High-temperature-resistant composite nanofluid scale inhibitor and preparation method thereof

By using high-temperature composite nanofluid scale inhibitors made of modified graphene oxide nano and calcium-based polysulfonic acid, the problem of calcium carbonate scale under high temperature, high salt and alkaline conditions in oil field development has been solved, and effective scale inhibition effect and improvement of flow capacity has been achieved.

CN119707133AActive Publication Date: 2025-03-28XINJIANG GUANGYA OIL & GAS NEW TECH DEV CO LTD

Patent Information

Application Number
CN202510229278.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-28
Publication Date
2025-03-28
Estimated Expiration
2045-02-28

AI Technical Summary

Technical Problem

During the oil field development process, calcium carbonate scaling is prone to occur in reservoirs or wellbores under high temperature, high salt and alkaline conditions, resulting in a decrease in seepage capacity and flow capacity, affecting oil and gas production. The prior art is difficult to effectively suppress such scaling.

Method used

A high temperature resistant composite nanofluid scale inhibitor is used, which consists of modified graphene oxide nanoAP-GO, calcium-based nanomodifier calcium-based polysulfonic acid Ca-PAMPS, surfactant, inorganic salt and deionized water. Modified graphene oxide nanometers have large-scale conjugated rings and a large number of carboxylic acids and hydroxyl groups, and calcium-based polysulfonic acids have strong hydrophilicity, calcium ion tolerance and calcium ion chelating properties.

Benefits of technology

This scale inhibitor shows good scale inhibition effect under high temperature, high salt and alkaline conditions, effectively inhibits calcium carbonate scale, improves the flow capacity of oil field water injection and fracturing reflow, and has good promotion prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119707133A_ABST
    Figure CN119707133A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant composite nanofluid scale inhibitor and a preparation method thereof, and belongs to the technical field of oilfield chemistry. The composite nano fluid scale inhibitor is prepared from modified graphene oxide nano AP-GO, a calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS, a surfactant, an inorganic salt and deionized water, the calcium-based nano modifier calcium-based polysulfonic acid contains a large amount of sulfonic acid, carboxylic acid and hydroxyl groups, has strong hydrophilicity, calcium ion tolerance and calcium ion chelating property, and has a good scale inhibition effect on calcium carbonate scale and barium sulfate scale; meanwhile, the modified graphene oxide nanoparticles have large-scale conjugated rings, a large amount of carboxylic acid and hydroxyl groups, and have synergistic interaction with calcium-based polysulfonic acid under the action of anion shielding and large steric hindrance effects, so that the high temperature resistance and scale inhibition performance of the nano scale inhibitor are further improved, a good scale inhibition effect is achieved, and the problems of oilfield water injection and fracturing flowback scaling are effectively solved; good popularization prospects are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield exploitation, and in particular relates to a high-temperature resistant composite nanofluid scale inhibitor and a preparation method thereof. Background Art

[0002] The development of unconventional tight / shale oil and gas reservoirs uses water-based fracturing fluids for fracturing transformation. The scale of fracturing is large, and a large amount of fracturing fluid is injected into the formation, which leads to two problems: first, the water-based fracturing fluid injected into the formation dissolves the soluble salt minerals in the reservoir, resulting in high salinity of the return fluid; second, the fracturing fluid system reacts with the rock during the high-temperature gel breaking process of the reservoir, dissolving a large amount of metal ions (sodium, potassium, calcium, magnesium, etc.). Especially for special alkaline salt-rich strata, the return fluid and formation water are rich in bicarbonate ions. Under the combined effect of the above factors, they are easily affected by temperature, pressure, salinity, and ion composition in the formation or wellbore, resulting in scaling of the formation or wellbore, greatly reducing the seepage capacity in the gaps of the oil and gas formation and the flow capacity in the wellbore, seriously affecting the oil test and later production. In recent years, the scale inhibitors used in water treatment and oilfield produced water have evolved from the initial phosphate scale inhibitors that easily cause water pollution to green scale inhibitors such as homopolymer high temperature resistant scale inhibitors and copolymer high temperature resistant scale inhibitors. However, there is no effective scale inhibitor for calcium carbonate scaling or crystallization in reservoirs or wells under high temperature, high mineralization and sodium bicarbonate water conditions.

[0003] Through searching, the following patent disclosures related to the patent application of the present invention were found; for example, a high temperature resistant composite corrosion inhibitor and its preparation method CN114716031A, synthesized a Mannich base salt and polyaspartic acid sodium salt, and compounded the two to form a composite scale inhibitor, which is green, high temperature resistant, and highly effective in scale inhibition and corrosion inhibition. However, the preparation process of polyaspartic acid sodium salt is relatively complex, and the reaction temperature is high (>200°C). A high temperature resistant scale inhibitor and its preparation method CN114920367B, a polymer scale inhibitor is obtained by copolymerizing carboxymethyl β-cyclodextrin, 2-acrylamide-2-methylpropanesulfonic acid monomer and sodium p-styrene sulfonate, which has high temperature resistance and high scale inhibition efficiency, but has limited scale inhibition performance under high calcium ion and carbonate or bicarbonate conditions. A neutral high temperature resistant salt inhibitor and its preparation method CN117776418B, which is composed of a tetrapolymer of alcohol carboxylic acid, polyepoxysuccinic acid, nitrilotriacetic acid, polyethylene glycol, a pH regulator and water, has a good and sufficient effect under neutral and high temperature (120°C) conditions, but is not ideal for calcium carbonate scale inhibition under alkaline and high temperature conditions. A thermally induced associative scale inhibitor, alkaline scale-inhibiting polymer fracturing fluid system and preparation method thereof CN117362658A, wherein a temperature-sensitive oligomer containing terminal amino groups is synthesized by N,N-dimethylacrylamide and diacetone amide, a multipolymer is obtained by maleic anhydride, 2-acrylamide-2-methylpropanesulfonic acid and sodium allyl polyoxyethylene propylene sulfonate, and then the oligomer and the multipolymer are subjected to a grafting reaction to obtain a thermally induced associative scale inhibitor. The scale inhibitor has good compatibility with the fracturing fluid, high scale inhibition efficiency, and strong resistance to calcium ions and bicarbonate ions, but has the disadvantages of high dosage (0.1-0.3%), and relatively insufficient high temperature resistance and long-term effectiveness. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art, and to provide a high-temperature resistant composite nanofluid scale inhibitor and a preparation method thereof, which can effectively inhibit the occurrence of calcium carbonate scaling and still have good scale inhibition effect under high temperature, high salt and alkalinity (pH=7-9); the composite nanofluid scale inhibitor is prepared from modified graphene oxide nano AP-GO, calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS, surfactant, inorganic salt and deionized water; the calcium-based nano modifier calcium-based polysulfonic acid contains a large amount of sulfonic acid, carboxylic acid and hydroxyl groups, has strong hydrophilicity, calcium ion tolerance and calcium ion chelation, and has good scale inhibition effect on calcium carbonate scale and barium sulfate scale; at the same time, the modified graphene oxide nano has a large-scale conjugated ring, a large amount of carboxylic acid and hydroxyl groups, and synergizes with the calcium-based polysulfonic acid in anion shielding and large steric effect, further improves the high temperature resistance and scale inhibition performance of the nano scale inhibitor, has good scale inhibition effect, effectively solves the scaling problem of oil field water injection and fracturing flowback, and has good promotion prospects.

[0005] In order to achieve the above technical effects, the following technical solutions are adopted: A high temperature resistant composite nanofluid antiscalant, comprising: Modified graphene oxide nano AP-GO, calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS, surfactant, inorganic salt and deionized water; The mass concentration of the modified graphene oxide nano AP-GO in the scale inhibitor is 0.01-0.1%; The mass concentration of the surfactant in the scale inhibitor is 0.1 to 0.4%; The mass concentration of the inorganic salt in the scale inhibitor is 0.3 to 0.5%; The mass ratio of the modified graphene oxide nano AP-GO to the calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS is 1:4 to 1:6; The inorganic salt is one or more of potassium chloride and sodium chloride; The surfactant is one or more of sodium dodecylbenzene sulfonate, sodium hexadecyl sulfate, sodium hexadecyl sulfonate, sodium lauryl polyoxyethylene ether sulfate and disodium lauryl sulfosuccinate.

[0006] Furthermore, the structural formula of the modified graphene oxide nano AP-GO is: .

[0007] Furthermore, the water is deionized water; and the surfactant is sodium hexadecyl sulfate and disodium lauryl sulfosuccinate.

[0008] Furthermore, the specific preparation method of the modified graphene oxide nano AP-GO is: 0.5-1.0 g of graphene oxide GO is ultrasonically dispersed in 100-200 g of deionized water for 1-2 h to form a GO dispersion; 3-amino-1,2-propylene glycol AP is added to the GO dispersion at 5-10 mL / min under stirring conditions, and the reaction is continued at 50-80° C. for 4-6 h; 0.5-2 g of sodium chloride is added to the reaction mixture, stirred and dispersed, and then centrifuged at 1000-2000 r / min for 10-20 min, the upper clear liquid is discarded, and the lower solid is washed, and the process is repeated 2-3 times to obtain 3-amino-1,2-propylene glycol-modified graphene oxide nano AP-GO; the preparation method reaction formula is as follows: .

[0009] Furthermore, the mass ratio of the graphene oxide GO to 3-amino-1,2-propylene glycol AP is 1:1 to 1:4.

[0010] Furthermore, the lower layer of solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1.

[0011] Furthermore, the specific preparation method of the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS is: Calcium chloride is dissolved in water to form a calcium chloride solution, wherein the mass concentration of the calcium chloride solution is 0.1-1%; Dissolve poly (2-acrylamide-2-methylpropanesulfonic acid) (PAMPS) in water to form a PAMPS solution, wherein the mass concentration of the PAMPS solution is 0.5 to 1.5%; The calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 5 to 10 mL / min to produce a white suspension, which is continuously stirred for 15 to 30 min; the suspension is centrifuged at 1000 to 3000 r / min for 5 to 20 min, the supernatant is discarded, and the solid is washed with water for 2 to 3 times; the washed white solid is dried at 50-80° C. to prepare a Ca-PAMPS solid, which is a calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0012] Furthermore, the mass ratio of calcium chloride to poly (2-acrylamide-2-methylpropane sulfonic acid) PAMPS is 1:1 to 1:3.

[0013] Furthermore, the preparation method of the high temperature resistant composite nanofluid antiscalant is specifically as follows: The modified graphene oxide nano AP-GO and the calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS are mixed with an inorganic salt, a surfactant and water according to the concentration and mass ratio, and then heated at 40 to 60° C. and ultrasonically dispersed for 10 to 30 minutes to obtain the high-temperature resistant composite nanofluid scale inhibitor.

[0014] Beneficial effects: The beneficial effects of the present invention are: (1) The present invention provides a high temperature resistant composite nanofluid scale inhibitor, which is composed of anion modified graphene oxide and calcium-based polysulfonic acid. The calcium-based polysulfonic acid contains a large amount of sulfonic acid, carboxylic acid and hydroxyl groups, has strong hydrophilicity, calcium ion tolerance and calcium ion chelation, and has a good scale inhibition effect on calcium carbonate scale and barium sulfate scale. In addition, the modified graphene oxide in the present invention has a large-scale conjugated ring, a large amount of carboxylic acid and hydroxyl groups, and synergizes with the calcium-based polysulfonic acid in anion shielding and large steric effect. The modified graphene oxide nano, calcium-based polysulfonic acid, surfactant and inorganic salt synergistic effect are used to further improve the high temperature resistance and scale inhibition performance of the nanoscale scale inhibitor.

[0015] (2) The high temperature resistant composite nanofluid scale inhibitor provided by the present invention has a relatively simple preparation process, mild reaction conditions, is phosphorus-free and environmentally friendly, has good dispersibility, a particle size of <500nm, and has strong environmental adaptability. It is highly effective in preventing scale under conditions of high temperature, high mineralization, high concentration of carbonate or bicarbonate (>10000mg / L) and high calcium ion water quality, and has a good effect in solving the scaling problem of oil field water injection and fracturing flowback, and has a good promotion prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the infrared spectrum of the modified graphene oxide nano AP-GO in the embodiment of the present invention. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0018] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0019] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and " / " or "including" are used in this specification, it indicates the presence of features, steps, operations and / or combinations thereof.

[0020] The experimental methods in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are commercially available unless otherwise specified. Among them, the main experimental raw materials are as follows: graphene oxide (AR, Evonik), 3-amino-1,2-propanediol (AR, TCI Chemical), calcium chloride (AR, Sinopharm), poly (2-acrylamide-2-methylpropanesulfonic acid) (AR, Sigma, Merck), sodium hexadecyl sulfonate, disodium lauryl sulfosuccinate (AR, Shengke Biochemical).

[0021] Embodiment 1: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.5 g of graphene oxide (GO) was ultrasonically dispersed in 100 g of deionized water for 1 h to form a GO dispersion; 0.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 50 °C for 6 h; 0.5 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1, and the washing was repeated twice to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0022] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 0.5 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 15 min; the suspension is centrifuged at 3000 r / min for 15 min, the supernatant is discarded, and the solid is washed with water twice; the washed white solid is dried at 60°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0023] (3) Weigh 0.2 g of sodium hexadecyl sulfate and 0.2 g of potassium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 40 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.2 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to disperse the mixture for 20 min to obtain a high temperature and alkali-resistant composite nano salt scale inhibitor.

[0024] like Figure 1 As shown in the infrared spectrum, 3416 cm -1 is the stretching vibration of -OH, 2919 cm -1 、2850 cm -1 -CH 2 -CH stretching vibration peak, 1717 cm -1 is the stretching vibration peak of C=O, 1623 cm -1 To preserve graphene sp 2 The stretching vibration peak of C=C on the hybrid structure skeleton is at 1403 cm -1 The CN stretching vibration peak appeared at 1220 cm -1 、1050cm -1The stretching vibration peaks of naphthalene ring and sulfonic acid group appeared respectively.

[0025] Embodiment 2: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.55 g of graphene oxide (GO) was ultrasonically dispersed in 100 g of deionized water for 1 h to form a GO dispersion; 0.75 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 50 °C for 6 h; 0.5 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated twice to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0026] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 0.75 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 15 min; the suspension is centrifuged at 3000 r / min for 5 min, the supernatant is discarded, and the solid is washed with water twice; the washed white solid is dried at 60°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0027] (3) Weigh 0.3 g of sodium hexadecyl sulfate and 0.5 g of potassium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 50 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.2 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to disperse the mixture for 10 min to obtain a high temperature and alkali-resistant composite nano salt scale inhibitor.

[0028] Embodiment 3: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.6 g of graphene oxide (GO) was ultrasonically dispersed in 120 g of deionized water for 1.5 h to form a GO dispersion; 1.0 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 10 mL / min under stirring conditions, and the reaction was continued at 60 °C for 5 h; 1.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated three times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0029] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 20 min; the suspension is centrifuged at 3000 r / min for 10 min, the supernatant is discarded, and the solid is washed with water twice; the washed white solid is dried at 70°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0030] (3) Weigh 0.1 g of disodium lauryl sulfosuccinate and 0.3 g of sodium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 50 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.2 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to disperse the mixture for 20 min to obtain a high temperature and alkali-resistant composite nano salt scale inhibitor.

[0031] Embodiment 4: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.7 g of graphene oxide (GO) was ultrasonically dispersed in 150 g of deionized water for 1.5 h to form a GO dispersion; 1.25 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 10 mL / min under stirring conditions, and the reaction was continued at 70 °C for 5 h; 1.5 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 2000 r / min for 15 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated three times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0032] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 1.5 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 30 min; the suspension is centrifuged at 3000 r / min for 10 min, the supernatant is discarded, and the solid is washed with water three times; the washed white solid is dried at 70°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0033] (3) Weigh 0.2 g of disodium lauryl sulfosuccinate and 0.3 g of sodium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 60 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.3 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in turn. Use an ultrasonic disperser to disperse the mixture for 20 min to obtain a high temperature and alkali-resistant composite nano salt scale inhibitor.

[0034] Embodiment 5: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.8 g of graphene oxide (GO) was ultrasonically dispersed in 150 g of deionized water for 2 h to form a GO dispersion; 1.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 80 °C for 4 h; 2.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 2000 r / min for 10 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated 3 times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0035] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 30 min; the suspension is centrifuged at 2000 r / min for 20 min, the supernatant is discarded, and the solid is washed with water three times; the washed white solid is dried at 80°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0036] (3) Weigh 0.1 g of sodium hexadecyl sulfate, 0.1 g of disodium lauryl sulfosuccinate, and 0.3 g of potassium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 60 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.3 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in turn. Use an ultrasonic disperser for 30 minutes to prepare a high temperature and alkali-resistant composite nano salt scale inhibitor.

[0037] Embodiment 6: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 1.0 g of graphene oxide (GO) was ultrasonically dispersed in 200 g of deionized water for 2 h to form a GO dispersion; 2.0 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 10 mL / min under stirring conditions, and the reaction was continued at 80 °C for 4 h; 2.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 2000 r / min for 10 min, the upper clear liquid was discarded, and the lower solid was washed with a mixed solution of ethanol and deionized water in a volume ratio of 1:1. This was repeated 3 times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0038] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 1.5 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at 5 mL / min to produce a white suspension, which is continuously stirred for 30 min; the suspension is centrifuged at 2000 r / min for 20 min, the supernatant is discarded, and the solid is washed with water three times; the washed white solid is dried at 80°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0039] (3) Weigh 0.2 g of sodium hexadecyl sulfate, 0.2 g of disodium lauryl sulfosuccinate, and 0.3 g of sodium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 60 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.3 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in turn. Use an ultrasonic disperser for 30 min to prepare a high temperature and alkali resistant composite nano salt scale inhibitor.

[0040] Comparative Example 1: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.5 g of graphene oxide (GO) was ultrasonically dispersed in 100 g of deionized water for 1 h to form a GO dispersion; 0.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 50 °C for 6 h; 0.5 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1, and the washing was repeated twice to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0041] (2) Weigh 0.2 g of sodium hexadecyl sulfate and 0.2 g of potassium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 40 °C in a constant temperature water bath. Then add 0.25 g of modified graphene oxide nano AP-GO powder and disperse the mixture for 10 min using an ultrasonic disperser to obtain a scale inhibitor.

[0042] Comparative Example 2: (1) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: 0.5 g of calcium chloride was dissolved in 100 g of deionized water to form a calcium chloride solution, and 0.5 g of poly (2-acrylamide-2-methylpropanesulfonic acid) (PAMPS) was dissolved in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution was continuously stirred, and the PAMPS solution was added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which was continuously stirred for 15 min; the suspension was centrifuged at 3000 r / min for 15 min, the supernatant was discarded, and the solid was washed with water twice; the washed white solid was dried at 60°C to obtain a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0043] (2) Weigh 0.2 g of sodium hexadecyl sulfate and 0.2 g of potassium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 40°C in a constant temperature water bath. Add 0.25 g of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS powder and disperse the mixture for 10 min using an ultrasonic disperser to obtain a scale inhibitor.

[0044] Comparative Example 3: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.5 g of graphene oxide (GO) was ultrasonically dispersed in 100 g of deionized water for 1 h to form a GO dispersion; 0.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 50 °C for 6 h; 0.5 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1, and the washing was repeated twice to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0045] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 0.5 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 15 min; the suspension is centrifuged at 3000 r / min for 15 min, the supernatant is discarded, and the solid is washed with water twice; the washed white solid is dried at 60°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0046] (3) Weigh 0.4 g of sodium hexadecyl sulfate and dissolve it in 100 mL of deionized water. Heat the mixture to 40 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.2 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to disperse the mixture for 20 min to obtain a high temperature and alkali-resistant composite nano salt scale inhibitor.

[0047] Comparative Example 4: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.5 g of graphene oxide (GO) was ultrasonically dispersed in 100 g of deionized water for 1 h to form a GO dispersion; 0.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 50 °C for 6 h; 0.5 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1, and the washing was repeated twice to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0048] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 0.5 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 15 min; the suspension is centrifuged at 3000 r / min for 15 min, the supernatant is discarded, and the solid is washed with water twice; the washed white solid is dried at 60°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0049] (3) Weigh 0.4 g of potassium chloride and dissolve it in 100 mL of deionized water. Heat the mixture to 40°C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.2 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to disperse the mixture for 20 min to obtain a scale inhibitor.

[0050] Comparative Example 5: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.6 g of graphene oxide (GO) was ultrasonically dispersed in 120 g of deionized water for 1.5 h to form a GO dispersion; 1.0 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 10 mL / min under stirring conditions, and the reaction was continued at 60 °C for 5 h; 1.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated three times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0051] (2) Weigh 0.1 g of disodium lauryl sulfosuccinate and 0.3 g of sodium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 50° C. in a constant temperature water bath. Add 0.25 g of modified graphene oxide nano AP-GO powder and disperse the mixture for 20 min using an ultrasonic disperser to obtain a scale inhibitor.

[0052] Comparative Example 6: (1) Preparation of calcium-based nano-modifier Ca-PAMPS: 0.5 g of calcium chloride was dissolved in 100 g of deionized water to form a calcium chloride solution, and 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) was dissolved in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution was continuously stirred, and the PAMPS solution was added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which was continuously stirred for 20 min; the suspension was centrifuged at 3000 r / min for 10 min, the supernatant was discarded, and the solid was washed with water twice; the washed white solid was dried at 70°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0053] (2) Weigh 0.1 g of disodium lauryl sulfosuccinate and 0.3 g of sodium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 50°C in a constant temperature water bath. Add 0.25 g of calcium-based nano-modifier calcium-based polysulfonic acid (Ca-PAMPS) powder and disperse the mixture for 20 minutes using an ultrasonic disperser to obtain a scale inhibitor.

[0054] Comparative Example 7: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.6 g of graphene oxide (GO) was ultrasonically dispersed in 120 g of deionized water for 1.5 h to form a GO dispersion; 1.0 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 10 mL / min under stirring conditions, and the reaction was continued at 60 °C for 5 h; 1.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated three times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0055] (2) Preparation of calcium-based nano-modifier Ca-PAMPS: 0.5 g of calcium chloride was dissolved in 100 g of deionized water to form a calcium chloride solution, and 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) was dissolved in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution was continuously stirred, and the PAMPS solution was added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which was continuously stirred for 20 min; the suspension was centrifuged at 3000 r / min for 10 min, the supernatant was discarded, and the solid was washed with water twice; the washed white solid was dried at 70°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0056] (3) Weigh 0.4 g of disodium lauryl sulfosuccinate and dissolve it in 100 mL of deionized water. Heat the mixture to 50 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.2 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to disperse the mixture for 20 min to obtain a scale inhibitor.

[0057] Comparative Example 8: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.6 g of graphene oxide (GO) was ultrasonically dispersed in 120 g of deionized water for 1.5 h to form a GO dispersion; 1.0 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 10 mL / min under stirring conditions, and the reaction was continued at 60 °C for 5 h; 1.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 1000 r / min for 20 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated three times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0058] (2) Preparation of calcium-based nano-modifier Ca-PAMPS: 0.5 g of calcium chloride was dissolved in 100 g of deionized water to form a calcium chloride solution, and 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) was dissolved in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution was continuously stirred, and the PAMPS solution was added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which was continuously stirred for 20 min; the suspension was centrifuged at 3000 r / min for 10 min, the supernatant was discarded, and the solid was washed with water twice; the washed white solid was dried at 70°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0059] (3) Weigh 0.4 g of sodium chloride and dissolve it in 100 mL of deionized water. Heat the mixture to 50° C. in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.2 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to disperse the mixture for 20 min to obtain a scale inhibitor.

[0060] Comparative Example 9: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.8 g of graphene oxide (GO) was ultrasonically dispersed in 150 g of deionized water for 2 h to form a GO dispersion; 1.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 80 °C for 4 h; 2.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 2000 r / min for 10 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated 3 times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0061] (2) Weigh 0.1 g of sodium hexadecyl sulfate, 0.1 g of disodium lauryl sulfosuccinate, and 0.3 g of potassium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 60° C. in a constant temperature water bath. Add 0.35 g of modified graphene oxide nano AP-GO powder and use an ultrasonic disperser for 30 minutes to prepare a scale inhibitor.

[0062] Comparative Example 10: (1) Preparation of calcium-based nano-modifier Ca-PAMPS: 0.5 g of calcium chloride was dissolved in 100 g of deionized water to form a calcium chloride solution, and 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) was dissolved in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution was continuously stirred, and the PAMPS solution was added to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which was continuously stirred for 30 min; the suspension was centrifuged at 2000 r / min for 20 min, the supernatant was discarded, and the solid was washed with water three times; the washed white solid was dried at 80°C to obtain a Ca-PAMPS solid.

[0063] (3) Weigh 0.1 g of sodium hexadecyl sulfate, 0.1 g of disodium lauryl sulfosuccinate, and 0.3 g of potassium chloride and dissolve them in 100 mL of deionized water. Heat the mixture to 60°C in a constant temperature water bath, then add 0.35 g of Ca-PAMPS powder and use an ultrasonic disperser for 30 minutes to prepare a high temperature and alkali resistant composite nanoscale scale inhibitor.

[0064] Comparative Example 11: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.8 g of graphene oxide (GO) was ultrasonically dispersed in 150 g of deionized water for 2 h to form a GO dispersion; 1.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 80 °C for 4 h; 2.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 2000 r / min for 10 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated 3 times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0065] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 30 min; the suspension is centrifuged at 2000 r / min for 20 min, the supernatant is discarded, and the solid is washed with water three times; the washed white solid is dried at 80°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0066] (3) Weigh 0.25 g of sodium hexadecyl sulfate and 0.25 g of disodium lauryl sulfosuccinate and dissolve them in 100 mL of deionized water. Heat the mixture to 60 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.3 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in turn. Use an ultrasonic disperser for 30 min to prepare a scale inhibitor.

[0067] Comparative Example 12: (1) Preparation of modified graphene oxide nanoparticles AP-GO: 0.8 g of graphene oxide (GO) was ultrasonically dispersed in 150 g of deionized water for 2 h to form a GO dispersion; 1.5 g of 3-amino-1,2-propanediol (AP) was added to the GO dispersion at 5 mL / min under stirring conditions, and the reaction was continued at 80 °C for 4 h; 2.0 g of sodium chloride was added to the reaction mixture and stirred for dispersion, and then centrifuged at 2000 r / min for 10 min, the upper clear liquid was discarded, and the lower solid was washed with a mixture of ethanol and deionized water in a volume ratio of 1:1. This was repeated 3 times to obtain 3-amino-1,2-propanediol modified graphene oxide nanoparticles (AP-GO).

[0068] (2) Preparation of calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS: Take 0.5 g of calcium chloride and dissolve it in 100 g of deionized water to form a calcium chloride solution, take 1.2 g of poly (2-acrylamide-2-methylpropane sulfonic acid) (PAMPS) and dissolve it in 100 g of deionized water to form a PAMPS solution; the calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 10 mL / min to produce a white suspension, which is continuously stirred for 30 min; the suspension is centrifuged at 2000 r / min for 20 min, the supernatant is discarded, and the solid is washed with water three times; the washed white solid is dried at 80°C to form a Ca-PAMPS solid, which is the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

[0069] (3) Weigh 0.5 g of potassium chloride and dissolve it in 100 mL of deionized water. Heat the mixture to 60 °C in a constant temperature water bath. Then add 0.05 g of modified graphene oxide nano AP-GO powder and 0.3 g of calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS powder in sequence. Use an ultrasonic disperser to prepare a scale inhibitor for 30 min.

[0070] Performance comparison: The scale inhibition effect comparison experiment was conducted on the scale inhibitors in Examples 1 to 6 and Comparative Examples 1 to 12 and commercially available products (sodium polyepoxysuccinate and sodium polyaspartate). Test method: prepare 5000mg / L calcium chloride solution, add different concentrations (10mg / L, 20mg / L, 40mg / L) of scale inhibitor, and then mix it with simulated formation brine (10001.6mg / L potassium ion, 76000.0mg / L sodium ion, 54.3mg / L calcium ion, 68.3mg / L magnesium ion, 75179.7mg / L chloride ion, 11825.0mg / L sulfate, 36377.7mg / L bicarbonate, total mineralization 209506.5mg / L, pH=8.3) in a ratio of 1:1, place the solution in a constant temperature drying oven at 100℃ and 150℃ for 24h, take it out and test the scale inhibition rate. The specific results are shown in Table 1 and Table 2 respectively.

[0071] Table 1 Comparison of antiscalant stability and antiscaling rate at 100℃ .

[0072] Table 2 Test results of scale inhibition rate of different scale inhibitor concentrations (150℃) .

[0073] From the comparison test results in Table 1, it can be seen that the high temperature resistant composite nano-scale inhibitor of the embodiment of the present invention has excellent scale inhibition effect. At 100°C and the same concentration, the scale inhibition rates of the modified graphene oxide nano AP-GO and the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS nanofluid scale inhibitor are respectively lower than 40% and 70%. The scale inhibition rate and stability of the modified graphene oxide nano AP-GO, calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS, surfactant, and inorganic salt are greatly reduced. The scale inhibition rate of the high temperature resistant composite nano-scale inhibitor in the embodiment is within the range of 10-40 mg / L, and the scale inhibition rate is greater than 80%, and the highest can reach 94.2%, indicating that the various substances in the components have obvious synergistic scale inhibition and synergistic effects. At the same time, the addition of inorganic salts can improve the product stability to more than 90 days. As can be seen from Table 2, the temperature resistant composite nano-scale inhibitor described in Examples 1 to 6 can reach a temperature of 150°C when the dosage is appropriately increased, and also has a good scale inhibition effect.

[0074] In summary, the present invention discloses a high temperature resistant composite nanofluid scale inhibitor and a preparation method thereof, and belongs to the technical field of oilfield chemistry; the composite nanofluid scale inhibitor is prepared from modified graphene oxide nano AP-GO, calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS, surfactant, inorganic salt and deionized water; the calcium-based nano modifier calcium-based polysulfonic acid contains a large amount of sulfonic acid, carboxylic acid and hydroxyl groups, has strong hydrophilicity, calcium ion tolerance and calcium ion chelation, and has good scale inhibition effect on calcium carbonate scale and barium sulfate scale; at the same time, the modified graphene oxide nano has a large-scale conjugated ring, a large amount of carboxylic acid and hydroxyl groups, and synergizes with the calcium-based polysulfonic acid in anion shielding and large steric effect, and the modified graphene oxide nano, calcium-based polysulfonic acid, surfactant and inorganic salt are used to synergistically improve the high temperature resistance and scale inhibition performance of the nano scale inhibitor, has good scale inhibition effect, effectively solves the scaling problem of oilfield water injection and fracturing flowback, and has good promotion prospects.

[0075] At this point, those skilled in the art recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the contents disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.

Claims

1. A high temperature resistant composite nanofluid scale inhibitor, characterized in that: The composite nanofluid antiscalant comprises: Modified graphene oxide nano AP-GO, calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS, surfactant, inorganic salt and water; The mass concentration of the modified graphene oxide nano AP-GO in the scale inhibitor is 0.01-0.1%; The mass concentration of the surfactant in the scale inhibitor is 0.1 to 0.4%; The mass concentration of the inorganic salt in the scale inhibitor is 0.3 to 0.5%; The mass ratio of the modified graphene oxide nano AP-GO to the calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS is 1:4 to 1:6; The inorganic salt is one or more of potassium chloride and sodium chloride; The surfactant is one or more of sodium dodecylbenzene sulfonate, sodium hexadecyl sulfate, sodium hexadecyl sulfonate, sodium lauryl polyoxyethylene ether sulfate and disodium lauryl sulfosuccinate.

2. A high temperature resistant composite nanofluid antiscalant as claimed in claim 1, characterized in that: The structural formula of the modified graphene oxide nano AP-GO is: 。 3. A high temperature resistant composite nanofluid antiscalant as claimed in claim 1, characterized in that: The water is deionized water; the surfactant is sodium hexadecyl sulfonate and disodium lauryl sulfosuccinate.

4. A high temperature resistant composite nanofluid antiscalant as claimed in claim 1, characterized in that: The specific preparation method of the modified graphene oxide nano AP-GO is: 0.5-1.0 g of graphene oxide GO is ultrasonically dispersed in 100-200 g of deionized water for 1-2 h to form a GO dispersion; 3-amino-1,2-propylene glycol AP is added to the GO dispersion at 5-10 mL / min under stirring conditions, and the reaction is continued at 50-80° C. for 4-6 h; 0.5-2 g of sodium chloride is added to the reaction mixture, stirred and dispersed, and then centrifuged at 1000-2000 r / min for 10-20 min, the upper clear liquid is discarded, and the lower solid is washed, and the process is repeated 2-3 times to obtain 3-amino-1,2-propylene glycol-modified graphene oxide nano AP-GO; the preparation method reaction formula is as follows: 。 5. A high temperature resistant composite nanofluid antiscalant as claimed in claim 4, characterized in that: The mass ratio of the graphene oxide GO to 3-amino-1,2-propylene glycol AP is 1:1 to 1:

4.

6. A high temperature resistant composite nanofluid antiscalant as claimed in claim 4, characterized in that: The lower solid layer was washed with a mixture of ethanol and deionized water in a volume ratio of 1:

1.

7. A high temperature resistant composite nanofluid antiscalant as claimed in claim 1, characterized in that: The specific preparation method of the calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS is as follows: Calcium chloride is dissolved in water to form a calcium chloride solution, wherein the mass concentration of the calcium chloride solution is 0.1-1%; Dissolve poly (2-acrylamide-2-methylpropanesulfonic acid) (PAMPS) in water to form a PAMPS solution, wherein the mass concentration of the PAMPS solution is 0.5 to 1.5%; The calcium chloride solution is continuously stirred, and the PAMPS solution is added dropwise to the calcium chloride solution at a rate of 5 to 10 mL / min to produce a white suspension, which is continuously stirred for 15 to 30 min; the suspension is centrifuged at 1000 to 3000 r / min for 5 to 20 min, the supernatant is discarded, and the solid is washed with water for 2 to 3 times; the washed white solid is dried at 50-80° C. to prepare a Ca-PAMPS solid, which is a calcium-based nano-modifier calcium-based polysulfonic acid Ca-PAMPS.

8. A high temperature resistant composite nanofluid antiscalant as claimed in claim 7, characterized in that: The mass ratio of the calcium chloride to poly (2-acrylamide-2-methylpropane sulfonic acid) PAMPS is 1:1 to 1:

3.

9. The high temperature resistant composite nanofluid antiscalant according to claim 1, characterized in that: The preparation method of the scale inhibitor is specifically as follows: The modified graphene oxide nano AP-GO and the calcium-based nano modifier calcium-based polysulfonic acid Ca-PAMPS are mixed with an inorganic salt, a surfactant and water according to the concentration and mass ratio, and then heated at 40 to 60° C. and ultrasonically dispersed for 10 to 30 minutes to obtain the high-temperature resistant composite nanofluid scale inhibitor.

Citation Information

Patent Citations

  • A high-temperature resistant scale inhibitor and its preparation method

    CN114920367B

  • Thermally-induced association type scale inhibitor, alkaline scale inhibition polymer fracturing fluid system and preparation method of thermally-induced association type scale inhibitor and alkaline scale inhibition polymer fracturing fluid system

    CN117362658A

  • Application of calcium and magnesium scale inhibitor prepared by sewage in tertiary oil recovery

    CN109181668A

  • Graphene scale inhibition composite filter core and preparation method thereof

    CN110496449A

  • Low-alkali scale inhibitor and preparation method thereof

    CN110776115A

Cited By

  • Multifunctional anti-scale supramolecular fracturing fluid system for unconventional oil reservoir and application of multifunctional anti-scale supramolecular fracturing fluid system

    CN121555171A