Kneading and mixing method for gas-producing composition containing nitroguanidine and gas-producing composition

Through the kneading and mixing method of wet nitroguanidine, the preparation of gas-producing composition is directly used to solve the problems of high storage cost and high safety risks of nitroguanidine drying and dry nitroguanidine. It achieves high efficiency, safety and low cost of production.

CN119191923APending Publication Date: 2024-12-27SHAANXI QINGHUA AUTOMOTIVE SAFETY SYST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411307522.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-27

AI Technical Summary

Technical Problem

Nitroguanidine drying and dry nitroguanidine have high storage costs and high safety risks. The prior art requires pre-drying to reduce moisture content, increasing production costs and safety design requirements.

Method used

The wet nitroguanidine is used as a combustible agent, combined with a water-soluble binder and solvent, and the gas-producing composition is directly prepared by kneading and mixing method. The drying and drying steps of nitroguanidine are eliminated, and the feeding order and kneading process are clarified. Improved the success rate and craftsmanship of the joint operations.

Benefits of technology

It reduces safety risks, simplifies production line layout and workshop design, shortens kneading processing time, reduces manufacturing costs, and improves the safety and efficiency of the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119191923A_ABST
    Figure CN119191923A_ABST
Patent Text Reader

Abstract

The invention discloses a kneading and mixing method of a nitroguanidine-containing aerogenesis composition, which comprises the following steps: firstly feeding wet nitroguanidine, sequentially feeding and kneading a water-soluble adhesive and a solvent, sequentially feeding and kneading other materials, taking the final kneaded material, and carrying out extrusion molding to obtain the nitroguanidine-containing aerogenesis composition. According to the method, material pretreatment links such as drying of wet nitroguanidine and storage of dry nitroguanidine are solved, and the problems of high cost and high safety risk are solved. The invention further discloses the gas production composition containing nitroguanidine, the gas production composition containing nitroguanidine is prepared by adopting the kneading and mixing method of the gas production composition containing nitroguanidine, the preparation process is safe and efficient, and the cost is lower than that of a gas production composition prepared by a traditional method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of manufacturing pyrotechnic powder for explosives, relates to a kneading and mixing method of a gas generating composition containing nitroguanidine, and also relates to a gas generating composition containing nitroguanidine. Background Art

[0002] Most of the nitroguanidine sold on the market is hydrated, with a water content of more than 20% (its hazard level is 4.1, hereinafter referred to as wet nitroguanidine). Relevant data show that the moisture content of wet nitroguanidine must not be less than 15% when it is stored. Due to safety management requirements, nitroguanidine is transported and stored in a wet state. When used as a combustible agent in a gas-producing composition, it is usually dried in advance, such as drying to a water content of no more than 0.15%. After drying, the moisture content of nitroguanidine is low and the hazard becomes higher (the hazard level is 1.1 at this time, hereinafter referred to as dry nitroguanidine). The gas-producing composition is prepared according to the product process flow. The order or timing of feeding dry nitroguanidine has no obvious effect on the kneading, mixing and extrusion operations.

[0003] The drying of nitroguanidine and the storage place after drying have a high safety design level, which means high manufacturing cost. In addition, drying requires professional equipment, personnel and time management, all of which will increase manufacturing cost. Summary of the invention

[0004] The purpose of the present invention is to provide a kneading and mixing method for a gas-generating composition containing nitroguanidine, so as to solve the problems of high cost and high safety risk of material pretreatment such as drying of nitroguanidine and storage of dry nitroguanidine.

[0005] Another object of the present invention is to provide a gas-generating composition containing nitroguanidine, which is efficient and safe to produce.

[0006] The first technical scheme adopted by the present invention is a kneading and mixing method of a gas-generating composition containing nitroguanidine. The gas-generating composition containing nitroguanidine includes a combustible containing nitroguanidine, a water-soluble adhesive, a solvent, an oxidant and auxiliary components. The combustible containing nitroguanidine includes wet nitroguanidine. The kneading and mixing method first feeds the wet nitroguanidine, then feeds the water-soluble adhesive and the solvent, kneads them, and then feeds and kneads the other components of the combustible, feeds and kneads the oxidant, and feeds and kneads the auxiliary components before the solvent is added or is added and kneaded separately. The kneaded material finally obtained is extruded and formed. The kneaded material is in a wet granular or lumpy state and has ductility after being compressed.

[0007] The first technical solution of the present invention is also characterized in that: The mass percentage of water in the wet nitroguanidine is greater than or equal to 20%, and the mass percentage of the wet nitroguanidine in the total amount of the combustible agent is 25% to 100%.

[0008] The wet nitroguanidine is fed in at one time, that is, all the wet nitroguanidine is fed in at one time; other combustible components and oxidants are fed in after the previous kneading step is completed, and other combustible components and oxidants are fed in once or multiple times.

[0009] The solvent includes water and other solvents miscible with water, and the mass percentage of water in the total solvent is greater than or equal to 60%.

[0010] After kneading each batch of material, first evaluate the kneading effect of the kneaded material, and determine whether to proceed to the next step based on the kneading effect.

[0011] The kneading effect is evaluated and judged specifically as follows: if the kneaded material is in the form of lumps, and the kneaded material can be formed into sheets by rubbing it with fingers, then the kneading effect of the material is judged to be good, and the next step is carried out; if the kneaded material is in the form of loose powder, or the material is still loose after being rubbed and kneaded with fingers, then the current kneading is judged to be insufficient, and the next operation process is postponed, and kneading is continued until the kneading effect is good, and then the next step is carried out.

[0012] The second technical solution adopted by the present invention is a gas generating composition containing nitroguanidine, which is prepared by the kneading and mixing method of the gas generating composition containing nitroguanidine of the present invention.

[0013] The beneficial effects of the present invention are: The method for kneading and mixing a gas-generating composition containing nitroguanidine of the present invention directly uses wet nitroguanidine to knead and mix the materials, thereby eliminating material pretreatment operations such as drying of nitroguanidine and storage of dry nitroguanidine, effectively reducing safety risks; simplifying the layout of the production line and reducing workshop design requirements; clarifying the feeding sequence of wet nitroguanidine, adhesive and solvent, improving the success rate of the kneading operation, shortening the kneading processing time, and being conducive to improving the process performance of processes such as extrusion.

[0014] The kneading and mixing method of the gas-generating composition containing wet nitroguanidine of the present invention shortens the process flow, reduces the safety risk of the preparation process, and has lower manufacturing cost compared with the kneading preparation method using dry nitroguanidine. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The present invention is a flow chart of the kneading and mixing method of the gas generating composition containing nitroguanidine. DETAILED DESCRIPTION

[0016] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0017] The kneading and mixing method of the gas-generating composition containing nitroguanidine of the present invention completes the material mixing in a "kneading" manner, one of the combustibles is wet nitroguanidine, a hydrophilic material is used as a binder, and water is used as a main solvent. The gas-generating composition containing nitroguanidine includes a combustible containing nitroguanidine, a water-soluble binder, a solvent, an oxidant, and auxiliary components. The combustible containing nitroguanidine is wet nitroguanidine, and its water mass percentage is greater than or equal to 20%, and the mass proportion of wet nitroguanidine in the total amount of the combustible is 25% to 100%. The solvent includes water, and other solvents that are miscible with water and volatile. Other solvents can be selected from alcohol, and the mass percentage of water in the total solvent is greater than or equal to 60%. The water-soluble binder is one or more of hydroxypropyl methylcellulose, carboxymethyl cellulose, sodium carboxymethyl cellulose, guar gum, etc. The oxidant can be one or more combinations of perchlorate, nitro salt, basic nitrate, and metal oxide.

[0018] The kneading and mixing method takes wet nitroguanidine, measures its moisture content, calculates the wet nitroguanidine weighing amount according to the formula basis, calculates the total design water volume according to the solvent water ratio, subtracts the free water content in the wet nitroguanidine from the total design water volume, and the difference is the actual weighing water volume. Other materials are prepared according to the product formula table; Figure 1 As shown, wet nitroguanidine is fed first, followed by water-soluble adhesive and solvent, and kneaded. When feeding the adhesive, it is randomly sprinkled on the wet nitroguanidine. The solvent water is fed as the third material. Other solvents can be premixed with water and fed at once, or they can be fed separately with water. There is no special restriction on the feeding order of water and other solvents. Then, this round of kneading is carried out. After that, other components of the combustible agent are fed and kneaded in turn, and auxiliary components are fed and kneaded. There is no special requirement for the feeding order of auxiliary components. They can be fed before the solvent is fed, or they can be set as a separate feeding and kneading step. If the feeding is placed before the solvent, it is relatively more time-saving. If there is no auxiliary component, this step is skipped, and the oxidant is fed and kneaded. After all materials are kneaded, the kneaded material finally obtained is extruded, and pelletized as needed to complete the molding process.

[0019] The wet nitroguanidine, adhesive and solvent are all added at one time; when the proportion of other components is not less than 10%, it is advisable to divide the addition into multiple times. Adding small amounts and multiple times is more conducive to maintaining the consistency of the kneading material and preventing the material from powdering after a large amount of a certain raw material is added. After powdering, if the kneading effect is not evaluated after the process step is completed and necessary delayed remedial measures are not taken, kneading failure may occur.

[0020] There are two evaluation items for kneading effect in each process step, one is the appearance and flowability of the material, the other is the compression ductility. The ductility evaluation is better than the appearance and flowability evaluation.

[0021] The kneading effect evaluation method is as follows: if the kneaded material has poor fluidity and is in the form of lumps, and the kneaded material can be easily rubbed into sheets by fingers, then the material kneading effect is judged to be good and the next step of operation can be carried out; if the kneaded material has good fluidity and is in the form of loose powder or similar loose powder, or the kneaded material is loose when rubbed and kneaded by fingers and is difficult to deform and stretch into sheets, then the current kneading is judged to be insufficient, and the next operation process should be postponed, and kneading should be continued until the kneading effect is good, and then the next step can be carried out.

[0022] The present invention also provides a nitroguanidine-containing gas generating composition, which is prepared by the kneading and mixing method of the nitroguanidine-containing gas generating composition of the present invention.

[0023] Example 1 The present embodiment provides a method for kneading and mixing a gas-generating composition containing nitroguanidine. The gas-generating composition containing nitroguanidine includes a combustible containing nitroguanidine, a water-soluble adhesive, a solvent, an oxidant and auxiliary components. The combustible containing nitroguanidine includes wet nitroguanidine. The kneading and mixing method first feeds the wet nitroguanidine, then feeds the water-soluble adhesive and the solvent, kneads them, feeds the auxiliary components, kneads them, feeds the oxidant, kneads them, and finally takes the kneaded material to extrude strips and discharges the material.

[0024] After each kneading, the kneading effect of the kneaded material is judged, and whether to proceed to the next step of feeding or extrusion is determined based on the kneading effect.

[0025] The kneading effect evaluation method is as follows: if the kneaded material has poor fluidity and is in the form of lumps, and the kneaded material can be formed into sheets by rubbing it with fingers, then the material kneading effect is judged to be good and the next step of operation is carried out; if the kneaded material has good fluidity and is in the form of loose powder or similar loose powder, or the material is still loose after being rubbed and kneaded by fingers and is difficult to deform and stretch into sheets, then the current kneading is judged to be insufficient, and the next operation process should be postponed, and kneading should be continued until the kneading effect is good, and then the next step can be carried out.

[0026] The water content of wet nitroguanidine is 20%, and the mass proportion of wet nitroguanidine in the total amount of combustible agent is 100%.

[0027] The solvent includes water and alcohol, and the mass percentage of water in the total solvent is equal to 60%.

[0028] The wet nitroguanidine is fed in one go, i.e. all the wet nitroguanidine is fed in one go; all the auxiliary materials are fed in one go, while the oxidant is fed in multiple times.

[0029] This embodiment also provides a nitroguanidine-containing gas generating composition, which is prepared by the kneading and mixing method of the nitroguanidine-containing gas generating composition of this embodiment.

[0030] Example 2 The present embodiment provides a method for kneading and mixing a gas-generating composition containing nitroguanidine. The gas-generating composition containing nitroguanidine includes a combustible containing nitroguanidine, a water-soluble adhesive, a solvent, an oxidant and auxiliary components. The combustible containing nitroguanidine includes wet nitroguanidine and guanidine nitrate. The kneading and mixing method first feeds the wet nitroguanidine, then feeds the water-soluble adhesive and the solvent in turn, kneads them, then feeds and kneads the other components of the combustible, feeds and kneads the auxiliary components, feeds and kneads the oxidant, and kneads them, and finally takes the final kneaded material to extrude and discharge it.

[0031] After each kneading, the kneading effect of the kneaded material is judged, and whether to proceed to the next step of feeding or extrusion is determined based on the kneading effect.

[0032] The kneading effect evaluation method is as follows: if the kneaded material has poor fluidity and is in the form of lumps, and the kneaded material can be formed into sheets by rubbing it with fingers, then the material kneading effect is judged to be good and the next step is carried out; if the kneaded material has good fluidity and is in the form of loose powder or similar loose powder, or the kneaded material is loose when rubbed and kneaded by fingers and is difficult to deform and stretch into sheets, then the current kneading is judged to be insufficient, and the next operation process should be postponed, and kneading should be continued until the kneading effect is good, and then the next step can be carried out.

[0033] The water content of wet nitroguanidine is 22%, and the mass proportion of wet nitroguanidine in the total amount of combustible agent is 25%, and the rest is guanidine nitrate.

[0034] The solvent includes water and other solvents miscible with water, and the mass percentage of water in the total solvent is 70%.

[0035] The wet nitroguanidine is fed in one go, i.e. all the wet nitroguanidine is fed in one go; the other components of the combustible agent and the oxidant are fed in multiple times.

[0036] This embodiment also provides a nitroguanidine-containing gas generating composition, which is prepared by the kneading and mixing method of the nitroguanidine-containing gas generating composition of this embodiment.

[0037] Comparative Example 1 This comparative example provides a gas-generating composition containing nitroguanidine, wherein the nitroguanidine is dried dry nitroguanidine (the moisture content of the sample is 0.1% according to a rapid moisture meter). When dry nitroguanidine is used, the order of feeding has no significant effect on the kneading effect.

[0038] Test number "Test 1#", its process and material status are described as follows: 5% of the binder hydroxypropyl methylcellulose and 20% of water are added and kneaded to obtain a mass-like material; 25% dry nitroguanidine was added twice and kneaded separately to obtain agglomerated materials; 25% guanidine nitrate was added twice and kneaded separately to obtain agglomerated materials; 2% auxiliary materials are added at one time and kneaded to obtain a mass-like material; 43% potassium perchlorate was added twice and kneaded separately to obtain agglomerated materials.

[0039] After each operation step, only the appearance of the material is recorded, and no evaluation of the kneading effect is performed.

[0040] After the kneading of all materials is completed, the kneaded materials are extruded into shape using a press, and then pelletized, screened, dried, and other operations are performed to obtain the final product.

[0041] Comparative Example 2: Wet nitroguanidine was used instead of dry nitroguanidine, the proportions of various raw materials were the same as those in comparative example 1, and the kneading process flow was exactly the same as that in "Test 1#".

[0042] Take wet nitroguanidine and measure its water content with a rapid moisture meter (the actual sample water content is 22%). Calculate the weight of wet nitroguanidine according to the design formula, calculate the free water content in wet nitroguanidine, and subtract the free water content in wet nitroguanidine from the total water consumption to obtain the actual water consumption. Prepare the remaining materials according to the product formula.

[0043] The test number is "2A# test": after the first portion of wet nitroguanidine is added and kneaded, the second portion of wet nitroguanidine is directly transferred to the kneading operation. During this period, only the appearance of the material is recorded, and no effect evaluation is performed. No improvement measures are taken for abnormal kneading. After that, the kneading operation is carried out according to the established process and the entire kneading process is completed. The batch test results of "2A# test" are that the kneaded material is powdery, the extrusion pressure is high and the material cannot be discharged stably and continuously, and the subsequent operation fails.

[0044] The test number is "Test 2B#": It repeats Test 2A#, but the difference is that the kneading effect is evaluated at each link. According to the evaluation conclusion, the kneading is delayed for those with poor ductility in order to improve the effect, ensure that the kneaded material has good ductility, complete all kneading operations, and have good processability for extrusion operations, that is, the extrusion discharging process is continuous and relatively stable.

[0045] Comparative Example 3 Test number "Test #3", the ratio of various raw materials is the same as that of Comparative Example 1, wet nitroguanidine is used, and the process is described as follows: Take wet nitroguanidine and measure its water content with a rapid moisture meter. Based on the water content, calculate the amount of wet nitroguanidine and solvent water respectively. Prepare the remaining materials according to the product formula.

[0046] Based on the "2B# test", wet nitroguanidine is added at one time, after the binder is added and before the solvent is added, that is, the binder is added first, then the wet nitroguanidine, and finally the solvent. The rest of the process is the same as the 2B# test.

[0047] The kneading effect is evaluated after each kneading step, and delayed kneading is implemented for those in poor condition until the ductility improves. Then the entire process is completed as planned, and the extrusion process has good processability.

[0048] Example 3 The present embodiment provides a method for kneading and mixing a gas-generating composition containing nitroguanidine, with the test number "Test #4". Wet nitroguanidine is taken, and its water content is measured with a rapid moisture meter. According to the mass percentage, 50% of a combustible agent containing nitroguanidine, 5% of hydroxypropyl methylcellulose, 20% of water, 43% of potassium perchlorate and 2% of an auxiliary component are taken. The combustible agent containing nitroguanidine includes wet nitroguanidine and guanidine nitrate. The mass ratio of wet nitroguanidine to guanidine nitrate is 1:1, i.e., 25% of each.

[0049] Based on the "3# test", the difference is that wet nitroguanidine is added first, and then the binder and solvent are added in sequence. During the kneading operation, the material is observed to be lumpy in appearance, with poor fluidity and good ductility. Within the same kneading time, this embodiment is more conducive to fully kneading the material.

[0050] Afterwards, guanidine nitrate was added twice and kneaded separately to evaluate the effect.

[0051] Add auxiliary materials and knead them, and evaluate the effect.

[0052] Potassium perchlorate was added twice and kneaded separately, and the effect was evaluated.

[0053] The final kneaded material is extruded and molded, and the processability is good.

[0054] Compared with the "3# test", the "4# test" has similar process and no obvious difference in material status, but the operation time is significantly shortened.

[0055] Example 4 This embodiment provides a kneading and mixing method for a gas-generating composition containing nitroguanidine, the test number is "5# test", wet nitroguanidine is taken, its water content is measured by a rapid moisture meter, 50% of a combustible containing nitroguanidine, 5% of hydroxypropyl methylcellulose, 20% of water, 43% of potassium perchlorate and 2% of an auxiliary component are taken according to mass percentage, the combustible containing nitroguanidine includes wet nitroguanidine and guanidine nitrate, and the mass ratio of wet nitroguanidine to guanidine nitrate is 9:1. Based on "4# test", the difference is that the combustible is only wet nitroguanidine, and it is fed first, followed by the binder, the auxiliary material, and finally the solvent. During the kneading operation, the appearance of the material is observed to be lumpy, with poor fluidity and good ductility.

[0056] The guanidine nitrate was added once and kneaded separately. The effect was evaluated Potassium perchlorate was added twice and kneaded separately, and the effect was evaluated.

[0057] The kneaded material is extruded and formed, and the processability is good.

[0058] In the "5# test", the "auxiliary materials" were kneaded together with wet nitroguanidine. There was no obvious difference in the materials at the end of each step, and the operation time was shortened.

[0059] See Table 1 for experimental comparison. The materials and marked proportions in the table are only used to provide necessary schematic illustrations of the method of the present invention, and their specific components and proportions depend on product specifications.

[0060] Table 1 Test data

[0061] Through the above comparison, it can be found that, by using the kneading and mixing method of the present invention (Examples 3 and 4), the wet nitroguanidine does not need to be dried before the gas-generating composition containing nitroguanidine is kneaded and mixed, and the production line design and process flow design are simplified. In addition, the material change in each kneading step is simple, the kneading time is short, the extrusion pressure is moderate, and the material yield is high.

Claims

1. A method for kneading and mixing a gas generating composition containing nitroguanidine, wherein the gas generating composition containing nitroguanidine comprises a combustible containing nitroguanidine, a water-soluble adhesive, a solvent, an oxidant and auxiliary components, characterized in that: The nitroguanidine-containing combustible comprises wet nitroguanidine. The kneading and mixing method first feeds the wet nitroguanidine, then feeds and kneads the water-soluble adhesive and the solvent, then feeds and kneads the other combustible components, feeds and kneads the oxidant, feeds and kneads the auxiliary components before the solvent is added or feeds and kneads them separately, and finally obtains the kneaded material by extrusion molding. The kneaded material is in the form of wet particles or lumps and is ductile after being compressed.

2. The method for kneading and mixing a gas generating composition containing nitroguanidine according to claim 1, characterized in that: The water content of the wet nitroguanidine is greater than or equal to 20%, and the mass proportion of the wet nitroguanidine in the total amount of the combustible agent is 25% to 100%.

3. The kneading and mixing method of the gas generating composition containing nitroguanidine according to claim 1, characterized in that: The wet nitroguanidine is fed in at one time, that is, all the wet nitroguanidine is fed in at one time; other combustible components and oxidants are fed in after the previous kneading step is completed, and other combustible components and oxidants are fed in once or multiple times.

4. The kneading and mixing method of the gas generating composition containing nitroguanidine according to claim 1, characterized in that: The solvent includes water and other solvents miscible with water, and the mass percentage of water in the total solvent is greater than or equal to 60%.

5. The method for kneading and mixing a gas generating composition containing nitroguanidine according to claim 1, characterized in that: After kneading each batch of material, first evaluate the kneading effect of the kneaded material, and determine whether to proceed to the next step based on the kneading effect.

6. The method for kneading and mixing a gas generating composition containing nitroguanidine according to claim 5, characterized in that: The kneading effect evaluation method is as follows: if the kneaded material is in a lump shape, and the kneaded material can be formed into a sheet shape by rubbing and kneading with fingers, it is judged that the kneading effect of the material is good, and the next link operation is carried out; if the kneaded material is in a loose powder state, or the material is still loose after being rubbed and kneaded with fingers, it is judged that the current kneading is insufficient, and the next operation process is postponed, and kneading is continued until the kneading effect is good, and the next link is carried out.

7. A gas generating composition containing nitroguanidine, characterized in that: The nitroguanidine-containing gas-generating composition is prepared by kneading and mixing method according to any one of claims 1 to 6.