquinoline, o-phenanthroline (C12H8N2), and potassium sodium tartrate.

9. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The zinc salt in S3 is one or more of ZnCl2, ZnSO4, Zn(NO3)2, Zn(ClO4)2, and Zn(BF4)2.

Citation Information

Patent Citations

  • A method for preparing a novel sodium-ion battery negative-electrode material

    CN109553081A

  • Hard carbon material and preparation method thereof, electrochemical device and electronic device

    CN115332538A

  • Sodium-ion battery hard carbon negative electrode material, preparation method thereof and sodium-ion battery

    CN115924912A

  • Preparation method of high-rate and low-temperature-resistant hard carbon negative electrode material and application of high-rate and low-temperature-resistant hard carbon negative electrode material in sodium-ion battery

    CN116161643A

  • Preparation method of high-capacity asphalt-based hard carbon sodium ion battery negative electrode material

    CN116969442A