Utilization method of tail gas in production of bamboo activated carbon and production method of bamboo activated carbon

By condensing, solid-liquid separation, membrane separation, extraction and reduced pressure distillation of bamboo activated carbon production, the problem of failure to effectively utilize the exhaust gas is solved, and efficient extraction of biomass oil and efficient utilization of bamboo resources are achieved.

CN120079195APending Publication Date: 2025-06-03成都达奇科技股份有限公司
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510114849.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-24
Publication Date
2025-06-03

AI Technical Summary

Technical Problem

The exhaust gas generated during bamboo activated carbon production cannot be effectively utilized, resulting in waste of resources and low bamboo resource utilization.

Method used

By condensing, solid-liquid separation, membrane separation, extraction and reduced pressure distillation of the bamboo activated carbon production exhaust gas, the organic matter in the exhaust gas is successfully converted into high-calorie biomass oil.

Benefits of technology

It increases the overall added value of bamboo activated carbon, maximizes the use of the energy and chemical composition of bamboo raw materials, reduces resource waste, and increases the economic benefits of the company.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120079195A_ABST
    Figure CN120079195A_ABST
Patent Text Reader

Abstract

The invention discloses a bamboo activated carbon production tail gas utilization method and a bamboo activated carbon production method.The utilization method comprises the following steps that production tail gas is subjected to condensation treatment, and condensate is obtained; carrying out solid-liquid separation treatment on the condensate to obtain permeate; carrying out membrane separation treatment on the permeate liquid by adopting a nanofiltration membrane to obtain oily liquid; performing extraction treatment on the oily liquid by adopting an extraction agent to obtain an extraction agent soluble liquid; and carrying out reduced pressure distillation treatment on the extractant soluble liquid to obtain the biomass oil. By means of condensation treatment, solid-liquid separation treatment, membrane separation treatment, extraction treatment and distillation treatment, organic matter steam in carbonized tail gas is converted into biomass oil with a high calorific value (HHV), the overall additional value of bamboo activated carbon is increased, energy and chemical components of bamboo raw materials are utilized to the maximum extent, resource waste is reduced, and environmental protection is achieved. And economic benefits of enterprises are increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of bamboo activated carbon production, and specifically, to a method for utilizing the tail gas in bamboo activated carbon production and a method for producing bamboo activated carbon. Background Art

[0002] Biomass energy is the fourth-largest energy source after coal, oil, and natural gas. Biomass energy is the energy carried by biomass, usually from firewood, straw, livestock manure, and municipal waste, etc. Modern technologies usually convert these biomasses into solid, liquid, or gaseous fuels for utilization. Bamboo energy is an important form of biomass energy, with the advantages of low pollution, wide distribution, large reserves, and renewability. China is the country with the richest bamboo resources in the world, possessing favorable conditions and environment for the development of bamboo energy.

[0003] Currently, an important use of bamboo resources in China is for the preparation of bamboo activated carbon. The preparation process mainly includes a carbonization process and an activation process, and the carbonization process can be one or two times. Secondary carbonization usually means that the primary carbonized material obtained from the first carbonization is ground, kneaded, and granulated into special shapes such as columns, honeycombs, spheres, etc., and then secondary carbonization is carried out to remove the binder used in granulation. In addition to a large amount of tail gas generated during the activation process, both the first carbonization process and the secondary carbonization process will also generate relatively more tail gas, and the components of the tail gas generated by the two carbonizations are significantly different.

[0004] In the tail gas generated by the first carbonization, in addition to the protective gas and water vapor, the main components are CO, CO 2 generated by the pyrolysis of biomass components (such as lignin and hemicellulose, etc.), H 2 , volatile organic compounds (such as alkanes, alkenes, aldehydes, etc.), organic vapors (such as terpenes, tannic acid, methanol, etc.), acidic gases (such as formic acid, phenol, acetic acid, H 2 S, SO 2 , NH 3 , nitrogen oxides, etc.).

[0005] The tail gas generated by the secondary carbonization varies greatly depending on the type of binder. For example, the main components of the secondary carbonization tail gas with traditional asphalt or coal tar as the binder are protective gas, water vapor, CO, CO 2 , volatile organic compounds (such as benzene, toluene, xylene, methylphenol, ethylphenol, etc.), and acidic gases (such as phenol, formic acid, acetic acid, aldehydes, nitrogen oxides, etc.), which are highly toxic. When using polymer binders (such as starch, molasses, carboxymethyl cellulose, lignin, gelatin, chitosan, etc.), the content of volatile organic compounds and acidic gases in the secondary carbonization tail gas is significantly reduced, and the main components are protective gas, water vapor, CO, and CO 2 .

[0006] During the activation process, the activator reacts with carbon elements, resulting in the erosion of pores and the formation of a large number of micropores. In addition to the protective gas and the activator (such as water vapor, CO 2 , O 2 ), the main components of the resulting activation waste gas also include H 2 , CO, a small amount of volatile organic compounds (such as CH 4 , C 2 H 4 , propylene), and acidic gases (such as phenol).

[0007] If the tail gas generated during the carbonization process and the activation process can be converted into clean energy, the utilization rate of bamboo resources can be significantly improved. Chinese invention patent CN116332128A discloses a system for preparing methanol by co-producing high-quality activated carbon from biomass and its preparation method. This method directly conducts a water-gas shift reaction on the tail gas generated during the activation process, and then conducts a CO hydrogenation reaction to finally obtain methanol. On the one hand, a large amount of tail gas generated during the carbonization process is not recycled. On the other hand, directly conducting a synthesis reaction on the activation tail gas not only easily causes catalyst poisoning but also results in a relatively low purity of methanol. Summary of the Invention

[0008] The technical problem to be solved by the present invention is to provide a simple and efficient method and system for utilizing the tail gas of bamboo-based activated carbon production that can convert the tail gas of bamboo-based activated carbon production into clean energy, as well as a production method and production system for bamboo-based activated carbon.

[0009] To achieve the above object, according to the first aspect of the present invention, there is provided a method and system for utilizing the tail gas of bamboo-based activated carbon production, and the technical solution is as follows:

[0010] A method for utilizing the tail gas of bamboo-based activated carbon production, wherein the production tail gas at least includes the carbonization tail gas generated by carbonizing bamboo raw materials, and the utilization method includes the following steps:

[0011] Conduct condensation treatment on the production tail gas to obtain condensate;

[0012] Conduct solid-liquid separation treatment on the condensate to obtain a permeate;

[0013] Conduct membrane separation treatment on the permeate using a nanofiltration membrane to obtain an oily liquid;

[0014] Conduct extraction treatment on the oily liquid using an extractant to obtain an extractant-soluble liquid;

[0015] Conduct vacuum distillation treatment on the extractant-soluble liquid to obtain bio-oil.

[0016] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: The condensation treatment is divided into two stages. First, condensation is carried out at 70 - 100 °C, and then at 40 - 60 °C.

[0017] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: The permeate is subjected to vacuum filtration treatment with a vacuum degree of 50 - 200 mmHg, a temperature of 35 - 45 °C, and the pore size of the nanofiltration membrane is 1 - 10 nm.

[0018] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: The extractant is ethanol and / or acetone; the volume of the extractant is 1.5 - 2 times the volume of the condensate.

[0019] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: The vacuum distillation treatment is carried out at 45 - 55 °C and 15 - 18 kPa; it also includes reusing the condensate obtained from the vacuum distillation treatment for extracting the oily liquid.

[0020] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: It also includes distilling the biomass oil into a solid at normal pressure at 200 - 250 °C. The utilization method also includes crushing, grinding, and vacuum drying the solid to obtain solid-state biomass oil.

[0021] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: It also includes distilling the biomass oil into a concentrated liquid at normal pressure at 200 - 250 °C. The utilization method also includes hydrorefining the concentrated liquid, including the steps of: preparing a reaction solution according to the mass ratio of biomass oil: methanol: catalyst = (15 - 25):(20 - 30):1, and carrying out hydrothermal reaction at 180 - 200 °C and 1 MPa hydrogen pressure for 2 - 4 h to obtain refined biomass oil.

[0022] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: An activated carbon-based Ni / BC catalyst is used, and its preparation method is: dispersing soluble nickel salt and activated carbon in ethanol and stirring for 4 - 6 h; rotating and evaporating completely at 80 °C to remove the ethanol solvent and then drying in a vacuum oven; calcining at 500 - 600 °C for 1 - 3 h under a reducing atmosphere to obtain the activated carbon-based Ni / BC catalyst.

[0023] As a further improvement to the above method for utilizing the tail gas from bamboo-based activated carbon production: When the bamboo raw material is subjected to segmented carbonization treatment, the production tail gas at least includes the segmented tail gas generated during carbonization treatment at 300 - 400 °C.

[0024] Utilization system for the tail gas in the production of bamboo-based activated carbon, including a carbonization furnace for carbonizing bamboo raw materials to obtain carbonization tail gas. The utilization system includes: a condensation device for condensing the production tail gas and outputting condensate; a solid-liquid separation device for performing solid-liquid separation on the condensate and outputting permeate; the liquid inlet of the solid-liquid separation device is connected to the liquid outlet of the condensation device; a membrane separation device for performing membrane separation on the permeate and outputting oily liquid; the membrane used in the membrane separation device is a nanofiltration membrane; the liquid inlet of the membrane separation device is connected to the liquid outlet of the solid-liquid separation device; an extraction device for extracting the oily liquid and outputting extractant-soluble liquid; the liquid inlet of the extraction device is connected to the oily liquid outlet of the membrane separation device; a first-stage distillation device for performing vacuum distillation on the extractant-soluble liquid and outputting biomass oil; the liquid inlet of the first-stage distillation device is connected to the extractant-soluble liquid outlet of the extraction device.

[0025] As a further improvement of the above utilization system for the tail gas in the production of bamboo-based activated carbon: the solid-liquid separation device is a filtration device or a centrifugal separation device.

[0026] As a further improvement of the above utilization system for the tail gas in the production of bamboo-based activated carbon: the membrane separation device is a vacuum filtration device using nanofiltration membrane sheets.

[0027] As a further improvement of the above utilization system for the tail gas in the production of bamboo-based activated carbon: it further includes a delivery pipeline for inputting extractant into the extraction device; it further includes a reflux pipeline for returning the condensate distilled by the first-stage distillation device to the extraction device.

[0028] As a further improvement of the above utilization system for the tail gas in the production of bamboo-based activated carbon: it further includes a second-stage distillation device for performing atmospheric distillation on the biomass oil; the liquid inlet of the second-stage distillation device is connected to the liquid outlet of the first-stage distillation device.

[0029] As a further improvement of the above utilization system for the tail gas in the production of bamboo-based activated carbon: the second-stage distillation distills the biomass oil into a solid, and the utilization system further includes a crushing device, a grinding device, and a drying device for successively crushing, grinding, and vacuum drying the solid.

[0030] As a further improvement of the above utilization system for the tail gas in the production of bamboo-based activated carbon: the second-stage distillation distills the biomass oil into a concentrated liquid, and the utilization system further includes a hydrothermal reaction device for refining the concentrated liquid.

[0031] To achieve the above object, according to the second aspect of the present invention, there is provided a method and a system for producing bamboo activated carbon by using the method and system for utilizing the tail gas generated in the production of bamboo activated carbon described in the first aspect above. The technical solutions are as follows:

[0032] A method for producing bamboo activated carbon includes carbonizing bamboo raw materials, and further includes utilizing the production tail gas by using the method for utilizing the tail gas generated in the production of bamboo activated carbon described in the first aspect above. The production tail gas at least includes the carbonization tail gas generated by carbonizing bamboo raw materials;

[0033] The carbonization treatment at least includes a primary carbonization treatment, including the steps of:

[0034] Put the dried bamboo raw materials into a carbonization furnace, and under an inert atmosphere, raise the furnace temperature from room temperature to 130 - 280 °C and keep it warm for 0.5 - 1.5 hours;

[0035] Continue to raise the temperature to 300 - 400 °C and keep it warm for 0.5 - 1.5 hours;

[0036] Continue to raise the temperature to 500 - 600 °C, keep it warm for 0.5 - 1.5 hours and then cool it with the furnace to obtain the primary carbonized material; after the carbonization is completed, activation treatment can be carried out to obtain bamboo activated carbon.

[0037] A preparation system for the tail gas generated in the production of bamboo activated carbon includes a carbonization furnace for carbonizing bamboo raw materials, and further includes utilizing the production tail gas by using the system for utilizing the tail gas generated in the production of bamboo activated carbon described in the first aspect above. The production tail gas at least includes the carbonization tail gas generated by carbonizing bamboo raw materials.

[0038] Biomass oil is an important resource and has uses such as fuel, chemical raw material, and energy storage. The present invention effectively utilizes the organic matter generated by the pyrolysis of the biomass component of bamboo raw materials during carbonization, and by using simple and efficient purification means, through condensation treatment, solid-liquid separation treatment, membrane separation treatment, extraction treatment, and distillation treatment, converts the organic matter vapor in the carbonization tail gas into biomass oil with a high heating value (HHV), improves the overall added value of bamboo activated carbon, maximally utilizes the energy and chemical components of bamboo raw materials, reduces resource waste, and increases the economic benefits of the enterprise.

[0039] The following further describes the embodiments of the invention provided in this specification in conjunction with the accompanying drawings and specific implementation manners. The additional aspects and advantages of the embodiments of the invention provided in this specification will be partially given in the following description, partially become obvious from the following description, or be understood through the practice of the embodiments of the invention provided in this specification. Description of the Drawings

[0040] The accompanying drawings, which form a part of the embodiments of the invention provided in this specification, are used to assist in understanding the embodiments of the invention provided in this specification. The content provided in the accompanying drawings and the explanations related to them in the embodiments of the invention provided in this specification can be used to explain the embodiments of the invention provided in this specification, but do not constitute an improper limitation to the embodiments of the invention provided in this specification. In the accompanying drawings:

[0041] Figure 1 It is a schematic structural diagram of the first embodiment of the bamboo-based activated carbon production system and the utilization system of the tail gas from bamboo-based activated carbon production.

[0042] Figure 2 It is a schematic structural diagram of the second embodiment of the bamboo-based activated carbon production system and the utilization system of the tail gas from bamboo-based activated carbon production.

[0043] Figure 3 It is the XRD pattern of the Cu-Zr catalyst.

[0044] The relevant markings in the above-mentioned accompanying drawings are as follows:

[0045] 210 - Condensing equipment, 220 - Solid-liquid separation equipment, 230 - Membrane separation equipment, 240 - Extraction equipment, 250 - First-stage distillation equipment, 260 - Second-stage distillation equipment. Detailed implementation manners

[0046] The following clearly and completely describes the embodiments of the invention provided in this specification with reference to the accompanying drawings. Those of ordinary skill in the art will be able to implement the embodiments of the invention provided in this specification based on these descriptions. Before describing the embodiments of the invention provided in this specification with reference to the accompanying drawings, it should be particularly noted that:

[0047] In the embodiments of the invention provided in this specification, the technical solutions and technical features provided in each part including the following descriptions can be combined with each other without conflict.

[0048] In addition, the embodiments of the invention provided in this specification involved in the following descriptions are usually only a partial embodiment rather than all embodiments of the embodiments of the invention provided in this specification. Therefore, all other embodiments obtained by those of ordinary skill in the art based on the embodiments of the invention provided in this specification without creative efforts should fall within the scope of protection of the embodiments of the invention provided in this specification.

[0049] Regarding the terms and units in the embodiments of the invention provided in this specification: In the specification, claims, and relevant parts of the embodiments of the invention provided in this specification, the terms "comprising", "including", "having", and any variations thereof are intended to cover non-exclusive inclusion. In addition, other relevant terms and units in the embodiments of the invention provided in this specification can be reasonably explained based on the relevant content of the embodiments of the invention provided in this specification.

[0050] The first embodiment of the method for producing bamboo-based activated carbon of the present invention includes the steps:

[0051] Drying treatment: Put the fresh bamboo raw materials into an oven and dry them at 100°C for 48 hours.

[0052] Primary carbonization treatment: Put the dried bamboo raw materials into a carbonization furnace. Under an inert atmosphere, raise the furnace temperature from room temperature to 200°C and keep it warm for 1 hour; continue to raise the temperature to 350°C and keep it warm for 1 hour; continue to raise the temperature to 550°C, keep it warm for 1 hour, and then cool it with the furnace to obtain carbonized materials.

[0053] Activation treatment: Put the carbonized materials into an activation furnace. Under an inert atmosphere, use water vapor as the activator. The volume of liquid water introduced per 100 g of the green body per hour is 40 mL. Keep it warm at 1000°C for 3 hours and then cool it with the furnace to obtain bamboo-based activated carbon.

[0054] Compared with the first embodiment, the difference of the second embodiment of the method for producing bamboo-based activated carbon of the present invention is that it further includes a secondary carbonization treatment: Grind the primary carbonized materials to a particle size of 325 mesh, then use molasses as the binder and water as the auxiliary agent. According to the mass ratio of molasses to the primary carbonized materials being 0.5 and adding 30 mL of the auxiliary agent per 100 g of the primary carbonized materials, granulate them into green bodies in a kneader. Put the green bodies into a carbonization furnace. Under an inert atmosphere, raise the furnace temperature from room temperature to 550°C, keep it warm for 1 hour, and cool it with the furnace to obtain secondary carbonized materials. Then perform activation treatment on the secondary carbonized materials to obtain bamboo-based activated carbon.

[0055] The method for utilizing the production tail gas of bamboo-based activated carbon of the present invention is used to utilize the production tail gas generated by the method for producing bamboo-based activated carbon described in the above first embodiment or second embodiment. The production tail gas at least includes the segmented tail gas generated during carbonization treatment at 300 - 400°C. For example, the production tail gas can only include the segmented tail gas generated during carbonization treatment at 300 - 400°C, or can include all the primary carbonization tail gas, and can further include secondary carbonization tail gas and / or activation tail gas.

[0056] The first embodiment of the method for utilizing the production tail gas of bamboo-based activated carbon includes the following steps:

[0057] The production tail gas is subjected to condensation treatment to obtain condensate; preferably, the condensation treatment is divided into two stages. First, condensation is carried out at 85 °C, and then at 50 °C. In this way, as much organic vapor as possible can be condensed.

[0058] The condensate is subjected to solid-liquid separation treatment to obtain a permeate; the solid-liquid separation treatment is filtration treatment or centrifugal separation treatment. Thus, particulate impurities captured by droplets during the condensation process can be removed.

[0059] The permeate is subjected to membrane separation treatment using a nanofiltration membrane to obtain an oily liquid; preferably, the membrane separation treatment is vacuum filtration treatment of the permeate, with a vacuum degree of 100 mmHg, a temperature of 40 °C, and the pore size of the nanofiltration membrane being 5 nm. Thus, water can pass through the nanofiltration membrane, while most of the organic substances are effectively intercepted, and most of the organic substances are enriched in the oily liquid.

[0060] The oily liquid is subjected to extraction treatment using an extractant to obtain an extractant-soluble liquid; preferably, the extractant is ethanol and / or acetone; the volume of the extractant is 2 times the volume of the condensate.

[0061] The extractant-soluble liquid is subjected to vacuum distillation treatment at 50 °C and 16 kPa to obtain bio-oil. Through the vacuum distillation treatment, the extractant can be evaporated and condensed, and the condensate obtained from the vacuum distillation treatment can be reused for the extraction treatment of the oily liquid, which can improve the utilization rate of the extractant.

[0062] The second embodiment of the method for utilizing the production tail gas of bamboo charcoal-based activated carbon is: on the basis of the first embodiment, it further includes atmospheric distilling the bio-oil into a solid at 200 - 250 °C (preferably 235 °C), and the utilization method further includes crushing, grinding, and vacuum drying the solid, and then solid bio-oil is obtained.

[0063] The third embodiment of the method for utilizing the production tail gas of bamboo charcoal-based activated carbon is: on the basis of the first embodiment, it further includes atmospheric distilling the bio-oil into a concentrated liquid at 200 - 250 °C (preferably 235 °C), and the utilization method further includes hydrorefining treatment of the concentrated liquid, including the steps of: preparing a reaction solution according to the mass ratio of bio-oil:methanol:catalyst of 20:25:1, and carrying out hydrothermal reaction at 190 °C and 1 MPa hydrogen pressure for 3 h, and then refined bio-oil is obtained.

[0064] An activated carbon-based Ni / BC catalyst is used, and its preparation method is: dispersing 0.5 g of nickel nitrate and 1 g of activated carbon in ethanol, and stirring for 5 h; rotating and evaporating completely at 80 °C to remove the ethanol solvent and then drying in a vacuum oven; using 20% H 2 -Ar as the reducing atmosphere, and calcining at 550 °C for 2 h, and then the activated carbon-based Ni / BC catalyst is obtained.

[0065] Figure 1 This is a schematic structural diagram of the first embodiment of a bamboo-based activated carbon production system and a utilization system for the tail gas of bamboo-based activated carbon production. As Figure 1 shown, the bamboo-based activated carbon production system includes a carbonization furnace (one or two) for carbonizing bamboo raw materials to obtain carbonization tail gas and a utilization system for the production tail gas. The production tail gas at least includes the segmented tail gas generated by carbonization treatment at 300-400 °C. For example, the production tail gas can only include the segmented tail gas generated by carbonization treatment at 300-400 °C, or can include all the primary carbonization tail gas, and can further include secondary carbonization tail gas and activation tail gas.

[0066] The first embodiment of the utilization system for the tail gas of bamboo-based activated carbon production includes a condensation device 210, a solid-liquid separation device 220, a membrane separation device 230, an extraction device 240, and a primary distillation device 250.

[0067] The condensation device 210 is used to condense the production tail gas and output condensate. The solid-liquid separation device 220 is used to perform solid-liquid separation on the condensate and output the permeate. The liquid inlet of the solid-liquid separation device 220 is connected to the liquid outlet of the condensation device 210. The solid-liquid separation device 220 is a filtration device or a centrifugal separation device. The membrane separation device 230 is used to perform membrane separation on the permeate and output an oily liquid. The membrane separation device 230 is a vacuum filtration device using a nanofiltration membrane. The liquid inlet of the membrane separation device 230 is connected to the liquid outlet of the solid-liquid separation device 220. The extraction device 240 is used to extract the oily liquid and output an extractant-soluble liquid. The liquid inlet of the extraction device 240 is connected to the oily liquid outlet of the membrane separation device 230. The primary distillation device 250 is used to perform vacuum distillation on the extractant-soluble liquid and output bio-oil. The liquid inlet of the primary distillation device 250 is connected to the extractant-soluble liquid outlet of the extraction device 240.

[0068] The utilization system further includes a delivery pipeline for inputting an extractant into the extraction device 240 and a reflux pipeline for returning the condensate distilled by the primary distillation device 250 to the extraction device 240.

[0069] After testing, the obtained bio-oil contains 53.57% O, 37.65% C, 7.61% H, and 1.17% N.

[0070] Figure 2 This is a schematic structural diagram of the second embodiment of a bamboo-based activated carbon production system and a utilization system for the tail gas of bamboo-based activated carbon production. As Figure 2As shown, compared with the first embodiment, the utilization system of the second embodiment further includes a secondary distillation device 260 for subjecting bio-oil to atmospheric distillation; the liquid inlet of the secondary distillation device 260 is connected to the liquid outlet of the primary distillation device 250.

[0071] When the secondary distillation device 260 distills bio-oil into a solid, the utilization system further includes a crushing device, a milling device, and a drying device for successively crushing, grinding, and vacuum-drying the solid. Thus, the resulting solid bio-oil is more convenient for storage, transportation, and use.

[0072] When the secondary distillation device 260 distills bio-oil into a concentrated liquid, the utilization system further includes a hydrothermal reaction device for refining the concentrated liquid. Thus, through hydrotreating, the C / O and H / O ratios can be further increased, and the HHV value can be further improved.

[0073] After the secondary distillation device 260 performs atmospheric distillation, the C content of the bio-oil continuously increases from 37.65% to 57.74%, the O content continuously decreases from 53.57% to 34.72%, the H content decreases from 7.61% to 6.05%, and the N content remains basically unchanged. It can be seen that through atmospheric distillation, the C / O and H / O ratios increase, resulting in a significant improvement in the HHV value.

[0074] After condensing the carbonization tail gas, the non-condensable gas still contains resources such as CO, H 2 , CO 2 etc. In order to deeply recover the valuable resources in the production tail gas, the utilization method of the bamboo-based activated carbon production tail gas of the present invention further utilizes the non-condensable gas. On the basis of the third embodiment, its fourth embodiment further includes the steps:

[0075] For the non-condensable gas after condensing the production tail gas, it is purified to remove volatile organic compounds, acidic gases, and particulate impurities in the non-condensable gas. The purification treatment includes successively performing dust removal treatment, adsorption treatment, and deacidification treatment on the production tail gas. Among them, the dust removal treatment is preferably filtration dust removal. The volatile organic compounds in the production tail gas can be adsorbed through adsorption treatment, and activated carbon is preferably used as the adsorbent. The residual acidic gases in the production tail gas can be removed through deacidification treatment, and the deacidification treatment preferably uses a spray tower for wet deacidification, and the deacidification is performed by circulating and spraying a liquid absorbent. Thus, the volume fraction content of water vapor in the production tail gas obtained through purification treatment is 15-25%, the COD content ≤ 5 ppm, the volatile organic compound content ≤ 3 ppm, the acidic gas content ≤ 2 ppm, and the particulate matter content ≤ 20 mg / Nm 3 .

[0076] Use a CO 2 selective separation membrane to remove CO from the production tail gas2 , and then introduce the production tail gas into a reaction device containing a Cu-Zr catalyst, and carry out a catalytic reaction at 240-300 °C to generate syngas containing H 2 . The CO 2 selective separation membrane is used to remove CO from the syngas 2 .

[0077] Among them, the preparation method of the Cu-Zr catalyst includes the following steps:

[0078] Dissolve zirconium nitrate and urea in 150 mL of deionized water to form an aqueous solution. The molar ratio of urea to zirconium ions in the aqueous solution is 2, and the zirconium ion concentration is 0.2 mol / L; carry out hydrothermal treatment on the aqueous solution. The hydrothermal reaction temperature is 150 °C, and the hydrothermal reaction duration is 24 hours. Collect, wash, and dry the generated first solid;

[0079] Carry out calcination treatment on the first solid. The calcination temperature is 250 °C, and the calcination duration is 4 hours to obtain a zirconium precursor;

[0080] Grind and mix the zirconium precursor and copper nitrate. The molar ratio of copper ions to zirconium ions (calculated according to zirconium nitrate) is 0.12; then disperse the ground mixture in 200 mL of deionized water to form a dispersion. Stir for 2 hours under the water bath condition with a water bath temperature of 60 °C, and continue to slowly add sodium hydroxide to the dispersion under the water bath condition until the pH of the dispersion = 9. Collect, wash, and dry the generated second solid;

[0081] Carry out calcination treatment on the second solid. The calcination temperature is 400 °C, and the calcination duration is 4 hours to obtain the Cu-Zr catalyst.

[0082] Figure 3 is the XRD pattern of the Cu-Zr catalyst. As Figure 3 shown, the Cu-Zr catalyst has a good crystal form, and its XRD pattern has characteristic peaks of CuO x and ZrO 2 , indicating that Cu is not embedded in the zirconium precursor (ZrO 2 ) during the preparation process, but is uniformly attached to the surface of ZrO 2 in the form of CuOx, and through the interaction between the two, a good catalytic effect is produced.

[0083] Through N 2 adsorption-desorption experiment and BET (Brunauer-Emmett-Teller) method, the specific surface area of the zirconium precursor (ZrO 2 ) is 37.35 m 2 / g, and the total pore volume is 0.22 cm 3 / g, the average pore size is 23.6 nm, and the specific surface area of the Cu-Zr catalyst is 56.48 m 2 / g, and the total pore volume is 0.30 cm 3 / g, with an average pore size of 21.8 nm. It can be seen that after loading CuO x , the specific surface area of the Cu-Zr catalyst has increased significantly, which plays a decisive role in the adsorption and activation of gases.

[0084] Mix a gas mixture with a volume fraction of 15% CO, 40% H 2 , 35% N 2 , 10% CO 2 with water vapor, and use the Cu-Zr catalyst for catalysis at 180 - 300 °C. The results show that the CO conversion rate first increases sharply and then gradually levels off with the increase of the catalytic temperature. The corresponding CO conversion rates at 180 °C, 210 °C, 240 °C, 270 °C, and 300 °C are 62%, 79%, 85%, 86%, and 87% respectively.

[0085] Use this Cu-Zr catalyst to catalyze the reaction gas for removing CO 2 (data of one embodiment is: 21.54% CO, 3.14% CO 2 , 23.55% H 2 , 22.35% water vapor, and the balance is N 2 ), the reaction temperature is 270 °C, the reaction pressure is 5 MPa, and the space velocity is 5000 h -1 , and the CO conversion rate is 81%.

[0086] Different from the fourth embodiment, the fifth embodiment of the utilization method of the tail gas from bamboo-based activated carbon production is as follows:

[0087] Condense the second tail gas and the third tail gas to obtain the second non-condensable gas.

[0088] The mixed gas composed of the first non-condensable gas obtained by condensing the first tail gas and the second non-condensable gas is purified to obtain a reaction gas; the purification treatment includes successively performing acid removal treatment, dust removal treatment, and adsorption treatment on the mixed gas; wherein, the acid removal treatment adopts dry acid removal, that is, spraying a solid absorbent for acid removal. Thus, through the acid removal treatment, the residual acid gas in the mixed gas can be removed and a relatively dry low-acid gas can be obtained, avoiding the influence of the introduction of more water vapor by wet acid removal on the methanol synthesis reaction; the dust removal treatment is preferably filtration dust removal. Setting dust removal after the acid removal treatment can not only remove the particulate impurities carried by the mixed gas, but also remove the acid removal agent used in the acid removal treatment. Through the adsorption treatment, volatile organic compounds in the mixed gas can be adsorbed, and activated carbon is preferably used as the adsorbent. Thus, through the purification treatment, particulate impurities, volatile organic compounds, and residual acid gas can be removed. The reaction gas obtained after the mixed gas is purified contains mainly CO 2 、CO and mainly, the volume fraction of water vapor is 2-5%, the COD content ≤ 5 ppm, the volatile organic compound content ≤ 3 ppm, the acid gas content ≤ 2 ppm, and the particulate matter content ≤ 20 mg / Nm 3 .

[0089] Use a CO 2 selective separation membrane to remove CO in the reaction gas 2 , and then pass the reaction gas and H 2 into a reaction device loaded with a multi-layer structured catalyst for catalytic reaction to generate synthesis gas containing methanol.

[0090] The core of the multi-layer structured catalyst is Fe 3 O 4 , the inner layer is CeO 2 , the middle layer is a Cu-Zn alloy, the outer layer is ZrO 2 , and the surface layer is graphene quantum dots. Its preparation method includes the following steps:[[]]

[0091] Preparation of the Fe 3 O 4 core by coprecipitation: Using FeCl 3 ·6H 2 O, FeCl 2 ·4H 2 O and ammonia water as raw materials, under nitrogen protection, mixing equal volumes of Fe 3+ solution and Fe 2+ solution, Fe 3+ and Fe 2+The molar ratio is 2:1; the mixed solution is heated to 80 °C, and ammonia water is added to the mixed solution to a pH of 10 - 11 at a stirring speed of 500 rpm; after reacting for another 30 minutes, magnetic separation is carried out, and the collected solid is washed 3 times with deionized water and ethanol, and dried in vacuum at 60 °C for 12 hours to obtain Fe 3 O 4 core.

[0092] Preparation of CeO by hydrothermal method 2 Inner layer: Dissolve Ce(NO 3 ) 3 ·6H 2 O and urea in water, the concentration of Ce 3+ is 0.05 M, and the concentration of urea is 0.5 M; Disperse 1 g of Fe 3 O 4 core in 150 mL of the above solution, transfer to a hydrothermal reactor, and react at 180 °C for 12 hours; After cooling to room temperature, centrifugal separation is carried out, and the collected solid is washed 3 times with water and ethanol, dried at 60 °C for 12 hours, and then calcined at 350 °C for 2 hours, that is, CeO 3 O 4 is coated on the surface of the Fe 2 core to obtain CeO 2 @Fe 3 O 4 .

[0093] Preparation of Cu-Zn alloy intermediate layer by chemical reduction method: Dissolve Cu(NO 3 ) 2 ·3H 2 O, Zn(NO 3 ) 2 ·6H 2 O in water, the concentration of Cu 2+ is 0.1 M, and the concentration of Zn 2+ is 0.05 M; Disperse 0.8 g of CeO 2 @Fe 3 O 4 in 100 mL of the above solution and sonicate for 30 minutes; Stir in an ice bath and slowly add NaBH 4 solution (concentration 0.2 M) until a precipitate forms; Then stir at room temperature for 2 hours and then carry out centrifugal separation, and the collected solid is washed 3 times with water and ethanol and dried in vacuum at 50 °C for 8 hours, that is, a Cu-Zn alloy intermediate layer is deposited on the surface of the CeO 2 inner layer to obtain Cu-Zn@CeO 2 @Fe 3 O 4 .

[0094] Preparation of ZrO by sol-gel method2 Outer layer: Dissolve Zr(OC 4 H 9 ) 4 in ethanol, with the concentration of Zr(OC 4 H 9 ) 4 being 0.1 M; Add a small amount of water (the molar ratio of water to Zr = 2) and 0.6 g of Cu-Zn@CeO 2 @Fe 3 O 4 to 100 mL of the above solution, stir at room temperature for 4 hours; then reflux at 60 °C for 2 hours, followed by centrifugation, dry at 80 °C for 12 hours, and then calcine at 450 °C for 3 hours, thus coating the surface of the Cu-Zn alloy intermediate layer with a ZrO 2 outer layer to obtain ZrO 2 @Cu-Zn@CeO 2 @Fe 3 O 4 .

[0095] Preparation of graphene quantum dots (GQDs) by impregnation method: Prepare an aqueous solution of GQDs with a concentration of 1 mg / mL; then disperse 0.5 g of ZrO 2 @Cu-Zn@CeO 2 @Fe 3 O 4 in 100 mL of the GQDs aqueous solution; sonicate for 30 minutes, then stir at room temperature for 4 hours, followed by centrifugation, and dry in vacuum at 50 °C for 12 hours, thus loading graphene quantum dots on the surface of the ZrO 2 outer layer to obtain GQDs@ZrO 2 @Cu-Zn@CeO 2 @Fe 3 O 4 .

[0096] Calcination treatment: In air, calcine GQDs@ZrO 2 @Cu-Zn@CeO 2 @Fe 3 O 4 at 450 °C for 4 hours to obtain a precursor.

[0097] Reduction treatment: In a mixed gas atmosphere of N 2 and H 2 with the volume fraction of H 2 being 10%, reduce the precursor at 350 °C for 2 hours to obtain the catalyst.

[0098] Use this multi-layer structured catalyst to remove CO 2The reaction gas (one set of example data is: 25.41% CO, 3.05% CO 2 , 26.21% H 2 , 2.45% water vapor, with the balance being N 2 ) is catalyzed. The volume ratio of the reaction gas to the supplementary H 2 is (4.05 - 4.5):1. The reaction temperature is 240 °C (any temperature from 220 to 300 °C is acceptable), the reaction pressure is 4 MPa (any pressure from 3 to 10 MPa is acceptable), the space velocity is 6000 h -1 (any value from 3000 to 10000 h -1 is acceptable), the space - time yield is 0.2 - 0.6 kg methanol / (L catalyst·h), and the purity of the liquid methanol is above 95%.

[0099] Different from the fifth embodiment, the sixth embodiment of the utilization method of the tail gas from bamboo - based activated carbon production is as follows:

[0100] For the non - condensable gas after condensing the carbonization tail gas, it is successively subjected to de - acidification treatment, dust removal treatment, and adsorption treatment to obtain the first reaction gas and the adsorption - saturated liquid; among them, the de - acidification treatment adopts dry de - acidification, that is, spraying a solid absorbent for de - acidification. Thus, through the de - acidification treatment, the residual acidic gas in the carbonization tail gas can be removed and relatively dry low - acid gas can be obtained, avoiding the influence of introducing more water vapor by wet de - acidification on the methanol synthesis reaction; the dust removal treatment is preferably filtration dust removal. Setting dust removal after de - acidification treatment can not only remove the particulate impurities carried by the carbonization tail gas, but also remove the de - acidifying agent used in the de - acidification treatment. The adsorption treatment uses alcohol as the adsorbent, which can adsorb the volatile organic compounds in the carbonization tail gas and form the first reaction gas and the adsorption - saturated liquid.

[0101] The adsorption - saturated liquid is subjected to combustion treatment to obtain combustion tail gas; since the adsorption - saturated liquid mainly contains volatile organic compounds, burning it can not only prevent environmental pollution caused by emissions, but also generate more CO 2 for reaction with methane.

[0102] The combustion tail gas and methane are introduced into the first reaction device loaded with a catalyst for catalytic reaction, and the reaction generates a second reaction gas containing H 2 and CO.

[0103] The activation tail gas is successively subjected to condensation treatment, de - acidification treatment, dust removal treatment, and adsorption treatment to obtain the third reaction gas; since the volatile organic compounds in the activation tail gas are relatively less, here the adsorption treatment can be carried out by using activated carbon for adsorption.

[0104] The mixed gas composed of the first reaction gas, the second reaction gas, and the third reaction gas and H 2It is introduced into a second reaction device loaded with a catalyst (the above-mentioned multi-layer structure catalyst) for catalytic reaction to generate syngas containing methanol; among them, the volume fraction of water vapor in the mixed gas is 2-5%, the COD content is ≤5 ppm, the volatile organic compound content is ≤3 ppm, the acid gas content is ≤2 ppm, and the particulate matter content is ≤20 mg / Nm 3 。

[0105] The catalyst in the first reaction device is a perovskite-type nickel-based composite catalyst. Soluble cerium salts and zirconium salts are dissolved in deionized water, and the molar ratio of cerium ions to zirconium ions is 1; ammonia water is added dropwise to the solution under stirring until the pH is 9-10; then stirring is continued for 2 h, and aging is carried out at 80 °C for 2 hours; after collecting, washing and drying the solid, it is calcined in air at 600 °C for 4 hours to obtain CeO 2 -ZrO 2 support;

[0106] Soluble lanthanum salts, soluble strontium salts, soluble nickel salts, soluble ferric salts and soluble ruthenium salts are weighed according to the molar ratio of La, Sr, Ni, Fe, Ru of 0.8:0.2:0.7:0.2:0.1 and dissolved in deionized water; according to the molar ratio of metal ions to citric acid of 1:1.5, an appropriate amount of citric acid is added to the solution; stirring and evaporation are carried out at 80 °C until a gel is formed; the gel is dried at 120 °C for 12 hours to obtain a perovskite precursor;

[0107] The perovskite precursor and CeO 2 -ZrO 2 support are weighed according to the perovskite precursor loading of 20%, dispersed in a small amount of ethanol and mixed evenly; after stirring and evaporating the ethanol at 80 °C, it is first dried at 110 °C, and then calcined in air at 900 °C for 6 hours to form a perovskite structure, and finally reduced in a mixed atmosphere of H 2 and Ar at 700 °C for 2 hours to obtain a perovskite-type nickel-based composite catalyst.

[0108] Using this perovskite-type nickel-based composite catalyst to catalyze combustion exhaust gas (the volume fraction composition of one embodiment is: 5.68% CO, 74.32% CO 2 、1.54% H 2 、2.14% water vapor, and the balance is N 2 ) and methane, the volume ratio of combustion exhaust gas to methane is (1.05-1.5):1, the reaction temperature is 700 °C, the reaction pressure is 0.1 MPa, and the space velocity is 20000 h -1 ,CO 2 conversion rate is 81%.

[0109] Using the above multi-layer structured catalyst to catalyze the mixed gas (data of one embodiment: 39.65% CO, 2.56% CO 2 , 38.56% H 2 , 2.68% water vapor, and the balance is N 2 ), the volume ratio of the mixed gas to the supplementary H 2 is (2.05 - 2.5):1, the reaction temperature is 240°C (any temperature in the range of 220 - 300°C is acceptable), the reaction pressure is 4 MPa (any pressure in the range of 3 - 10 MPa is acceptable), the space velocity is 6000 h -1 (any space velocity in the range of 3000 - 10000 h -1 is acceptable), the space-time yield is 0.4 - 0.9 kg methanol / (L catalyst·h), and the purity of the liquid methanol is above 95%.

[0110] The above has described the relevant content of the embodiments of the invention provided in this specification. Those of ordinary skill in the art will be able to implement the embodiments of the invention provided in this specification based on these descriptions. Based on the above content of the embodiments of the invention provided in this specification, all other preferred embodiments and examples obtained by those of ordinary skill in the art without creative efforts shall fall within the scope of protection of the embodiments of the invention provided in this specification.

Claims

1. A method for utilizing tail gas produced by bamboo activated carbon, wherein the tail gas produced at least comprises carbonized tail gas generated by carbonizing bamboo raw materials, characterized in that: The exploitation method includes the following steps: Condensing the production tail gas to obtain condensate; Performing solid-liquid separation on the condensate to obtain a permeate; The permeate is subjected to membrane separation treatment using a nanofiltration membrane to obtain an oily liquid; The oily liquid is extracted by using an extractant to obtain an extractant-soluble liquid; The extractant-soluble liquid is subjected to reduced pressure distillation to obtain biomass oil.

2. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 1, characterized in that: The condensation process is divided into two stages, firstly condensation is carried out at 70-100°C, and then condensation is carried out at 40-60°C.

3. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 1, characterized in that: The permeate is subjected to vacuum filtration treatment, the vacuum degree is 50-200 mmHg, the temperature is 35-45°C, and the pore size of the nanofiltration membrane is 1-10 nm.

4. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 1, characterized in that: The extractant is ethanol and / or acetone; the volume of the extractant is 1.5 to 2 times the volume of the condensate.

5. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 1, characterized in that: The reduced pressure distillation treatment is carried out at 45-55°C and 15-18 kPa; and the condensate obtained from the reduced pressure distillation treatment is repeatedly used for extraction treatment of the oily liquid.

6. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 1, characterized in that: The method also includes distilling the biomass oil into solid at 200-250° C. under normal pressure. The utilization method also includes crushing, grinding and vacuum drying the solid to obtain solid biomass oil.

7. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 1, characterized in that: The method also includes distilling the biomass oil at 200-250°C under normal pressure into a concentrated liquid. The utilization method also includes performing a hydrogenation refining treatment on the concentrated liquid, including the steps of preparing a reaction liquid according to a mass ratio of biomass oil: methanol: catalyst of (15-25): (20-30): 1, and performing a hydrothermal reaction at 180-200°C and 1MPa hydrogen pressure for 2-4h to obtain refined biomass oil.

8. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 7, characterized in that: An activated carbon-based Ni / BC catalyst is used, and its preparation method is as follows: dispersing soluble nickel salt and activated carbon in ethanol, stirring for 4 to 6 hours; rotary evaporating at 80°C to completely remove the ethanol solvent and then drying in a vacuum oven; calcining at 500 to 600°C for 1 to 3 hours under a reducing atmosphere to obtain an activated carbon-based Ni / BC catalyst.

9. The method for utilizing tail gas produced by bamboo activated carbon production as claimed in claim 1, characterized in that: When the bamboo raw material is subjected to a segmented carbonization treatment, the produced tail gas at least includes segmented tail gas generated by the carbonization treatment at 300-400°C.

10. A method for producing bamboo activated carbon, comprising carbonizing bamboo raw materials, characterized in that: The method further comprises utilizing the production tail gas of bamboo activated carbon according to any one of claims 1 to 9, wherein the production tail gas at least comprises carbonized tail gas generated by carbonizing bamboo raw materials; The carbonization treatment includes at least one carbonization treatment, including the steps of: Put the dried bamboo raw material into the carbonization furnace, and raise the furnace temperature from room temperature to 130-280°C in an inert atmosphere, and keep it warm for 0.5-1.5 hours; Continue to raise the temperature to 300-400°C and keep it warm for 0.5-1.5 hours; Continue to raise the temperature to 500-600°C, keep warm for 0.5-1.5 hours, and then cool with the furnace to obtain the primary carbonized material; after the carbonization is completed, activate the material to obtain bamboo activated carbon.

Citation Information

Patent Citations

  • System for preparing methanol and co-producing high-quality activated carbon from biomass and preparation method thereof

    CN116332128A