Gelatin embolism particles as well as preparation method and application thereof

By refining the preparation process of gelatin embolic particles through controlled parameters, the method achieves rapid degradation and enhanced structural stability, addressing safety concerns and improving clinical applicability.

CN119185631AActive Publication Date: 2024-12-27BEIJING GUANHE MEDICAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411092267.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-27
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Conventional gelatin embolic particles have long degradation times and residual cross-linking agents, posing potential harm to patients and requiring a more rapid degradation and safer alternative.

Method used

A method involving dissolution, foaming, freeze-drying, thermal cross-linking, crushing, and sterilization of low-endotoxin, high-purity gelatin to produce embolic particles with controlled parameters, ensuring rapid degradation and improved structural stability.

Benefits of technology

The prepared gelatin embolic particles are completely degradable, exhibit high porosity and water absorption, and have excellent suspension and catheter passability, facilitating their use in medical procedures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986910180000071
    Figure BDA0004986910180000071
  • Figure BDA0004986910180000081
    Figure BDA0004986910180000081
  • Figure BDA0004986910180000082
    Figure BDA0004986910180000082
Patent Text Reader

Abstract

The invention relates to the technical field of biological medicine, and particularly discloses gelatin embolism particles as well as a preparation method and application thereof. The preparation method of the gelatin embolism particles comprises the following steps: by taking gelatin as a raw material, dissolving, foaming, freeze-drying, thermally crosslinking, crushing, screening and sterilizing; in the foaming step, nitrogen is introduced below the liquid level of 20-100 g / L gelatin aqueous solution, foaming is performed under the rotating speed condition of 2500-3500 rpm until no obvious liquid exists at the bottom of a container, and the foaming volume is 1-10 times of the original liquid volume; the thermal crosslinking step comprises the following steps: carrying out vacuum drying on the gelatin sponge body under the condition of 60-90 DEG C for 20-30 minutes, and then carrying out vacuum drying on the gelatin sponge body under the condition of 110-130 DEG C for 10-36 hours. The gelatin embolism particles obtained by the preparation method provided by the invention are high in porosity, proper in water absorption and good in in-vitro degradability; the suspension performance and the conduit passing performance are excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of biomedicine, and specifically to a gelatin embolic particle and a preparation method and application thereof. Background Art

[0002] With the mature preparation of low-endotoxin gelatin, medical devices prepared with gelatin have been widely recognized and applied. Iodized oil and gelatin sponge particles are often used in conventional transcatheter arterial chemoembolization (TACE). The gelatin particles are cross-linked with aldehydes and freeze-dried. The degradation time is relatively long, usually 90 days. In addition, there are residual cross-linking agents after degradation, and the residual cross-linking agents can also bring potential harm to patients.

[0003] Therefore, there is an urgent need to develop a gelatin embolic product that is degradable in a short period of time and can be completely degraded. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a gelatin embolic particle and a preparation method and application thereof.

[0005] The present application provides a method for preparing gelatin embolic particles, which specifically comprises the following steps in sequence: Using gelatin as raw material, it is dissolved, foamed, freeze-dried, crushed, thermally cross-linked, sieved and sterilized; The specific steps of foaming are: introducing nitrogen gas below the liquid surface of a 20-80 g / L gelatin aqueous solution, foaming at a rotation speed of 2500-3500 rpm until there is no obvious liquid at the bottom of the container and the foaming volume is 1-10 times the original liquid volume, to obtain a gelatin foam; The specific steps of the thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying under vacuum drying conditions at 60-90° C. for 20-30 minutes, and then placing it under vacuum drying conditions at 110-130° C. for 10-36 hours.

[0006] The present application utilizes the above-mentioned technical scheme, improves the preparation process, selects low-endotoxin, high-purity gelatin, and obtains related products through dissolution, foaming, freeze-drying, thermal cross-linking, crushing, screening and sterilization. The provided gelatin embolic particles can be completely degraded in a short period of time, thereby meeting clinical needs; the gelatin embolic particles obtained by the preparation method provided by the present application have high porosity and appropriate water absorption; the suspension performance and catheter passability are excellent, which helps to suspend and transport the particles in the blood, as well as better combine with the target blood vessels, which is conducive to the further application of the embolic particles.

[0007] The specific steps of thermal cross-linking can stabilize the three-dimensional structure of the gelatin mixture, which is not easy to disintegrate and absorb liquid when in contact with water and affect the three-dimensional structure; at the same time, it can achieve the effect of sterilization; remove endotoxins; reduce the use of cross-linking agents and avoid residual increased cytotoxicity.

[0008] In the above technical solution, the quality of raw materials, parameters of the preparation process and operating conditions should be strictly controlled during the preparation process to ensure the quality and stability of the product. At the same time, the prepared particles should be strictly tested and verified to ensure their safety and effectiveness.

[0009] Preferably, the specific steps of the thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying under vacuum drying at 70-80°C for 20-30 minutes, and then placing it under vacuum drying at 115-125°C for 110-130 minutes.

[0010] Preferably, the specific steps of the thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying at 60-90°C for vacuum drying for 20-30 minutes, then placing it at 110-130°C for vacuum drying for 12-18 hours, taking it out and placing it at 40-90°C for 20-30 minutes, and then cooling it at room temperature.

[0011] Preferably, the specific steps of the thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying at 60-90°C for vacuum drying for 20-30 minutes, then placing it at 110-130°C for vacuum drying for 15-16 hours, taking it out and placing it at 60-80°C for 20-30 minutes, and then cooling it at room temperature.

[0012] During the experiment, the inventors found that when the temperature of vacuum drying for thermal cross-linking is low, the gelatin embolic particles degrade quickly and become hydrophilic, but are prone to clogging tubes and agglomeration; when the temperature of vacuum drying for thermal cross-linking is high, the gelatin embolic particles degrade slowly and become hydrophobic, the sponge becomes harder, and clogs tubes; therefore, the present application controls the process parameters of thermal cross-linking to be within the above range.

[0013] Preferably, the specific steps of freeze-drying are: transferring the gelatin foam to a freeze dryer, freezing at -45°C to -25°C for 8 to 16 hours, and then thawing at 4 to 25°C for 8 to 16 hours to obtain a gelatin sponge.

[0014] Preferably, the specific steps of freeze-drying are: transferring the gelatin foam to a freeze dryer, freezing at -45°C to -25°C for 8 to 16 hours, then thawing at 15 to 25°C for 2 to 6 hours, and then thawing at 4 to 15°C for 4 to 12 hours to obtain a gelatin sponge.

[0015] During the experiment, the inventors found that freeze-drying affects the shape and microstructure of the sponge. When the processing temperature is high, the gelatin embolic particle sponge shrinks greatly and the pore size becomes smaller, which affects the softness and makes it easy to block the tube or the liquid absorption speed is too slow. Therefore, the present application controls the freeze-drying process parameters to the above range.

[0016] Preferably, the specific steps of dissolving are: adding a corresponding weight of gelatin particles into water at a concentration of 20 to 80 g / L, stirring and heating to 55 to 65° C., and cooling to 25 to 32° C. after fully dissolving to obtain a gelatin aqueous solution.

[0017] Preferably, the specific steps of dissolving are: adding a corresponding weight of gelatin particles into water at a concentration of 20 to 80 g / L, stirring and heating to 58 to 62° C., and cooling to 25 to 32° C. after fully dissolving to obtain a gelatin aqueous solution.

[0018] In a second aspect, the present application provides a gelatin embolic particle, wherein the gelatin embolic particle is prepared using the above-mentioned preparation method.

[0019] In a third aspect, the present application provides the use of the above-mentioned gelatin embolic particles in hepatic arterial chemoembolization for non-diagnostic purposes.

[0020] In summary, the technical solution of this application has the following effects: The present application improves the preparation process, selects low-endotoxin, high-purity gelatin, and obtains related products through dissolution, foaming, freeze-drying, thermal cross-linking, crushing, screening and sterilization. The provided gelatin embolic particles can be completely degraded in a short period of time, thereby meeting clinical needs; the gelatin embolic particles obtained by the preparation method provided by the present application have high porosity and appropriate water absorption; the suspension performance and catheter passability are excellent, which helps to suspend and transport the particles in the blood, and better combine with the target blood vessels, which is conducive to the further application of the embolic particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 These are morphological pictures of gelatin foams under different foaming volume conditions in Example 1 (from left to right: unfoamed, foamed 3 times, foamed 4 times).

[0022] Figure 2 This is a morphological picture of the gelatin sponge prepared by freeze-drying in Example 1.

[0023] Figure 3 This is a microscope image of the gelatin particles in Example 1. DETAILED DESCRIPTION

[0024] The gelatin raw material (X-Pure 10P HBLV) used in this application was purchased from Rousselot.

[0025] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application. Example

[0026] Example 1 Example 1 provides a gelatin embolic particle and a preparation method thereof.

[0027] The specific steps of the preparation method of gelatin embolic particles in this embodiment are as follows.

[0028] Dissolution: Dissolve 7g of gelatin granules in 100ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved to obtain a gelatin aqueous solution with a concentration of 70g / L, and set aside.

[0029] Foaming: Place the above gelatin solution into a high-speed stirrer and introduce nitrogen gas below the liquid surface, and foam at 3000 rpm until there is no obvious liquid at the bottom of the container and the foaming volume is 4 times the original liquid volume, thereby obtaining gelatin foam. Figure 1 These are morphological images of gelatin foams under different foaming volume conditions in Example 1 (from left to right: no foaming, foaming 3 times, foaming 4 times); therefore, the foaming volume in subsequent tests is 4 times the original liquid volume.

[0030] Freeze drying: transfer the gelatin foam to a freeze dryer, freeze at -35°C for 12 h, then thaw at 20°C for 4 h, and then thaw at 8°C for 8 h to obtain a gelatin sponge. The morphology is shown in the figure. Figure 1 As shown, the morphology is uniform and complete.

[0031] Thermal crosslinking: The gelatin sponge prepared by freeze-drying is placed in a vacuum dryer at 75°C for 25 minutes, and then placed in a vacuum dryer at 120°C for 24-24 hours. After being taken out, it is placed in a 70°C condition for 25 minutes, and then cooled to room temperature.

[0032] Crushing and screening: Put the sponge into the crusher, arrange the screen to collect the sponge particles of 50 to 2000 microns, and observe the morphology under a microscope. Figure 3 As shown, the morphology is uniform and complete, and the particles are average; the above sponge is placed in a sieve with a specification of 50 to 2000 microns, and sieved and collected layer by layer.

[0033] Filling and sterilization: weigh 100 mg of the granules into a 7 ml vial and seal it; sterilize it by irradiation at 25 kgy.

[0034] Embodiment 2-8 Examples 2-8 respectively provide a gelatin embolic particle and a preparation method thereof.

[0035] The difference between the above embodiment and embodiment 1 is that the specific steps of thermal cross-linking are different, as shown below.

[0036] In Example 2: The specific steps of thermal crosslinking are: the gelatin sponge prepared by freeze-drying is placed in a vacuum drying condition at 60°C for 25 minutes, then placed in a vacuum drying condition at 120°C for 24 hours, taken out and placed in a condition at 70°C for 25 minutes, and then cooled to room temperature.

[0037] In Example 3: The specific steps of thermal crosslinking are: vacuum drying the gelatin sponge prepared by freeze-drying at 90°C for 25 minutes, then vacuum drying it at 120°C for 24 hours, taking it out and placing it at 70°C for 25 minutes, and then cooling it at room temperature.

[0038] In Example 4: The specific steps of thermal crosslinking are: the gelatin sponge prepared by freeze-drying is placed in a vacuum drying condition at 75°C for 25 minutes, then placed in a vacuum drying condition at 110°C for 24 hours, taken out and placed in a condition at 70°C for 25 minutes, and then cooled to room temperature.

[0039] In Example 5: The specific steps of thermal crosslinking are: the gelatin sponge prepared by freeze-drying is placed in a vacuum drying condition at 75°C for 25 minutes, then placed in a vacuum drying condition at 130°C for 24 hours, taken out and placed in a condition at 70°C for 25 minutes, and then cooled to room temperature.

[0040] In Example 6, the specific steps of thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying under vacuum drying at 75°C for 25 minutes, then placing it under vacuum drying at 120°C for 10 hours, taking it out and cooling it at room temperature.

[0041] In Example 7: The specific steps of thermal crosslinking are: vacuum-dry the gelatin sponge prepared by freeze-drying at 75°C for 25 minutes, then vacuum-dry at 120°C for 36 hours, take it out and place it at 40°C for 25 minutes, then cool it to room temperature.

[0042] In Example 8: The specific steps of thermal crosslinking are: vacuum drying the gelatin sponge prepared by freeze-drying at 75°C for 25 minutes, then vacuum drying at 120°C for 24 hours, taking it out and placing it at 90°C for 25 minutes, and then cooling it at room temperature.

[0043] The remaining steps of the preparation method of gelatin embolic particles in the above embodiment are the same as those in Example 1.

[0044] Examples 9-11 Examples 9-11 respectively provide a gelatin embolic particle and a preparation method thereof.

[0045] The difference between the above embodiment and embodiment 1 is that the specific steps of freeze-drying are different, as shown below.

[0046] In Example 9, the specific steps of freeze drying are: transferring the gelatin foam to a freeze dryer, freezing at -45°C for 12 hours, and then thawing at 20°C for 12 hours to obtain a gelatin sponge.

[0047] In Example 10, the specific steps of freeze drying are: transferring the gelatin foam to a freeze dryer, freezing at -45°C for 12 hours, and then thawing at 8°C for 12 hours to obtain a gelatin sponge.

[0048] In Example 11: The specific steps of freeze drying are: transfer the gelatin foam to a freeze dryer, freeze it at -45°C for 12 hours, then thaw it at 8°C for 4 hours, and then thaw it at 20°C for 8 hours to obtain a gelatin sponge.

[0049] The remaining steps of the preparation method of gelatin embolic particles in the above embodiment are the same as those in Example 1.

[0050] Examples 12-14 Examples 12-14 respectively provide a gelatin embolic particle and a preparation method thereof.

[0051] The difference between the above embodiment and embodiment 1 is that the concentration of the gelatin aqueous solution in the dissolution step is different, as shown below.

[0052] In Example 12: Dissolution: Dissolve 2 g of gelatin particles in 100 ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved, and obtain a gelatin aqueous solution with a concentration of 20 g / L for standby use.

[0053] In Example 13: Dissolution: Dissolve 5 g of gelatin granules in 100 ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved, and obtain a gelatin aqueous solution with a concentration of 50 g / L for standby use.

[0054] In Example 14: Dissolution: Dissolve 10 g of gelatin particles in 100 ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved, and obtain a gelatin aqueous solution with a concentration of 100 g / L for standby use.

[0055] The remaining steps of the preparation method of gelatin embolic particles in the above embodiment are the same as those in Example 1.

[0056] Comparative Example Comparative Example 1 This comparative example provides a gelatin embolic particle and a preparation method thereof.

[0057] The specific steps of the preparation method of gelatin embolic particles in this comparative example are as follows.

[0058] Dissolution: Dissolve 7g of gelatin granules in 100ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved to obtain a gelatin aqueous solution with a concentration of 70g / L, and set aside.

[0059] Foaming: Add 20 ml of formaldehyde with a concentration of 1 mg / mL to the above gelatin solution, put it into a high-speed stirrer and pass nitrogen gas under the liquid surface, and foam it at 3000 rpm until there is no obvious liquid at the bottom of the container to obtain gelatin foam.

[0060] Freeze drying: transfer the gelatin foam to a freeze dryer, freeze at -35°C for 12 h, then thaw at 20°C for 4 h, and then thaw at 8°C for 8 h to obtain gelatin sponge.

[0061] Thermal crosslinking: The gelatin sponge prepared by freeze-drying is placed in a vacuum dryer at 75°C for 25 minutes, and then placed in a vacuum dryer at 120°C for 24 hours. After being taken out, it is placed in a 70°C condition for 25 minutes, and then cooled to room temperature.

[0062] Crushing and screening: Place the sponge into a crusher and arrange the screen to collect sponge particles of 50 to 2000 microns; place the sponge into a sieve of 50 to 2000 microns and screen and collect layer by layer.

[0063] Filling and sterilization: weigh 100 mg of the granules into a 7 ml vial and seal it; sterilize it by irradiation at 25 kgy.

[0064] Comparative Example 2 This comparative example provides a gelatin embolic particle and a preparation method thereof.

[0065] The specific steps of the preparation method of gelatin embolic particles in this comparative example are as follows.

[0066] Dissolution: Dissolve 7g of gelatin granules in 100ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved to obtain a gelatin aqueous solution with a concentration of 70g / L, and set aside.

[0067] Foaming: Place the above gelatin solution into a high-speed stirrer and introduce nitrogen gas below the liquid surface, and foam at 3000 rpm until there is no obvious liquid at the bottom of the container to obtain gelatin foam.

[0068] Freeze drying: transfer the gelatin foam to a freeze dryer, freeze at -35°C for 12 h, then thaw at 20°C for 4 h, and then thaw at 8°C for 8 h to obtain gelatin sponge.

[0069] Thermal crosslinking: The gelatin sponge prepared by freeze-drying is placed under vacuum drying at 75°C for 24 hours, taken out and placed under 70°C for 25 minutes, and then cooled to room temperature.

[0070] Crushing and screening: Place the sponge into a crusher and arrange the screen to collect sponge particles of 50 to 2000 microns; place the sponge into a sieve of 50 to 2000 microns and screen and collect layer by layer.

[0071] Filling and sterilization: weigh 100 mg of the granules into a 7 ml vial and seal it; sterilize it by irradiation at 25 kgy.

[0072] Comparative Example 3 This comparative example provides a gelatin embolic particle and a preparation method thereof.

[0073] The specific steps of the preparation method of gelatin embolic particles in this comparative example are as follows.

[0074] Dissolution: Dissolve 7g of gelatin granules in 100ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved to obtain a gelatin aqueous solution with a concentration of 70g / L, and set aside.

[0075] Foaming: Place the above gelatin solution into a high-speed stirrer and introduce nitrogen gas below the liquid surface, and foam at 3000 rpm until there is no obvious liquid at the bottom of the container to obtain gelatin foam.

[0076] Freeze drying: transfer the gelatin foam to a freeze dryer, freeze at -35°C for 12 h, then thaw at 20°C for 4 h, and then thaw at 8°C for 8 h to obtain gelatin sponge.

[0077] Thermal crosslinking: The gelatin sponge prepared by freeze-drying is placed under vacuum drying at 140°C for 24 hours, taken out and placed under 70°C for 25 minutes, and then cooled to room temperature.

[0078] Crushing and screening: Place the sponge into a crusher and arrange the screen to collect sponge particles of 50 to 2000 microns; place the sponge into a sieve of 50 to 2000 microns and screen and collect layer by layer.

[0079] Filling and sterilization: weigh 100 mg of the granules into a 7 ml vial and seal it; sterilize it by irradiation at 25 kgy.

[0080] Comparative Examples 4-5 Comparative Examples 4-5 respectively provide a gelatin embolic particle and a preparation method thereof.

[0081] The difference between the comparative example and Example 1 is that the concentration of the gelatin aqueous solution in the dissolution step is different, as shown below.

[0082] In Comparative Example 4: Dissolution: Dissolve 1 g of gelatin particles in 100 ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved, and obtain a gelatin aqueous solution with a concentration of 10 g / L for standby use.

[0083] In Comparative Example 5: Dissolution: Dissolve 12 g of gelatin granules in 100 ml of water for injection, stir and heat to 60°C, cool to 30°C after fully dissolved, and obtain a gelatin aqueous solution with a concentration of 120 g / L for standby use.

[0084] The remaining steps of the preparation method of gelatin embolic particles in the above embodiment are the same as those in Example 1.

[0085] Performance testing (1) Average pore size: The pore size distribution of gelatin particles was determined by mercury intrusion porosimetry according to European Pharmacopoeia 2.9.32.

[0086] Test results: as shown in Table 1.

[0087] (2) Water absorption ratio: Weigh 100 mg of gelatin particles accurately and immerse them in a beaker filled with water at 20±2°C. Stir until the microspheres are completely soaked and all the air is expelled. After absorbing enough water, filter out the excess water in the beaker and weigh the embolism imaging microspheres again, record it as M2, and calculate the water absorption ratio A. The calculation formula is: A = (M2-M1) / M1×100%.

[0088] Test results: as shown in Table 1.

[0089] (3) In vitro degradation experiment: 20 mg of gelatin particles were soaked in a centrifuge tube containing 30 ml of sterile saline at 37°C and shaken, and the changes of the gelatin particles were observed every 1 hour.

[0090] Test results: as shown in Table 1.

[0091] (4) Suspension: 100 mg of gelatin particles were placed in the test solution consisting of water for injection, normal saline, a mixed solution of normal saline and iohexol contrast agent in a volume ratio of 1:5, or a mixed solution of normal saline and iohexol contrast agent in a volume ratio of 1:1. After mixing evenly and reaching a stable state, a 20 mL syringe was used for vertical tube timing to observe the suspension state of the microspheres (good, fair, or poor).

[0092] Test results: as shown in Table 1.

[0093] (5) Catheter passability: Connect the syringe containing the contrast agent-gelatin particle suspension in performance test method (4) to a 2.7F microcatheter, using a 2 ml syringe at a pushing rate of 2 ml / min. Observe and record the state of the microspheres when they enter the microcatheter and when they exit the microcatheter and enter the centrifuge tube (dispersion, adhesion, clumping, wall adhesion, tube blockage), and record the resistance to passage.

[0094] Test results: as shown in Table 1.

[0095] Table 1 Performance test results of gelatin particles in Examples 1-14 and Comparative Examples 1-5 Table 2 Performance test results of gelatin particles in Examples 1-14 and Comparative Examples 1-5 Combined with the test results in Tables 1-2, the present application uses gelatin as a raw material, and the gelatin embolic particles obtained through dissolution, foaming, freeze-drying, crushing, thermal cross-linking, screening, and sterilization have good appearance and morphology, and the embolic particles have high porosity, low average pore size, and appropriate water absorption; and the gelatin embolic particles prepared in the present application have excellent suspension properties and catheter passability, which is conducive to the application of embolic particles in hepatic artery chemoembolization for non-diagnostic purposes.

[0096] In Examples 12-14 and Comparative Examples 4-5: the different concentrations of the gelatin aqueous solution in the dissolution step directly affect the density of the gelatin sponge. When the concentration of the gelatin aqueous solution is low, the foaming effect is poor, liquid is easily generated at the bottom of the beaker, the sponge is not strong enough, the suspension is poor, it does not block the tube, and the embolization effect is poor; when the concentration of the gelatin aqueous solution is high, the gelatin sponge is hard and brittle, the liquid absorption speed is slow, it blocks the tube, cannot be suspended well, and is easy to sink to the bottom.

[0097] (5) Embolic agents are used in animal experiments. The animals selected are pigs. The experimental animals are placed in the experimental environment 7 days before the operation to adapt to the constant temperature and humidity environment in the animal room. The lighting is alternating 12h / 12h every day. The animals are fed an appropriate amount of animal feed once in the morning and afternoon every day. They are allowed to drink water freely. Each experimental animal is fasted for 12 hours before the operation, but can drink water freely. No water is allowed on the morning of the planned implantation day.

[0098] General anesthesia was performed through oral endotracheal intubation and anesthesia machine-assisted ventilation; echocardiography was performed before surgery.

[0099] After the animal is transferred to the operating room, it is transported to the operating room and placed in the right side lying position on the operating table; the heart rate, pulse, and oxygenation function of the animal are continuously monitored using surface electrodes; a temperature monitoring probe is placed to monitor the animal's body temperature; the surgical field is disinfected with iodine tincture and covered with sterile towels; arterial and venous access is established; renal artery angiography is performed before surgery; and the gelatin particles in Example 1 are injected.

[0100] Animal experiment results show that short-term embolization of gelatin particles can restore blood vessels within 2-24 hours and avoid overall organ necrosis.

[0101] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing gelatin embolic particles, characterized in that: Specifically, the following steps are performed in sequence: Using gelatin as raw material, it is dissolved, foamed, freeze-dried, crushed, thermally cross-linked, sieved and sterilized; The specific steps of foaming are: introducing nitrogen gas below the liquid surface of a 20-80 g / L gelatin aqueous solution, foaming at a rotation speed of 2500-3500 rpm until there is no obvious liquid at the bottom of the container, and the foaming volume is 1-10 times the original liquid volume, so as to obtain a gelatin foam; the specific steps of thermal crosslinking include: placing the gelatin sponge prepared by freeze-drying under vacuum drying at 60-90° C. for 20-30 minutes, and then placing it under vacuum drying at 110-130° C. for 10-36 hours, so as to obtain the product.

2. The method for preparing gelatin embolic particles according to claim 1, characterized in that: The specific steps of the thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying under vacuum drying at 70-80°C for 20-30 minutes, and then placing it under vacuum drying at 115-125°C for 110-130 minutes.

3. The method for preparing gelatin embolic particles according to claim 1, characterized in that: The specific steps of the thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying at 60-90°C for vacuum drying for 20-30 minutes, then placing it at 110-130°C for vacuum drying for 12-18 hours, taking it out and placing it at 40-90°C for 20-30 minutes, and then cooling it at room temperature.

4. The method for preparing gelatin embolic particles according to claim 3, characterized in that: The specific steps of the thermal crosslinking are: placing the gelatin sponge prepared by freeze-drying at 60-90°C for vacuum drying for 20-30 minutes, then placing it at 110-130°C for vacuum drying for 15-16 hours, taking it out and placing it at 60-80°C for 20-30 minutes, and then cooling it at room temperature.

5. The method for preparing gelatin embolic particles according to claim 1, characterized in that: The specific steps of freeze drying are: transferring the gelatin foam to a freeze dryer, freezing at -45°C to -25°C for 8 to 16 hours, and then thawing at 4 to 25°C for 8 to 16 hours to obtain a gelatin sponge.

6. The method for preparing gelatin embolic particles according to claim 5, characterized in that: The specific steps of freeze drying are: transferring the gelatin foam to a freeze dryer, freezing at -45°C to -25°C for 8 to 16 hours, then thawing at 15 to 25°C for 2 to 6 hours, and then thawing at 4 to 15°C for 4 to 12 hours to obtain a gelatin sponge.

7. The method for preparing gelatin embolic particles according to claim 1, characterized in that: The specific steps of dissolving are: adding corresponding weight of gelatin particles into water at a concentration of 30-70 g / L, stirring and heating to 55-65° C., cooling to 25-32° C. after fully dissolving to obtain gelatin aqueous solution.

8. The method for preparing gelatin embolic particles according to claim 7, characterized in that: The specific steps of dissolving are: adding corresponding weight of gelatin particles into water at a concentration of 40-60 g / L, stirring and heating to 58-62° C., cooling to 25-32° C. after fully dissolving to obtain a gelatin aqueous solution.

9. A gelatin embolic particle, characterized in that: The gelatin embolic particles are prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the gelatin embolic particles according to claim 9 in hepatic arterial chemoembolization for non-diagnostic purposes.

Citation Information

Patent Citations

  • Gelatin sponge embolic agent, preparation method and application thereof, and medicine for treating vascular diseases or tumors

    CN110876812A

  • Gelatin sponge, preparation method thereof and embolism material prepared from gelatin sponge

    CN115584050A

  • Preparation method of gelatin material capable of absorbing hemostatic fluid

    CN116251227A

  • Absorbing gelatin particle and gelatin particle for sustained-release of bioactive substance, and device for administration of bioactive substance

    JP2014058465A

  • Production method for gelatin sponge for regeneration of eardrum

    TW202135853A