Polyurethane damping vibration attenuation material as well as preparation method and application thereof

By introducing specific small molecule alcohols, vegetable oil polyols and isophorone diisocyanate into polyurethane materials, the molecular structure is improved, and the problem of low performance of polyurethane elastomers is solved, and higher damping and vibration damping performance and service life are achieved.

CN119081062APending Publication Date: 2024-12-06GUANGZHOU POWER SUPPLY BUREAU GUANGDONG POWER GRID CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411422916.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing polyurethane elastomers have low performance and are difficult to be used as damping and vibration-absorbing materials for cable trench/cable manhole cover plates. They cannot effectively withstand external environment and mechanical impacts, resulting in a shortened service life.

Method used

The raw materials of polyurethane damping and vibration-absorbing materials with specific ratios include small molecule alcohol dipropylene glycol, vegetable oil polyol polyadipate castor oil ester polyol and isophorone diisocyanate. By adjusting the molecular structure and proportion, the flexibility of the material is improved. Hardness and compatibility form a more uniform microphase separation structure to enhance damping performance.

Benefits of technology

It improves the loss factor of polyurethane materials, improves damping and vibration damping performance, meets the requirements of cable trench/cable manhole cover plates, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081062A_ABST
    Figure CN119081062A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of damping vibration attenuation materials, and particularly relates to a polyurethane damping vibration attenuation material and a preparation method and application thereof. According to the polyurethane damping vibration attenuation material provided by the invention, vegetable oil polyols such as poly (castor oil adipate) polyols, small molecular alcohols such as dipropylene glycol DPG and isophorone diisocyanate are introduced into the raw materials, the loss factor of the polyurethane material is increased to 0.42-0.57, and the polyurethane material also has the hardness of 50-70A, so that the performance of the polyurethane material is improved, and the service life of the polyurethane material is prolonged. The technical problems that in the prior art, polyurethane elastomers are low in performance and difficult to serve as damping vibration attenuation materials for cable trench / cable well cover plates are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of damping and vibration reduction materials, and in particular relates to a polyurethane damping and vibration reduction material and a preparation method and application thereof. Background Art

[0002] During the construction of cable trenches and cable wells, covers are used to cover the cable trenches / cable wells. However, when the construction quality of civil engineering pressure top construction is poor, defects such as inaccurate elevation of the covers after installation, excessive gaps between the plates leading to the entry of foreign objects or small animals, abnormal noises and unstable displacements when people walk or vehicles pass by are caused. During on-site construction, small stones, wooden boards, cable rubbers, glass glue and other materials are used to adjust the elevation of the covers and fill the gaps between the plates to make up for the defects of civil engineering pressure top construction. However, stones, wooden boards, cable rubbers, glass glue and other materials are not damping and vibration reduction materials and cannot withstand long-term wind and sun exposure and long-term impact from external forces such as people and vehicles, which affects the safe operation of power cables. Therefore, it is necessary to use damping and vibration reduction materials to transform the cable trench / cable well covers to reduce the impact and wear effect between the cable trench / cable well covers and the supporting base, so as to achieve the purpose of adjusting the cover height and eliminating noise.

[0003] Polyurethane elastomer (PU elastomer) is an important type of damping and vibration reduction material with the advantages of excellent elasticity, friction resistance, high strength and oil resistance. However, the damping and vibration reduction material used for cable trenches / cable well covers needs to be exposed to the outdoor environment and will be affected by factors such as hot air, ozone, ultraviolet rays, people walking, and vehicles running over, which can easily cause damage to the polyurethane molecular chain structure and internal structure, causing excessive loss of its original strength and impact and vibration reduction performance, and shortening its service life. Therefore, the performance of ordinary polyurethane elastomers is currently low, and it is difficult to directly use them as damping and vibration reduction materials for cable trenches / cable well covers.

[0004] The molecular chain of polyurethane includes soft segments (polyether, polyester diol, etc.) and hard segments (diisocyanate). The flexibility of the soft segment gives polyurethane good elasticity, and the rigidity of the hard segment forms a crystalline region. The soft segment and the hard segment are thermodynamically incompatible systems with polarity differences, which can cause microphase separation. By adjusting the ratio, structure, molecular distribution, etc. of the soft and hard segments, the mechanical strength, wear resistance, resilience and other properties of the polyurethane material can be improved to obtain a damping and vibration reduction material with a higher loss factor. Summary of the invention

[0005] In view of this, the present application provides a polyurethane damping and vibration reduction material and a preparation method and application thereof, which are used to solve the technical problem in the prior art that polyurethane elastomers have low performance and are difficult to be used as damping and vibration reduction materials for cable trenches / cable well covers.

[0006] In a first aspect, the present application provides a polyurethane damping and vibration reduction material, the raw materials of which include: a component A raw material and a component B raw material;

[0007] The raw materials of component A include: small molecule alcohol, vegetable oil polyol, polyether polyol, catalyst and polymer material additive;

[0008] The raw materials of component B include: isophorone diisocyanate, MDI, polyether polyol and polymer material additives.

[0009] Preferably, in the raw material of component A, the small molecule alcohol is selected from dipropylene glycol;

[0010] The vegetable oil polyol is selected from castor oil adipate polyol;

[0011] The polyether polyol is selected from polyether polyol MN-3050D;

[0012] The catalyst is selected from at least one of an organic bismuth catalyst BiCAT®8118, lead isooctanoate, and zinc isooctanoate;

[0013] The polymer material additive is selected from plasticizers and anti-aging agents.

[0014] Preferably, in the raw material of component B, the polyether polyol is selected from polyether polyol PPG-2000;

[0015] The polymer material additive is selected from plasticizers.

[0016] Preferably, the plasticizer is selected from at least one of dioctyl terephthalate, 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, acetyl tributyl citrate, and 1,2-cyclohexanedicarboxylic acid di(isononyl) ester;

[0017] The anti-aging agent is selected from at least one of UV-531, UV-02, UV-01, UV-1010, and UV-1076.

[0018] Preferably, calculated by weight, the raw materials of component A include: 10 to 17 parts by weight of small molecule alcohols, 20 to 30 parts by weight of vegetable oil polyols, 35 to 55.2 parts by weight of polyether polyols, 0.30 to 1 parts by weight of catalysts, and 5.5 to 22 parts by weight of polymer material additives.

[0019] Preferably, calculated in parts by mass, the raw materials of component B include: 5.5-21.6 parts by mass of isophorone diisocyanate, 33.7-65.2 parts by mass of MDI, 15.1-37.3 parts by mass of polyether polyol and 8-12 parts by mass of polymer material additives.

[0020] The second aspect of the present application provides a method for preparing a polyurethane damping and vibration reduction material, which can be used to prepare the polyurethane damping and vibration reduction material described in the first aspect. The preparation method comprises the steps of:

[0021] Step S1, mixing small molecule alcohol, vegetable oil polyol, polyether polyol and plasticizer in polymer material additive and dehydrating to obtain a dehydrated mixture;

[0022] Step S2, adding the catalyst and the anti-aging agent in the polymer material additive to the dehydrated mixture and mixing to obtain component A;

[0023] Step S3, subjecting isophorone diisocyanate, MDI, polyether polyol and polymer material additive to a prepolymerization reaction to obtain component B;

[0024] Step S4, mixing component A and component B and polymerizing them at room temperature to obtain a polyurethane damping and vibration reduction material.

[0025] Preferably, in step S1, the dehydration temperature is 95-110° C. and the pressure is -0.095 MPa.

[0026] Preferably, in step S2, the temperature during mixing is 50-60°C.

[0027] Preferably, in step S3, the prepolymerization reaction is carried out at a temperature of 80-100° C. and for a time of 3-12 hours.

[0028] Preferably, in step S4, the temperature during mixing is 30-35°C.

[0029] The third aspect of the present application provides the use of the polyurethane damping and vibration reduction material described in the first aspect in the preparation of damping and vibration reduction pads for cable trenches or cable well covers.

[0030] In summary, the present application provides a polyurethane damping vibration reduction material and a preparation method and application. The small molecule alcohol dipropylene glycol introduced into the raw material of a polyurethane damping vibration reduction material provided by the present application can improve the flexibility of the molecular chain of polyurethane, have a lower glass transition temperature, and reduce the physical crosslinking degree of polyurethane; and the introduction of vegetable oil polyol polyadipate castor oil ester polyol improves the damping performance of polyurethane by utilizing its molecular chain length and flexibility; at the same time, isophorone diisocyanate has a lower crystallinity, and the compatibility between the hard segment and the soft segment is better, which is conducive to forming a more uniform microphase separation structure. This structure helps to more effectively transfer and dissipate energy between the hard segment and the soft segment when subjected to external force, thereby improving the damping coefficient; thus, a polyurethane damping vibration reduction material with a large loss factor, hardness and stability is obtained, which can solve the technical problem that the polyurethane elastomer in the prior art has low performance and is difficult to be used as a damping vibration reduction material for cable trenches / cable well covers. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 A schematic flow chart of a method for preparing a polyurethane damping and vibration reduction material provided in an embodiment of the present application. DETAILED DESCRIPTION

[0033] The present application provides a polyurethane damping and vibration reduction material and a preparation method and application thereof, which are used to solve the technical problem in the prior art that polyurethane elastomers have low performance and are difficult to be used as damping and vibration reduction materials for cable trenches / cable well covers.

[0034] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0035] In view of the defect that common polyurethane materials currently have low performance and are difficult to be used as damping and vibration reduction materials for cable trenches / cable well covers, the present application provides a polyurethane damping and vibration reduction material. The raw material composition of the polyurethane damping and vibration reduction material provided by the present application includes component A raw materials such as small molecule alcohols such as dipropylene glycol, vegetable oil polyols such as polycastor adipate polyols, polyether polyols, catalysts and polymer material additives, and component B raw materials such as isophorone diisocyanate, MDI, polyether polyols and polymer material additives; the introduction of small molecule alcohol dipropylene glycol (DPG) in the raw materials can give the polyurethane molecular chain better flexibility, lower glass transition temperature, and reduce the physical crosslinking degree of the polyurethane, while the introduction of vegetable oil polyol polycastor adipate polyol improves the damping performance of the polyurethane by utilizing its molecular chain length and flexibility, and isophorone diisocyanate has a lower degree of crystallinity, better compatibility between the hard segment and the soft segment, and is conducive to forming a more uniform microphase separation structure. This structure helps to more effectively transfer and dissipate energy between the hard segment and the soft segment when subjected to external force, thereby improving the damping coefficient; therefore, the present application can improve the damping and vibration reduction performance of polyurethane by adding specific small molecule alcohols such as dipropylene glycol, vegetable oil polyols such as polycastor adipate polyols, and isophorone diisocyanate to the polyurethane raw materials. Experimental data show that the addition of small molecule alcohols such as dipropylene glycol, vegetable oil polyols such as polycastor adipate polyols, and isophorone diisocyanate can increase the loss factor of the polyurethane material to 0.42~0.57. The larger the loss factor, the better the damping and vibration reduction performance of the polyurethane material. At the same time, the polyurethane material also has good mechanical properties (hardness) and good stability, so that it can be used as a damping and vibration reduction material for cable trenches / cable well covers, overcoming the defect that the current polyurethane elastomer has low performance and is difficult to use as a damping and vibration reduction material for cable trenches / cable well covers.

[0036] Preferably, the small molecule alcohol of the raw material of component A in the polyurethane damping and vibration reduction material provided in the present application can be selected from dipropylene glycol (DPG) produced by Dow, with a number average molecular weight of 134 and a functionality of 2; and the polyether polyol can be selected from polyether polyol MN-3050D produced by Bluestar Dongda, with a number average molecular weight of 2000 and a functionality of 2; the polyether polyol of the raw material of component B is selected from polyether polyol MN-3050D produced by Bluestar Dongda, with a number average molecular weight of 3000 and a functionality of 3, and isophorone diisocyanate is selected from isophorone diisocyanate IPDI produced by Covestro.

[0037] The polyurethane damping and vibration reduction material provided in the present application will be specifically described below in combination with embodiments and experimental examples.

[0038] Example 1

[0039] Example 1 of the present application provides a method for preparing a polyurethane damping and vibration reduction material, which comprises the steps of preparing component A, prepolymerizing component B, and polymerizing.

[0040] The steps of preparing component A include:

[0041] 100 g of small molecule alcohol dipropylene glycol DPG, 572 g of polyether polyol MN-3050D, 270 g of polyadipate castor oil polyol, and 50 g of plasticizer dioctyl terephthalate were mixed, and dehydrated at 100° C. and a pressure of -0.095 MPa until the water content was less than 0.05% to obtain a dehydrated mixture;

[0042] The dehydrated mixture was then cooled to 55±5°C, and 5 g of an anti-aging agent UV-1076 and 3 g of a catalyst BiCAT®8118 were added in sequence. After stirring and melting, a polymer component A was obtained.

[0043] The step of prepolymerizing component B includes: prepolymerizing 178g of polyether polyol PPG-2000, 216g of isophorone diisocyanate IPDI, 505g of MDI, and 101g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0044] The steps of the polymerization reaction include: mixing 500g of component A and 275g of component B at a mass ratio of 100:55 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane damping and vibration reduction material; at the same time, it can also be poured into a vibration reduction pad mold at 35°C for 15 minutes to obtain a damping and vibration reduction pad suitable for a cable trench or a cable well.

[0045] Example 2

[0046] Example 2 of the present application provides a method for preparing a polyurethane damping and vibration reduction material, which comprises the steps of preparing component A, prepolymerizing component B, and polymerizing.

[0047] The steps of preparing component A include:

[0048] 130 g of a small molecule alcohol dipropylene glycol DPG, 510 g of a polyether polyol MN-3050D, 200 g of a polyadipate castor oil ester polyol, and 130 g of a plasticizer dioctyl terephthalate were mixed, and dehydrated at 100° C. and a pressure of -0.095 MPa until the water content was less than 0.05% to obtain a dehydrated mixture;

[0049] The dehydrated mixture was then cooled to 55±5°C, and 20 g of an anti-aging agent UV-1076 and 10 g of a catalyst BiCAT®8118 were added in sequence. After stirring and melting, a polymer component A was obtained.

[0050] The step of preparing component B by prepolymerization includes: prepolymerizing 373g of polyether polyol PPG-2000, 158g of isophorone diisocyanate IPDI, 369g of MDI, and 100g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0051] The steps of the polymerization reaction include: mixing 500g of component A and 400g of component B at a mass ratio of 100:80 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane damping and vibration reduction material; and also pouring into a vibration reduction pad mold at 35°C for 15 minutes to obtain a damping and vibration reduction pad suitable for a cable trench or a cable well.

[0052] Example 3

[0053] Example 3 of the present application provides a method for preparing a polyurethane damping and vibration reduction material, which comprises the steps of preparing component A, prepolymerizing component B, and polymerizing.

[0054] The steps of preparing component A include:

[0055] 100 g of a small molecule alcohol dipropylene glycol DPG, 372 g of a polyether polyol MN-3050D, 300 g of a polyadipate castor oil ester polyol, and 200 g of a plasticizer dioctyl terephthalate were mixed, and dehydrated at 100° C. and a pressure of -0.095 MPa until the water content was less than 0.05% to obtain a dehydrated mixture;

[0056] The dehydrated mixture was then cooled to 55±5°C, and 5 g of an anti-aging agent UV-1076 and 3 g of a catalyst BiCAT®8118 were added in sequence. After stirring and melting, a polymer component A was obtained.

[0057] The step of prepolymerizing component B includes: prepolymerizing 171g of polyether polyol PPG-2000, 75g of isophorone diisocyanate IPDI, 674g of MDI, and 80g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0058] The steps of the polymerization reaction include: mixing 500g of component A and 300g of component B at a mass ratio of 100:60 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane damping and vibration reduction material; and also pouring into a vibration reduction pad mold at 35°C for 15 minutes to obtain a damping and vibration reduction pad adapted to a cable trench or a cable well.

[0059] Example 4

[0060] Example 4 of the present application provides a method for preparing a polyurethane damping and vibration reduction material, which includes the steps of preparing component A, prepolymerizing component B, and polymerizing.

[0061] The steps of preparing component A include:

[0062] Dehydrate 170 g of small molecule alcohol dipropylene glycol DPG, 400 g of polyether polyol MN-3050D, 300 g of polycastor oil adipate polyol, and 100 g of plasticizer acetyl tributyl citrate at 105° C. and a pressure of -0.095 MPa until the water content is less than 0.05% to obtain a dehydrated mixture;

[0063] The dehydrated mixture was then cooled to 55±5°C, and 10 g of an anti-aging agent UV-531, 10 g of an anti-aging agent UV-02, and 10 g of a catalyst BiCAT®8118 were added in sequence, and the mixture was stirred and melted to obtain a polymer component A.

[0064] The step of preparing component B by prepolymerization includes: prepolymerizing 250g of polyether polyol PPG-2000, 158g of isophorone diisocyanate IPDI, 492g of MDI, and 100g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0065] The steps of the polymerization reaction include: mixing 500g of component A and 450g of component B at a mass ratio of 100:90 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane damping and vibration reduction material; at the same time, it can also be poured into a vibration reduction pad mold at 35°C for 15 minutes to obtain a damping and vibration reduction pad suitable for a cable trench or a cable well.

[0066] Example 5

[0067] Example 5 of the present application provides a method for preparing a polyurethane damping and vibration reduction material, which comprises the steps of preparing component A, prepolymerizing component B, and polymerizing.

[0068] The steps of preparing component A include:

[0069] 110 g of a small molecule alcohol dipropylene glycol DPG, 482 g of a polyether polyol MN-3050D, 250 g of a polyadipate castor oil ester polyol, and 150 g of a plasticizer dioctyl terephthalate were mixed, and dehydrated at 100° C. and a pressure of -0.095 MPa until the water content was less than 0.05% to obtain a dehydrated mixture;

[0070] The dehydrated mixture was then cooled to 55±5°C, and 5 g of an anti-aging agent UV-1076, 1 g of a catalyst BiCAT®8118, and 1 g of a catalyst zinc isooctanoate were added in sequence, and the mixture was stirred and melted to obtain a polymer component A.

[0071] The step of prepolymerizing component B includes: prepolymerizing 203g of polyether polyol PPG-2000, 70g of isophorone diisocyanate IPDI, 607g of MDI, and 120g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0072] The steps of the polymerization reaction include: mixing 500g of component A and 300g of component B at a mass ratio of 100:60 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane damping and vibration reduction material; and also pouring into a vibration reduction pad mold at 35°C for 15 minutes to obtain a damping and vibration reduction pad adapted to a cable trench or a cable well.

[0073] Example 6

[0074] Example 6 of the present application provides a method for preparing a polyurethane damping and vibration reduction material, which includes the steps of preparing component A, prepolymerizing component B, and polymerizing.

[0075] The steps of preparing component A include:

[0076] 170 g of small molecule alcohol dipropylene glycol DPG, 422 g of polyether polyol MN-3050D, 300 g of polycastor oil adipate polyol, and 100 g of plasticizer dioctyl terephthalate were mixed, and dehydrated at 100° C. and a pressure of -0.095 MPa until the water content was less than 0.05% to obtain a dehydrated mixture;

[0077] The dehydrated mixture was then cooled to 55±5°C, and 5 g of an anti-aging agent UV-1076 and 3 g of a catalyst BiCAT®8118 were added in sequence. After stirring and melting, a polymer component A was obtained.

[0078] The step of preparing component B by prepolymerization includes: prepolymerizing 333g of polyether polyol PPG-2000, 142g of isophorone diisocyanate IPDI, 425g of MDI, and 100g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0079] The steps of the polymerization reaction include: mixing 500g of component A and 300g of component B at a mass ratio of 100:60 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane damping and vibration reduction material; and also pouring into a vibration reduction pad mold at 35°C for 15 minutes to obtain a damping and vibration reduction pad adapted to a cable trench or a cable well.

[0080] Example 7

[0081] Example 7 of the present application provides a method for preparing a polyurethane material. As a first comparative example, the preparation method includes: a step of preparing component A, a step of prepolymerizing component B, and a step of polymerization reaction.

[0082] The steps of preparing component A include:

[0083] 120g of small molecule alcohol dipropylene glycol DPG, 372g of polyether polyol MN-3050D, 300g of polyadipate castor oil ester polyol, 100g of plasticizer dioctyl terephthalate and 100g of flaky mica are mixed, and dehydrated at 100°C and a pressure of -0.095MPa until the water content is less than 0.05% to obtain a dehydrated mixture;

[0084] The dehydrated mixture was then cooled to 55±5°C, and 5 g of an anti-aging agent UV-1076 and 3 g of a catalyst BiCAT®8118 were added in sequence. After stirring and melting, a polymer component A was obtained.

[0085] The step of preparing component B by prepolymerization includes: prepolymerizing 151g of polyether polyol PPG-2000, 75g of isophorone diisocyanate IPDI, 674g of MDI, and 100g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0086] The polymerization reaction step includes: mixing 500g of component A and 300g of component B at a mass ratio of 100:60 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane material.

[0087] Example 8

[0088] Example 8 of the present application provides a method for preparing a polyurethane material. As a second comparative example, the preparation method includes: a step of preparing component A, a step of prepolymerizing component B, and a step of polymerization reaction.

[0089] The steps of preparing component A include:

[0090] 450 g of polyether polyol MN-500 (number average molecular weight of 500, functionality of 3, produced by Bluestar Dongda), 342 g of polyether polyol MN-3030D, and 200 g of plasticizer dioctyl terephthalate were mixed, and dehydrated at 100° C. and a pressure of -0.095 MPa until the water content was less than 0.05% to obtain a dehydrated mixture;

[0091] The dehydrated mixture was then cooled to 55±5°C, and 5 g of an anti-aging agent UV-1076 and 3 g of a catalyst BiCAT®8118 were added in sequence. After stirring and melting, a polymer component A was obtained.

[0092] The step of preparing component B by prepolymerization includes: prepolymerizing 226g of polyether polyol PPG-2000, 674g of MDI, and 100g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0093] The polymerization reaction step includes: mixing 500g of component A and 300g of component B at a mass ratio of 100:60 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane material.

[0094] Example 9

[0095] Example 9 of the present application provides a method for preparing a polyurethane material. As a third comparative example, the preparation method includes: a step of preparing component A, a step of prepolymerizing component B, and a step of polymerization reaction.

[0096] The steps of preparing component A include:

[0097] 160 g of small molecule alcohol dipropylene glycol DPG, 632 g of polyether polyol MN-3050D, and 200 g of plasticizer dioctyl terephthalate were mixed, and dehydrated at 100° C. and a pressure of -0.095 MPa until the water content was less than 0.05% to obtain a dehydrated mixture;

[0098] The dehydrated mixture was then cooled to 55±5°C, and 5 g of an anti-aging agent UV-1076 and 3 g of a catalyst BiCAT®8118 were added in sequence. After stirring and melting, a polymer component A was obtained.

[0099] The step of preparing component B by prepolymerization includes: prepolymerizing 151g of polyether polyol PPG-2000, 75g of isophorone diisocyanate IPDI, 674g of MDI, and 100g of plasticizer dioctyl terephthalate at 90°C for 8h to obtain a prepolymer component B with an isocyanate mass content of 22%.

[0100] The polymerization reaction step includes: mixing 500g of component A and 300g of component B at a mass ratio of 100:60 at 35°C, placing at room temperature for 10 hours for polymerization reaction, and obtaining a polyurethane material.

[0101] Experimental Example 1

[0102] Experimental Example 1 of the present application performs performance tests on the polyurethane damping and vibration reduction materials provided in Examples 1-6 and the polyurethane materials provided in Examples 7-9. The performance tests include hardness test, loss factor test and stability test. The hardness test process is carried out in accordance with the national standard GB / T 531.1-2008, the loss factor test process is carried out in accordance with GB / T18258-2000, and the stability test is to observe whether there is precipitation within 60 days. The test results are shown in Table 1.

[0103] Table 1: Hardness, loss factor and stability test results

[0104]

[0105] As can be seen from Table 1, the polyurethane material provided in Example 8 as the second comparative experiment does not have vegetable oil polyols such as polycastorin adipate polyols, nor does it have small molecule alcohols such as dipropylene glycol DPG, in its component A raw material, and at the same time, does not have isophorone diisocyanate in its component B raw material, which makes the loss factor of the polyurethane material small, which is only 0.17. The smaller the loss factor, the poorer the damping and vibration reduction performance. As for the polyurethane material provided in Example 9 as the third comparative experiment, the vegetable oil polyols such as polycastorin adipate polyols were not added to its component A raw material, which makes the loss factor of the polyurethane material 0.31, which has It has certain damping and vibration reduction performance; the polyurethane damping and vibration reduction material provided in Examples 1-6 of the present application introduces vegetable oil polyols such as polycastor oil adipate polyol, small molecule alcohols such as dipropylene glycol DPG and isophorone diisocyanate and other ingredients into the raw materials, and the loss factor of the polyurethane material is increased to 0.42~0.57. The larger the loss factor, the better the damping and vibration reduction performance of the polyurethane material, thereby meeting the performance requirements of damping and vibration reduction materials for cable trenches / cable well covers. The polyurethane material provided in Example 6 of the first comparative experiment is doped with mica sheets, which have poor compatibility with polyurethane and are difficult to meet the requirements for long-term use of damping and vibration reduction materials.

[0106] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A polyurethane damping and vibration reduction material, characterized in that: The raw materials include: component A raw materials and component B raw materials; The raw materials of component A include: small molecule alcohol, vegetable oil polyol, polyether polyol, catalyst and polymer material additive; The raw materials of component B include: isophorone diisocyanate, MDI, polyether polyol and polymer material additives.

2. The polyurethane damping and vibration reduction material according to claim 1, characterized in that: In the raw material of component A, the small molecule alcohol is selected from dipropylene glycol; The vegetable oil polyol is selected from castor oil adipate polyol; The polyether polyol is selected from polyether polyol MN-3050D; The catalyst is selected from at least one of an organic bismuth catalyst BiCAT®8118, lead isooctanoate, and zinc isooctanoate; The polymer material additive is selected from plasticizers and anti-aging agents.

3. The polyurethane damping and vibration reduction material according to claim 1, characterized in that: In the raw materials of component B, the polyether polyol is selected from polyether polyol PPG-2000; The polymer material additive is selected from plasticizers.

4. The polyurethane damping and vibration reduction material according to claim 1, characterized in that: Calculated by weight, the raw materials of component A include: 10-17 weight parts of small molecule alcohol, 20-30 weight parts of vegetable oil polyol, 35-55.2 weight parts of polyether polyol, 0.30-1 weight part of catalyst and 5.5-22 weight parts of polymer material additive; The raw materials of component B include: 5.5-21.6 parts by mass of isophorone diisocyanate, 33.7-65.2 parts by mass of MDI, 15.1-37.3 parts by mass of polyether polyol and 8-12 parts by mass of polymer material additives.

5. A polyurethane damping and vibration reduction material according to claim 2 or 3, characterized in that: The plasticizer is selected from at least one of dioctyl terephthalate, 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, acetyl tributyl citrate, and 1,2-cyclohexanedicarboxylic acid di(isononyl) ester; The anti-aging agent is selected from at least one of UV-531, UV-02, UV-01, UV-1010, and UV-1076.

6. The method for preparing a polyurethane damping and vibration reduction material according to any one of claims 1 to 5, characterized in that: Includes steps: Step S1, mixing small molecule alcohol, vegetable oil polyol, polyether polyol and plasticizer in polymer material additive and dehydrating to obtain a dehydrated mixture; Step S2, adding the catalyst and the anti-aging agent in the polymer material additive to the dehydrated mixture and mixing to obtain component A; Step S3, subjecting isophorone diisocyanate, MDI, polyether polyol and polymer material additive to a prepolymerization reaction to obtain component B; Step S4, mixing component A and component B and polymerizing them at room temperature to obtain a polyurethane damping and vibration reduction material.

7. The method for preparing a polyurethane damping and vibration reduction material according to claim 6, characterized in that: In step S1, the dehydration temperature is 95-110°C and the pressure is -0.095MPa.

8. The method for preparing a polyurethane damping and vibration reduction material according to claim 6, characterized in that: In step S2, the temperature during the mixing is 50-60°C; in step S4, the temperature during the mixing is 30-35°C.

9. The method for preparing a polyurethane damping and vibration reduction material according to claim 6, characterized in that: In step S3, the prepolymerization reaction is carried out at a temperature of 80-100° C. and for a time of 3-12 hours.

10. Use of a polyurethane damping and vibration reduction material according to any one of claims 1 to 5 in preparing a damping and vibration reduction pad for a cable trench or a cable well cover.

Citation Information

Cited By

  • High-adhesion high-supporting-performance polyurethane shoe glue and preparation method thereof

    CN122427640A