Microcrystalline glass powder composition for packaging mica window GM counter as well as preparation method and application of microcrystalline glass powder composition
By designing a microcrystalline glass powder composition containing components such as Bi2O3 and ZnO, the problem of insufficient thermal expansion coefficient and wettability of mica window GM counter packaging materials in the prior art is solved, and a higher airtightness and more accurate packaging effect is achieved.
Patent Information
- Application Number
- CN202510237990.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-28
- Publication Date
- 2025-06-03
AI Technical Summary
In the prior art, the microcrystalline glass powder for packaging of mica window GM counters is difficult to take into account the appropriate thermal expansion coefficient, glass transition temperature, expansion softening temperature and good wetting with various substrates, and cannot meet the special sealing requirements of mica window GM counters.
A microcrystalline glass powder composition for mica window GM counter packaging is designed, including 70 to 90 parts of Bi2O3, 2 to 15 parts of ZnO, 1 to 12 parts of B2O3, 1 to 8 parts of BaO, 0.2 to 7 parts of Al2O3, 0.1 to 5 parts of CuO, 0.1 to 5 parts of K2O, 0.1 to 5 parts of Li2O3, 0.1 to 5 parts of La2O3, 0.1 to 8 parts of CeO2 and 0 to 5 parts of oxidizing agent. By optimizing the component ratio and preparation process, it is ensured that it has an appropriate thermal expansion coefficient and wettability.
The mica window GM counter is achieved with higher airtightness and more precise packaging, extending the service life of the equipment and meeting the demand for lead-free and high-performance packaging materials.
Smart Images

Figure BDA0005294025200000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sealing glass, and in particular, to a glass-ceramic powder for encapsulating a mica window GM counter, a preparation method thereof, and an application thereof. Background Art
[0002] A gas counter, also known as a Geiger counter or GM counter, is a detector with a gaseous working substance, and its function is to specifically detect ionizing radiation particles. A mica window GM counter is a special structure Geiger counter designed to detect low-energy γ-rays, β-rays, and α-rays. Its detection surface is sealed with an extremely thin mica sheet as a detection window, and the other surfaces are all metal structures, which can partially shield the influence of environmental γ-rays on the measurement results. At the same time, its top exhaust pipe is a glass tube, and the structure for fixing the anode wire is a ceramic material. The connection of the above three materials, namely the mica window thin sheet, the glass charging and exhaust pipe, and the ceramic column, to the metal shell is all achieved through high-temperature sintering of a glass solder.
[0003] During the assembly process of a mica window GM counter, it is necessary to seal the metal shell, ceramic column, charging and exhaust glass tube, and mica window to achieve the connection between the metal shell and the ceramic column, charging and exhaust glass tube, and mica window respectively. During its assembly and sintering process, there are at least two stages, and it is required to finally encapsulate the mica sheet. When sealing, the sealing material is required to have good airtightness to avoid leakage of the charged high-pressure gas; in addition, the sealing material should also have a good glass transition temperature and expansion softening temperature to maintain the performance of the sealing material after charging high-pressure gas; at the same time, the sealing material should have a good expansion coefficient to avoid cracks or breakage of the mica window due to the difference in thermal expansion coefficient between the mica window and the sealing material, thereby affecting the transparency of the mica window and reducing the sealing performance.
[0004] In response to the above problems, currently known glass materials that are used as sealing materials for mica window GM counters and have good effects are all lead-containing glass materials, which do not meet the development requirements of lead-free electronic products. At the same time, the existing glass powders for sealing are also difficult to balance an appropriate thermal expansion coefficient, an appropriate glass transition temperature, an appropriate softening expansion temperature, and good wettability with various substrates, and are difficult to meet the special sealing requirements of mica window GM counters.
[0005] Based on this, how to design a glass-ceramic powder for encapsulation according to the special sealing requirements of a mica window GM counter so that it has a more appropriate thermal expansion coefficient, a more appropriate glass transition temperature and expansion softening temperature, and at the same time can have good wettability with ceramics, glass, mica sheets, and metals, thereby making the mica window GM counter encapsulated with it have higher airtightness is one of the important technical problems to be solved in this field. Summary of the Invention
[0006] The main object of the present invention is to provide a glass-ceramic powder for encapsulating mica-window GM counters, a preparation method thereof, and an application thereof, so as to solve the problem that the glass-ceramic powder for encapsulation in the prior art fails to have a more suitable thermal expansion coefficient, a more suitable glass transition temperature and softening temperature of expansion, and it is difficult to have good wettability with ceramics, glass, mica sheets and metals, and thus it is difficult to meet the special sealing requirements of mica-window GM counters.
[0007] To achieve the above object, a first aspect of the present invention provides a glass-ceramic powder composition for encapsulating mica-window GM counters. By weight, the glass-ceramic powder composition for encapsulating mica-window GM counters comprises 70-90 parts of Bi 2 O 3 , 2-15 parts of ZnO, 1-12 parts of B 2 O 3 , 1-8 parts of BaO, 0.2-7 parts of Al 2 O 3 , 0.1-5 parts of CuO, 0.1-5 parts of K 2 O, 0.1-5 parts of Li 2 O, 0.1-5 parts of La 2 O 3 , 0.1-8 parts of CeO 2 and 0-5 parts of an oxidizing agent; the oxidizing agent is nitrate and / or nitrite, and the cations in the nitrate and / or nitrite are each independently selected from one or more of ammonium ions, bismuth ions, zinc ions, barium ions, aluminum ions, copper ions, potassium ions, lithium ions, lanthanum ions and cerium ions.
[0008] Further, the oxidizing agent is selected from one or more of Bi(NO 3 ) 3 ·5H 2 O, Ba(NO 3 ) 2 , KNO 3 , KNO 2 , NH 4 NO 3 and NH 4 NO 2 , preferably Bi(NO 3 ) 3 ·5H 2 O.
[0009] Further, in the glass-ceramic powder composition for encapsulating mica-window GM counters, Bi 2 O 3 and B 2 O 3The weight ratio is (7.5 to 45):1; and / or, in the glass-ceramic powder composition for encapsulating mica window GM counter, the weight ratio of ZnO to BaO is (1 to 5):1.
[0010] Further, by weight parts, the glass-ceramic powder composition for encapsulating mica window GM counter comprises 75 to 85 parts of Bi 2 O 3 , 5 to 13 parts of ZnO, 2 to 10 parts of B 2 O 3 , 1 to 5 parts of BaO, 0.5 to 5 parts of Al 2 O 3 , 0.1 to 3 parts of CuO, 0.1 to 3 parts of K 2 O, 0.1 to 3 parts of Li 2 O, 0.1 to 3 parts of La 2 O 3 , 0.1 to 5 parts of CeO 2 and 0.1 to 3 parts of oxidant; preferably, by weight parts, the glass-ceramic powder composition for encapsulating mica window GM counter comprises 75 to 78 parts of Bi 2 O 3 , 5 to 7 parts of ZnO, 2 to 10 parts of B 2 O 3 , 1.5 to 5 parts of BaO, 0.5 to 2 parts of Al 2 O 3 , 0.1 to 1 part of CuO, 0.1 to 3 parts of K 2 O, 1 to 3 parts of Li 2 O, 0.1 to 1 part of La 2 O 3 , 0.5 to 5 parts of CeO 2 and 0.1 to 1 part of Bi(NO 3 ) 3 ·5H 2 O.
[0011] Further, the particle size D50 of the glass-ceramic powder composition for encapsulating mica window GM counter is 1.0 μm to 5.0 μm, preferably 1.5 μm to 2.5 μm; and / or, the expansion coefficient α 30 / 300 of the glass-ceramic powder composition for encapsulating mica window GM counter is 90×10 -7 / ℃ to 110×10 -7 / ℃, preferably 95×10 -7 / ℃ to 105×10 -7 / °C; and / or, the glass transition temperature of the glass-ceramic powder composition for encapsulating mica window GM counter is 400°C to 450°C, preferably 410°C to 430°C; and / or, the expansion softening temperature of the glass-ceramic powder composition for encapsulating mica window GM counter is 420°C to 480°C, preferably 430°C to 460°C; and / or, the crystallization temperature of the glass-ceramic powder composition for encapsulating mica window GM counter is 520°C to 620°C, preferably 580°C to 600°C.
[0012] The second aspect of the present invention provides a preparation method of the above-mentioned glass-ceramic powder composition for encapsulating mica window GM counter, comprising: Step S1, mixing the raw materials of the glass-ceramic powder composition for encapsulating mica window GM counter to obtain a mixture; Step S2, subjecting the mixture to melting and rolling in sequence to obtain a rolled material; Step S3, subjecting the rolled material to ball milling and screening in sequence to obtain the glass-ceramic powder composition for encapsulating mica window GM counter.
[0013] Further, in Step S2, the melting is carried out at 850°C to 1200°C until the mixture is melted; and / or, the temperature of the rolling roll used for rolling is 5°C to 30°C; preferably, the melting is carried out at 900°C to 1000°C until the mixture is melted; and / or, the temperature of the rolling roll used for rolling is 10°C to 25°C.
[0014] Further, in Step S3, the rotation speed of the ball milling is 100 rap / min to 500 rap / min, and the time is 0.5 h to 3 h.
[0015] The third aspect of the present invention provides a mica window GM counter, comprising a metal housing, a ceramic column, an air charging and discharging glass tube, and a mica sheet, and the connections between the metal housing and the ceramic column, between the metal housing and the air charging and discharging glass tube, and between the metal housing and the mica sheet are all realized by coating and sintering a sealing glass, and the sealing glass is the above-mentioned glass-ceramic powder composition for encapsulating mica window GM counter.
[0016] Further, the assembly process of the mica window GM counter includes the following steps carried out in sequence: preparing a bonding slurry with a viscosity of 100000 CP to 200000 CP by mixing the glass-ceramic powder composition for encapsulating mica window GM counter and an organic solvent; coating the bonding slurry at the connection between the metal housing and the air charging and discharging glass tube, and forming a first seal after the first sintering; coating the bonding slurry at the connection between the metal housing and the ceramic column, and forming a second seal after the second sintering; coating the bonding slurry at the connection between the metal housing and the mica sheet, and forming a third seal after the third sintering; preferably, the air tightness of the mica window GM counter is 2.0×10 -9 Pa·m 3 / s to 10 -8 Pa·m3 / s.
[0017] Applying the technical solution of the present invention, by optimizing the specific components and the corresponding component contents of the glass-ceramic powder composition, it has excellent thermal stability and chemical compatibility, and at the same time has a more suitable thermal expansion coefficient, a more suitable glass transition temperature and softening temperature of expansion. It has good wettability with various materials such as ceramics, glass, mica sheets and metals, and thus can be used as an excellent encapsulation material for mica window GM counters, improving the airtightness of mica window GM counters. Specific Embodiments
[0018] It should be noted that, without conflict, the embodiments in the present application and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the embodiments.
[0019] As described in the background art, the existing glass-ceramic powder for encapsulation fails to have a more suitable thermal expansion coefficient, a more suitable glass transition temperature and softening temperature of expansion, and at the same time it is difficult to have good wettability with ceramics, glass, mica sheets and metals, and thus it is difficult to meet the special sealing requirements of mica window GM counters. To solve the above technical problems, a first aspect of the present invention provides a glass-ceramic powder composition for encapsulating mica window GM counters. By weight, the glass-ceramic powder composition for encapsulating mica window GM counters includes 70-90 parts of Bi 2 O 3 , 2-15 parts of ZnO, 1-12 parts of B 2 O 3 , 1-8 parts of BaO, 0.2-7 parts of Al 2 O 3 , 0.1-5 parts of CuO, 0.1-5 parts of K 2 O, 0.1-5 parts of Li 2 O, 0.1-5 parts of La 2 O 3 , 0.1-8 parts of CeO 2 and 0-5 parts of oxidant; the oxidant is nitrate and / or nitrite, and the cations in the nitrate and / or nitrite are independently selected from one or more of ammonium ion, bismuth ion, zinc ion, barium ion, aluminum ion, copper ion, potassium ion, lithium ion, lanthanum ion and cerium ion.
[0020] Regarding the mica window GM counter, there are mainly three parts involving the encapsulation glass during the assembly process: the connection between the mica window and the metal housing, the connection between the glass filling exhaust pipe and the metal housing, and the connection between the ceramic component and the metal housing. The encapsulation sequence of these connection parts is crucial for the correct assembly and performance of the counter, and generally follows the following process sequence:
[0021] First, the sealing of the filling exhaust pipe and the metal housing: In the assembly process of the GM counter, the first step is usually to seal the glass exhaust pipe and the metal housing. The purpose of this step is to provide a channel for the subsequent process of filling halogen gas after evacuation, and at the same time ensure that the already sealed exhaust pipe will not remelt or be affected during the subsequent encapsulation process, so as to maintain the integrity and airtightness of its structure. This sealing is usually carried out when the glass is melted and has a certain fluidity, satisfying that the glass completely wets the sealing interface and will not cause the glass filling exhaust pipe to soften and deform, so as to meet the need for a more stable connection for the encapsulation of the exhaust pipe to withstand the air pressure change inside the counter.
[0022] Second, the sealing of the ceramic component and the metal housing: The next step is to seal the ceramic component, that is, the ceramic tube with the anode plate fixing hole, and the metal housing. The ceramic component plays a role in fixing and supporting the anode plate and isolating the anode plate from the metal housing to achieve insulation. When sealing, it is necessary to ensure good electrical insulation and mechanical stability between them and the metal housing. Note that in order to simplify the process and reduce costs, the sealing processes of step one and step two can be carried out simultaneously.
[0023] Third, the sealing of the mica window and the metal housing: This is the last and most crucial step in the encapsulation of the GM counter. As the radiation detection window, the mica window must be thin and transparent, but it cannot melt or deform during the sealing process, otherwise the detection performance will be affected. Therefore, usually after the sealing of the exhaust pipe and the ceramic component is completed, a specific lead-free microcrystalline sealing glass powder is used to seal the mica window. This process requires that the sealing glass powder will not affect the previously sealed parts during the melting and sealing process, such as the secondary melting of the glass at the previously sealed parts resulting in the dislocation and detachment of the glass tube or ceramic tube, thus affecting the overall airtightness, and at the same time ensuring the physical integrity of the mica window. After one sintering, it will become crystalline glass, and the temperature required for the re-melting of this state of glass is 50 - 100 °C higher than the melting temperature of the crystal, and this special property just matches the special process requirements of the mica window GM counter.
[0024] In the above process sequence, this staged sealing strategy is to ensure that each sealing step can be carried out under optimal conditions, avoid damaging the already sealed components at high temperatures, and at the same time ensure that each connection point can achieve the required electrical insulation, airtightness, and mechanical stability. Especially for the mica window GM counter, its sensitive structure requires the sealing material to have a high degree of adjustability and compatibility to adapt to the connection requirements of different materials. Therefore, in view of this situation, the present invention specifically designs the formula of the glass powder composition, and by precisely controlling the composition ratio of the above glass powder composition, it is ensured that the glass-ceramic powder has a more suitable thermal expansion coefficient, a more suitable glass transition temperature and softening temperature of expansion, and has good wettability with various materials such as ceramics, glass, mica sheets, and metals, so as to meet the special packaging requirements of the mica window GM counter. Specifically, in the above formula:
[0025] 70 to 90 parts of Bi 2 O 3 In the formed glass powder composition, bismuthate is provided, which, as one of the main network formers, significantly reduces the melting point and viscosity of the glass, making the glass easy to melt and flow, which is crucial for the wettability and sintering performance of the glass powder slurry during the sealing process. At the same time, Bi 2 O 3 also provides a relatively high thermal expansion coefficient, which helps to match the thermal expansion coefficients of sealing materials such as metals and ceramics. 2 to 15 parts of ZnO are used to provide zincate, which, as a network modifier, can adjust the viscosity and melting point of the glass and improve the chemical stability of the glass. 1 to 12 parts of B 2 O 3 helps to form an amorphous network structure, improve the chemical stability of the glass, and reduce the melting point of the glass. The addition of B 2 O 3 plays an important role in controlling the melting behavior of the glass and improving its wettability with various materials. At the same time, B 2 O 3 and Bi 2 O 3 cooperation can ensure that the glass has good fluidity and sintering performance at a lower temperature, and at the same time also improves the mechanical strength of the glass. 1 to 8 parts of BaO can increase the refractive index and density of the glass, and at the same time improve the electrical insulation and water-resistant chemical stability of the glass; its cooperation with ZnO helps to enhance the mechanical strength and chemical stability of the glass while maintaining good fluidity and sintering performance.
[0026] In addition, the above formula also includes 0.2 to 7 parts of Al 2 O 3 , 0.1 to 5 parts of K 2 O and 0.1 to 5 parts of Li 2O, and the three of them are respectively used as additives to lower the melting point and improve the mechanical properties, thereby improving the wettability of the slurry. Since Li 2 O and K 2 O lower the melting point of the glass, making the slurry more fluid and easier to wet the substrate at a lower temperature. At the same time, the addition of Al 2 O 3 can form a more complex network structure, improve the chemical stability and mechanical strength of the glass, and indirectly enhance its wettability by improving the sintering behavior of the glass powder. 0.1 to 5 parts of CuO can cooperate with other components to help form a more complex glass network structure and thus improve the fluidity of the glass.
[0027] 0.1 to 5 parts of La 2 O 3 and 0.1 to 8 parts of CeO 2 both belong to rare earth metal oxides. They can improve the transparency, radiation resistance and crystallization ability of the glass. At the same time, CeO 2 can also act as an oxidant to help control the redox environment of the glass and prevent excessive crystallization during application and sintering. La 2 O 3 and CeO 2 used in the above dosages can further optimize the mechanical strength and chemical properties of the obtained glass powder after sintering and encapsulation. The function of 0 to 5 parts of the oxidant is to promote the redox reaction of the glass powder during sintering, prevent excessive crystallization, and ensure that the glass powder has good sintering fluidity. At the same time, under appropriate conditions, CeO 2 can partially undertake the function of the oxidant, but the additional oxidant can more effectively control the atmosphere during glass sintering.
[0028] In summary, each component in the formula provided by the present invention has a direct impact on the performance of the glass powder, and their cooperation relationship ensures that the glass powder can meet the requirements of the sealing process, including particularly good wettability, matching thermal expansion coefficient and melting characteristics. By adjusting the ratios of the components as above, the performance of the glass powder can be optimized to meet the special sealing requirements of the mica window GM counter.
[0029] In particular, the above glass powder composition formula provided by the present invention does not include the Sb element, especially the Sb 2 O 3 component. Because the inventor found through a large number of experiments that the addition of Sb 2 O 3 will cause the resistance of the glass powder composition to corrosive media such as acids and alkalis to decrease after sintering, thereby affecting the long-term stability and reliability of the finally obtained package. At the same time, Sb 2 O 3The absorption and re-release of oxygen inhibit the formation of crystals in the glass powder composition system provided by the present invention, which is not conducive to the preparation of glass ceramics.
[0030] In several preferred embodiments, the oxidizing agent is selected from Bi(NO 3 ) 3 ·5H 2 O, Ba(NO 3 ) 2 , KNO 3 , KNO 2 , NH 4 NO 3 and NH 4 NO 2 or more of them, thereby effectively promoting the melting of the glass ceramic powder at low temperature and reducing the problem of premature crystallization. The preferred oxidizing agent is Bi(NO 3 ) 3 ·5H 2 O, because bismuth nitrate decomposes at high temperature and releases oxidizing oxygen and nitrogen dioxide, thereby more effectively inhibiting the reduction reaction of Bi 3+ , and thus avoiding the reduction of Bi 3+ or the precipitation of Bi 3+ crystals during the melting process. At the same time, the gas generated by the decomposition of Bi(NO 3 ) 3 ·5H 2 O can stir the glass melt, promote glass clarification, and make the glass melting more uniform.
[0031] In the above glass powder composition formula provided by the present invention, Bi 2 O 3 and B 2 O 3 are the main network formers and network modifiers in the glass. At the same time, Bi 2 O 3 can significantly reduce the viscosity of the glass and promote melting, while B 2 O 3 helps to improve the chemical stability of the glass. When the weight ratio of Bi 2 O 3 and B 2 O 3 is (7.5-45):1, more preferably (7.5-37):1, the two of them can effectively synergistically improve the wettability of the glass powder slurry on various materials. This is because Bi 2 O 3 can reduce the surface energy of the glass, making it easier to contact and spread on the substrate, while B 2 O 3The addition of helps to form a more stable and thinner glass layer, further improving the wetting effect and suppressing premature crystallization of the glass to ensure the fluidity of the glass, ultimately achieving good connection of each material component in the mica window GM counter. Also, in the above formula, ZnO and BaO can cooperate synergistically to adjust the viscosity of the glass powder composition in the molten state, thereby affecting the fluidity and wettability of the slurry. Among them, ZnO helps to lower the melting point, while BaO tends to increase the melting point and viscosity of the glass. Preferably, the weight ratio of ZnO to BaO is (1-5):1, and more preferably (1.2-3.5):1, which can make the slurry show better fluidity at the sintering temperature, thus more significantly improving the wetting ability for different materials.
[0032] Further, by weight, the glass-ceramic powder composition for encapsulating a mica window GM counter comprises 75-85 parts of Bi 2 O 3 , 5-13 parts of ZnO, 2-10 parts of B 2 O 3 , 1-5 parts of BaO, 0.5-5 parts of Al 2 O 3 , 0.1-3 parts of CuO, 0.1-3 parts of K 2 O, 0.1-3 parts of Li 2 O, 0.1-3 parts of La 2 O 3 , 0.1-5 parts of CeO 2 and 0.1-3 parts of an oxidant. The above more precise formulation content design can further optimize the fluidity of the obtained glass-ceramic composition, making it form a tighter seal with the metal shell, ceramic column and mica sheet during the encapsulation process.
[0033] In several preferred embodiments, the glass-ceramic powder composition for encapsulating a mother window GM counter comprises 75-78 parts of Bi 2 O 3 , 5-7 parts of ZnO, 2-10 parts of B 2 O 3 , 1.5-5 parts of BaO, 0.5-2 parts of Al 2 O 3 , 0.1-1 part of CuO, 0.1-3 parts of K 2 O, 1-3 parts of Li 2 O, 0.1-1 part of La 2 O 3 , 0.5-5 parts of CeO 2 and 0.1-1 part of Bi(NO 3 ) 3 ·5H 2O. This narrower range of components allows for a more meticulous ratio of each component, thereby more precisely controlling the melting characteristics and fluidity of the resulting glass powder composition, and thus better compatible with the various components of the mica window GM counter, namely the metal housing, ceramic parts, glass exhaust pipes, etc., in order to provide the required sealing strength and airtightness during the encapsulation process, while reducing the stress caused by the mismatch of thermal expansion coefficients.
[0034] In several more preferred embodiments, by weight, the glass-ceramic powder composition for encapsulating a mica window GM counter comprises 75.2 parts of Bi 2 O 3 , 6 parts of ZnO, 10 parts of B 2 O 3 , 5 parts of BaO, 0.5 part of Al 2 O 3 , 0.2 part of CuO, 0.1 part of K 2 O, 1.2 parts of Li 2 O, 0.6 part of La 2 O 3 , 0.9 part of CeO 2 and 0.3 part of Bi(NO 3 ) 3 ·5H 2 O; or, by weight, the glass-ceramic powder composition for encapsulating a mica window GM counter comprises 77.3 parts of Bi 2 O 3 , 5.2 parts of ZnO, 2.1 parts of B 2 O 3 , 1.7 parts of BaO, 1.3 parts of Al 2 O 3 , 0.5 part of CuO, 3 parts of K 2 O, 3 parts of Li 2 O, 0.3 part of La 2 O 3 , 5 parts of CeO 2 and 0.6 part of Bi(NO 3 ) 3 ·5H 2 O. Through a large number of experiments, the inventors have preferably selected the glass-ceramic powder compositions for encapsulating a mica window GM counter with the above two specific component formulations. Under these component contents, the resulting glass powder compositions have a more matched thermal expansion coefficient, and the range of glass transition temperature and expansion softening temperature is also more suitable. More importantly, the above two glass powder compositions have particularly excellent wettability with ceramics, glass, mica sheets, and metals, thereby being able to more significantly achieve stable and highly airtight bonding therebetween.
[0035] In addition, preferably, the particle size D50 of the glass-ceramic powder composition for mica window GM counter encapsulation is 1.0 μm to 5.0 μm, more preferably 1.5 μm to 2.5 μm. The control of this preferred and more preferred particle size range can promote the uniform distribution of the glass-ceramic powder during the encapsulation process and improve the density and uniformity of the encapsulation layer formed by sintering. In order to better achieve better thermal expansion matching with the metal shell, ceramic column, glass tube and mica sheet of the mica window GM counter, the expansion coefficient α of the glass-ceramic powder composition for mica window GM counter encapsulation 30 / 300 is preferably 90×10 -7 / °C to 110×10 -7 / °C, more preferably 95×10 -7 / °C to 105×10 -7 / °C. Preferably, the glass transition temperature of the glass-ceramic powder composition for mica window GM counter encapsulation is 400 °C to 450 °C, more preferably 410 °C to 430 °C, in order to optimize the sealing temperature of the glass within a reasonable temperature range. Since the glass transition temperature is generally proportional to the softening temperature of the glass, controlling the glass transition temperature to regulate the glass softening temperature can further control the sealing temperature. If the sealing temperature is too high, the evacuation glass tube is prone to softening and deformation; glasses with too low sealing temperature often have a high expansion coefficient, resulting in sealing mismatch. The expansion and softening temperature of the glass-ceramic powder composition for mica window GM counter encapsulation is 420 °C to 480 °C, preferably 430 °C to 460 °C, and its function is similar to that of the glass transition temperature. The crystallization temperature of the glass-ceramic powder composition for mica window GM counter encapsulation is 520 °C to 620 °C, preferably 580 °C to 600 °C, which is to optimize the crystallization temperature. If the crystallization temperature is too low, that is, crystallization occurs prematurely during the sintering heating process, the fluidity of the glass decreases, and it cannot fully wet the materials to be sealed, resulting in insufficient sealing strength or even insufficient airtightness. If the crystallization temperature is too high, the glass does not crystallize or the crystallization amount is insufficient within the sealing temperature range, and the glass will melt and flow again when the mica sheet is secondarily sealed, resulting in displacement or even detachment of the glass tube or ceramic part.
[0036] The second aspect of the present invention provides a preparation method of the above-mentioned glass-ceramic powder composition for mica window GM counter encapsulation, including: Step S1, mixing the raw materials of the glass-ceramic powder composition for mica window GM counter encapsulation to obtain a mixed material; Step S2, subjecting the mixed material to melting and rolling in sequence to obtain a rolled material; Step S3, subjecting the rolled material to ball milling and screening in sequence to obtain the glass-ceramic powder composition for mica window GM counter encapsulation. Based on the above control of the component content, the present invention correspondingly provides a preparation method of the glass-ceramic powder composition for mica window GM counter encapsulation, thereby effectively controlling the particle size and morphology of the obtained glass-ceramic powder, optimizing its various physical and chemical properties, and improving its uniformity and density during the encapsulation process.
[0037] In several typical embodiments, in step S2, the melting is carried out at 850 °C to 1200 °C until the mixture is completely melted; more preferably, the melting is carried out at 900 °C to 1000 °C until the mixture is completely melted. For the above components of the glass powder composition provided by the present invention, at a temperature of 850 °C to 1200 °C, the components in the glass are sufficiently melted, while the more suitable temperature range of 900 °C to 1000 °C helps the formation of crystal nuclei and the control of the size and quantity thereof in the subsequent process, creates conditions for crystal growth, makes it exhibit better fluidity and sintering performance, and helps to form a dense and uniform sealing layer between different materials after sintering.
[0038] Moreover, since the cooling rate affects the crystal growth rate, the inventors preferably use a roll temperature of 5 °C to 30 °C, more preferably 10 °C to 25 °C, through a large number of experiments. The molten mixture is rapidly cooled under this condition, so as to more effectively control the crystal growth of the glass powder composition, avoid the rapid growth of crystals due to slow cooling, thereby obtaining a more uniform and finer microcrystalline structure, optimizing its melting performance and thermal expansion coefficient, improving its wetting performance on various materials, and finally enabling it to better meet the packaging requirements of the mica window GM counter.
[0039] In several particularly typical embodiments, further preferably, before cooling, it further includes heat preservation treatment of the completely melted mixture at 680 °C to 750 °C for 0.1 h to 2 h. The inventors preferably carry out heat preservation at this temperature through a large number of experiments. Within this temperature range, a certain number of crystal nuclei are formed in the glass melt obtained by melting and begin to grow slowly and stably, forming tiny crystals. At the same time, this heat preservation range can also provide appropriate time and energy to promote the formation of crystal nuclei, optimize the number and distribution of crystal nuclei, and at the same time regulate the grain size of the obtained glass powder composition, thereby adjusting its thermal expansion coefficient, enabling it to match the thermal expansion coefficients of a variety of materials to be sealed, and at the same time avoiding the reduction of the sintering fluidity of the glass powder caused by excessive crystallization.
[0040] Furthermore, in order to more effectively control the particle size distribution of the obtained glass powder composition, in step S3, the rotation speed of ball milling is preferably 100 rap / min to 500 rap / min, and the time is 0.5 h to 3 h, so as to improve the wettability and sintering performance of the glass powder composition. While more preferably, the rotation speed of ball milling is 200 rap / min to 300 rap / min, and the time is 1 h to 2 h, which can activate the surface, enhance the wettability, and at the same time minimize the deterioration of uniformity and the generation of defects that may occur during the ball milling of the glass powder, improve its purity and uniformity, and further enhance the consistency and airtightness of the package formed after sintering.
[0041] The third aspect of the present invention provides a mica window GM counter, which includes a metal housing, a ceramic column, an air filling and exhausting glass tube, and a mica sheet. The connections between the metal housing and the ceramic column, between the metal housing and the air filling and exhausting glass tube, and between the metal housing and the mica sheet are all achieved through the coating and sintering of sealing glass, and the sealing glass is the microcrystalline glass powder composition for encapsulating the above mica window GM counter. Since the microcrystalline glass powder composition for encapsulating the mica window GM counter obtained by the present invention has particularly suitable thermal expansion matching, more suitable glass transition temperature, melting softening temperature and crystallization softening temperature, and has good fluidity with metals, mica sheets, glass and ceramics, and the glass glaze has at least a certain luster after sintering, it can well meet the special encapsulation requirements of the mica window GM counter, and finally obtain a mica window GM counter with higher airtightness, higher precision and longer service life.
[0042] Further, the assembly process of the mica window GM counter includes the following steps carried out in sequence: preparing a bonding slurry with a viscosity of 100,000 CP to 200,000 CP by mixing the microcrystalline glass powder composition for encapsulating the mica window GM counter with an organic solvent; coating the bonding slurry at the connection between the metal housing and the air filling and exhausting glass tube, and forming a first seal after the first sintering; coating the bonding slurry at the connection between the metal housing and the ceramic column, and forming a second seal after the second sintering; coating the bonding slurry at the connection between the metal housing and the mica sheet, and forming a third seal after the third sintering. The above assembly process can better utilize the melting characteristics of the obtained microcrystalline glass powder composition for encapsulating the mica window GM counter, thereby improving the airtightness and structural stability of the mica window GM counter during the encapsulation process. In several preferred embodiments, the airtightness of the mica window GM counter is 2.0×10 -9 Pa·m 3 / s to 10 -8 Pa·m 3 / s.
[0043] The following further describes the present application in detail with specific embodiments, and these embodiments should not be construed as limiting the scope claimed by the present application.
[0044] Unless otherwise defined, all professional terms used hereinafter have the same meaning as commonly understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the protection scope of the present invention.
[0045] Example 1
[0046] A preparation method of a microcrystalline glass powder composition for encapsulating a mica window GM counter:
[0047] The raw material components of the glass-ceramic powder composition for mica window GM counter packaging are shown in Table 1-1 and Table 1-2.
[0048] Step (1): Mix the raw materials in the above table to obtain a mixed material.
[0049] Step (2): Quickly add the obtained mixed material to 900 °C for melting until all the raw materials are completely melted; keep the completely melted mixed material at 680 °C for 0.2 h for heat preservation treatment; then pour the molten glass into a rolling mill and roll it into a glass sheet under the condition that the roll temperature is 25 °C to obtain a rolled sheet.
[0050] Step (3): Place the obtained rolled sheet in a planetary ball mill and ball mill it at a speed of 200 rap / min for 1.2 h, and then pass it through a 150-mesh sieve to remove the porcelain balls for ball milling to obtain the glass-ceramic powder composition for mica window GM counter packaging.
[0051] Example 2
[0052] A preparation method of a glass-ceramic powder composition for mica window GM counter packaging:
[0053] The raw material components of the glass-ceramic powder composition for mica window GM counter packaging are shown in Table 1-1 and Table 1-2.
[0054] Step (1): Mix the raw materials in the above table to obtain a mixed material.
[0055] Step (2): Quickly add the obtained mixed material to 950 °C for melting until all the raw materials are completely melted; keep the completely melted mixed material at 700 °C for 0.5 h for heat preservation treatment; then pour the molten glass into a rolling mill and roll it into a glass sheet under the condition that the roll temperature is 15 °C to obtain a rolled sheet.
[0056] Step (3): Place the obtained rolled sheet in a planetary ball mill and ball mill it at a speed of 250 rap / min for 1.5 h, and then pass it through a 150-mesh sieve to remove the porcelain balls for ball milling to obtain the glass-ceramic powder composition for mica window GM counter packaging.
[0057] Example 3
[0058] A preparation method of a glass-ceramic powder composition for mica window GM counter packaging:
[0059] The raw material components of the glass-ceramic powder composition for mica window GM counter packaging are shown in Table 1-1 and Table 1-2.
[0060] Step (1): Mix the raw materials in the above table to obtain a mixed material.
[0061] Step (2): Rapidly add the obtained mixture to be melted at 1000 °C until all raw materials are completely melted; keep the completely melted mixture at 750 °C for heat preservation for 0.7 h; then pour the molten glass into a rolling mill and roll it into glass sheets under the condition that the temperature of the rolling rolls is 10 °C to obtain rolled sheets.
[0062] Step (3): Place the obtained rolled sheets in a planetary ball mill, ball mill at a speed of 300 rap / min for 1.5 h, and then pass through a 100-mesh sieve to remove the porcelain balls used for ball milling, to obtain the glass-ceramic powder composition for encapsulating mica window GM counters.
[0063] Examples 4 to 7
[0064] The differences between Examples 4 to 7 and Example 1 are only as follows:
[0065] The content of the raw material components of the glass-ceramic powder composition for encapsulating mica window GM counters is different, as shown in Table 1-1 and Table 1-2 in detail.
[0066] Example 8
[0067] A preparation method of a glass-ceramic powder composition for encapsulating mica window GM counters:
[0068] The difference between this example and Example 1 is only the preparation method. Specifically:
[0069] Change the melting temperature in step (2) to 850 °C and change the temperature of the rolling rolls used for rolling to 5 °C.
[0070] Example 9
[0071] A preparation method of a glass-ceramic powder composition for encapsulating mica window GM counters:
[0072] The difference between this example and Example 1 is only the preparation method. Specifically:
[0073] Change the melting temperature in step (2) to 1200 °C and change the temperature of the rolling rolls used for rolling to 30 °C.
[0074] Example 10
[0075] A preparation method of a glass-ceramic powder composition for encapsulating mica window GM counters:
[0076] The difference between this example and Example 1 is only the preparation method. Specifically:
[0077] Change the temperature of the heat preservation treatment in step (2) to 600 °C and change the time to 2.5 h.
[0078] Example 11
[0079] Preparation method of glass-ceramic powder composition for encapsulating mica-window GM counter:
[0080] The difference between this example and Example 1 lies only in the different preparation methods. Specifically:
[0081] Change the temperature of the heat preservation treatment in step (2) to 850 °C and the time to 5 min.
[0082] Example 12
[0083] Preparation method of glass-ceramic powder composition for encapsulating mica-window GM counter:
[0084] The difference between this example and Example 1 lies only in the different preparation methods. Specifically:
[0085] Change the rotation speed of ball milling in step (3) to 100 rap / min and the time to 3 h.
[0086] Example 13
[0087] Preparation method of glass-ceramic powder composition for encapsulating mica-window GM counter:
[0088] The difference between this example and Example 1 lies only in the different preparation methods. Specifically:
[0089] Change the rotation speed of ball milling in step (3) to 500 rap / min and the time to 0.5 h.
[0090] Comparative Examples 1 to 3
[0091] The difference between Comparative Examples 1 to 3 and Example 1 lies only in the different contents of the raw material components of the glass-ceramic powder composition for encapsulating mica-window GM counter. See Tables 1-1 and 1-2 for details.
[0092] Table 1-1
[0093] Components / parts by weight <![CDATA[Bi 2 O 3 > ZnO <![CDATA[B 2 O 3 > BaO <![CDATA[Al 2 O 3 > CuO <![CDATA[K 2 O]]> Example 1 81.5 7.8 3.5 1.3 0.5 0.1 1.3 Example 2 75 8.6 2 3 1.6 3 1.5 Example 3 76.6 13 2.1 1.1 5 0.2 0.2 Example 4 75.2 6 10 5 0.5 0.2 0.1 Example 5 77.3 5.2 2.1 1.7 1.3 0.5 3 Example 6 85 5 2 1 0.5 0.2 0.1 Example 7 81.5 7.8 3.5 1.3 0.5 0.1 1.3 Comparative Example 1 73 1 11 6 0.2 4 0.05 Comparative Example 2 87 1 1 0.05 6 0.05 4 Comparative Example 3 81.5 7.8 3.5 1.3 0.5 0.1 1.3
[0094] Table 1-2
[0095] Components / parts by weight <![CDATA[Li 2 O]]> <![CDATA[La 2 O 3 > <![CDATA[CeO 2 > <![CDATA[Bi(NO 3 ) 3 ·5H 2 O]]> <![CDATA[Bi 2 O 3 / B 2 O 3 > ZnO / BaO Example 1 0.2 0.2 0.8 2.8 23.3 6.0 Example 2 2.1 0.1 1.5 1.6 37.5 2.9 Example 3 0.2 0.2 0.3 1.1 36.48 11.8 Example 4 1.2 0.6 0.9 0.3 7.52 1.2 Example 5 3 0.3 5 0.6 36.8 3.1 Example 6 0.1 3 0.1 3 42.5 5.0 Example 7 0.2 0.2 3.6 0 23.3 6.0 Comparative Example 1 0.05 4 0.1 0.6 6.6 0.2 Comparative Example 2 0.05 0.05 0.2 0.6 87 20 Comparative Example 3 0.2 0.2 0.8 2.0 23.3 6.0
[0096] In addition, on the basis of Tables 1-1 and 1-2, Comparative Example 3 further includes 1.0 part by weight of Sb 2 O 3 .
[0097] Testing method
[0098] Particle size distribution: Tested by a laser particle size distribution analyzer, and the D50 of each glass powder composition is obtained.
[0099] Coefficient of thermal expansion α 30 / 300 , Glass transition temperature, expansion softening temperature: All were tested by the Netzsch DIL402 dilatometer.
[0100] Crystallization temperature: Tested by NETZSCH STA 449F5.
[0101] Sinterability and wettability:
[0102] The glass powders obtained from each example and comparative example were respectively pressed into cylindrical shapes with an axial height of 10 mm and a radius of 5 mm on a forsterite ceramic substrate, and then sintered at 600 °C for 1 h. The glossiness of the sintered glass was used to reflect the appearance after sintering, and the axial height of the sintered glass column was used to reflect the sintering fluidity on the ceramic substrate, that is, the wettability.
[0103] The substrate was replaced with a 430 stainless steel metal substrate, and the above sintering steps were repeated to obtain the wettability of the glass powder composition on the metal substrate.
[0104] The substrate was then replaced with a common window glass substrate, and the above sintering steps were repeated to obtain the wettability of the glass powder composition on the glass substrate. The smaller this value, the better the wettability.
[0105] Assembly of mica window GM counter and airtightness test: Obtained by testing with a helium mass spectrometer leak detector. The smaller this value, the better the airtightness.
[0106] The above test results are shown in Table 2.
[0107] Table 2
[0108]
[0109] From the above description, it can be seen that the above examples of the present invention achieve the preparation of a glass powder composition with excellent performance. It has a more matching coefficient of thermal expansion, a more suitable glass transition temperature range, crystallization temperature range and expansion softening temperature range, and at the same time shows good wettability with various materials such as metals, ceramics, glass and mica sheets, and finally well meets the special encapsulation requirements of the mica window GM counter.
[0110] Specifically, compared with Example 1, the content of Bi in Example 2 2 O 3 is slightly lower and the content of Al 2 O 3 is slightly higher, resulting in a slightly lower glass expansion coefficient, a larger high-temperature viscosity of the glass, and a slightly reduced self-fluidity. Compared with Example 2, the Al in Example 3 2 O 3As the content further increases, the high-temperature viscosity of the glass increases. Introducing more ZnO promotes the crystallization of the glass, resulting in a slightly larger degree of crystallization of the glass after sintering and the loss of some glass luster.
[0111] However, a relatively large amount of B was introduced in the formulation of Example 4 2 O 3 which increased the crystallization temperature of the glass and inhibited crystallization, and had better wettability. In Example 5, the alkali metal content was relatively high, which lowered the softening point of the glass and increased CeO 2 which helped to increase the fluidity of the glass and improve the wettability with the substrate material. More importantly, in Examples 4 and 5, the weight ratio of Bi 2 O 3 and B 2 O 3 as well as the weight ratio of ZnO and BaO were more suitable, so that the wetting ability of the obtained glass powder composition for different materials could be improved more significantly. As can be seen from the data in the table, for the glass powder compositions obtained in these two examples, after sintering on three different substrate materials respectively, their heights were all less than 6.5 mm, and the airtightness of the finally obtained mica window GM counter was also the best.
[0112] In Example 6, the content of Bi 2 O 3 was high and the glass softening temperature was relatively low; adding a small amount of La 2 O 3 provided a certain number of crystal nuclei and promoted crystallization. Compared with Example 1, in Example 7, no additional oxidant was added, but the content of CeO 2 was increased, and cerium oxide could release a certain amount of oxygen to create an oxidizing atmosphere, which also belonged to an oxidant.
[0113] By comparing Example 1 with Examples 8 and 9, it can be seen that when the preferred melting temperature is 900 °C to 1000 °C and the roll temperature used for rolling is 10 °C to 25 °C, it is helpful for the formation of subsequent crystal nuclei and the control of the size and quantity, resulting in a more uniform and finer microcrystalline structure and optimizing its melting properties and thermal expansion coefficient. Therefore, compared with Example 1, the glass powder composition obtained in Example 8 had a lower melting temperature, less volatilization of low-temperature components, especially Bi 2 O 3 and B 2 O 3 , and the overall thermal performance of the glass was relatively low, while the crystallization ability was weak, which would cause the softening of the primary sealing position during secondary sealing and affect the airtightness. In Example 9, on the premise of sufficient melting of the glass, the roll temperature was relatively high, which prolonged the crystal growth time during the cooling process of the glass melt. Therefore, the airtightness of the mica window GM counter prepared using it as the sealing glass was slightly worse than that of Example 1.
[0114] By comparing Example 1 with Examples 10 and 11, it can be seen that preferably, the heat preservation temperature and time before cooling the completely melted mixture can also optimize the number and distribution of crystal nuclei, and at the same time control the crystal grain size of the obtained glass powder composition, thereby adjusting its thermal expansion coefficient so that it can match the thermal expansion coefficients of a variety of materials to be sealed, and at the same time satisfying one-time sealing and crystallization without being affected by secondary heating. In contrast, the heat preservation temperature in Example 10 is too low, which is not conducive to crystal nucleus formation, and the heat preservation time in Example 11 is too short, resulting in insufficient crystal nuclei, so that effective microcrystal number and size cannot be formed. Eventually, during the secondary sealing process, the primary sealing part softens, deforms or even displaces, resulting in slightly poor airtightness of the obtained mica window GM counter.
[0115] By comparing Example 1 with Examples 12 and 13, it can be seen that more preferably, the rotation speed of ball milling is 200 rap / min to 300 rap / min, and the time is 1 h to 2 h, which can reduce the deterioration of uniformity and the generation of defects that may occur during the ball milling of glass powder, improve its purity and uniformity, and further improve the consistency and airtightness of the package formed after sintering. Among them, too long ball milling time in Example 12 and too fast ball milling speed in Example 13 will both result in too fine particle size of the glass powder, reduced crystallization activation energy, easy premature crystallization, which affects the fluidity and wettability of the glass, and reduces the airtightness after sealing.
[0116] By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the present invention has prepared a glass powder composition with excellent sealing performance through a strictly controlled glass-ceramic powder composition formula for the encapsulation of mica window GM counters, and finally well meets the special encapsulation requirements of mica window GM counters.
[0117] Especially for Comparative Example 3, although it can obtain a glass powder composition with suitable wettability, thermal expansion coefficient and melting characteristics, because its formula contains Sb 2 O 3 , therefore, after sintering, the resistance of the sealing part to corrosive media such as acids and alkalis decreases, which has a particularly adverse effect on the long-term stability and reliability of the finally obtained package, and does not have practical application value. At the same time, it also inhibits the formation of crystals, resulting in the crystallization temperature shifting to a higher temperature, making it difficult to meet the process requirements.
[0118] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and do not have to be used to describe a specific order or sequence. It should be understood that such terms can be interchanged under appropriate circumstances so that the embodiments of the present application described here can be implemented in an order other than those described here.
[0119] The above are only the preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included within the protection scope of the present invention.
Claims
1. A glass-ceramic powder composition for packaging a mica window GM counter, characterized in that: The microcrystalline glass powder composition for packaging a mica window GM counter includes, by weight, 70 to 90 parts of Bi2O3, 2 to 15 parts of ZnO, 1 to 12 parts of B2O3, 1 to 8 parts of BaO, 0.2 to 7 parts of Al2O3, 0.1 to 5 parts of CuO, 0.1 to 5 parts of K2O, 0.1 to 5 parts of Li2O, 0.1 to 5 parts of La2O3, 0.1 to 8 parts of CeO2, and 0 to 5 parts of an oxidant; The oxidant is nitrate and / or nitrite, and the cations in the nitrate and / or nitrite are each independently selected from one or more of ammonium ion, bismuth ion, zinc ion, barium ion, aluminum ion, copper ion, potassium ion, lithium ion, lanthanum ion and cerium ion.
2. The microcrystalline glass powder composition for mica window GM counter packaging according to claim 1, characterized in that: The oxidant is selected from one or more of Bi(NO3)3·5H2O, Ba(NO3)2, KNO3, KNO2, NH4NO3 and NH4NO2, preferably Bi(NO3)3·5H2O.
3. The microcrystalline glass powder composition for packaging a mica window GM counter according to claim 1 or 2, characterized in that: In the microcrystalline glass powder composition for packaging a mica window GM counter, the weight ratio of Bi2O3 to B2O3 is (7.5-45):1; and / or, In the microcrystalline glass powder composition for packaging a mica window GM counter, the weight ratio of the ZnO to the BaO is (1-5):
1.
4. The microcrystalline glass powder composition for packaging a mica window GM counter according to any one of claims 1 to 3, characterized in that: In parts by weight, the microcrystalline glass powder composition for packaging a mica window GM counter includes 75 to 85 parts of Bi2O3, 5 to 13 parts of ZnO, 2 to 10 parts of B2O3, 1 to 5 parts of BaO, 0.5 to 5 parts of Al2O3, 0.1 to 3 parts of CuO, 0.1 to 3 parts of K2O, 0.1 to 3 parts of Li2O, 0.1 to 3 parts of La2O3, 0.1 to 5 parts of CeO2 and 0.1 to 3 parts of the oxidant; Preferably, in parts by weight, the microcrystalline glass powder composition for mica window GM counter packaging includes 75 to 78 parts of Bi2O3, 5 to 7 parts of ZnO, 2 to 10 parts of B2O3, 1.5 to 5 parts of BaO, 0.5 to 2 parts of Al2O3, 0.1 to 1 parts of CuO, 0.1 to 3 parts of K2O, 1 to 3 parts of Li2O, 0.1 to 1 parts of La2O3, 0.5 to 5 parts of CeO2 and 0.1 to 1 parts of Bi(NO3)3·5H2O.
5. The microcrystalline glass powder composition for packaging a mica window GM counter according to any one of claims 1 to 4, characterized in that: The particle size D50 of the microcrystalline glass powder composition for packaging a mica window GM counter is 1.0 μm to 5.0 μm, preferably 1.5 μm to 2.5 μm; and / or, The expansion coefficient α of the microcrystalline glass powder composition for packaging the mica window GM counter 30 / 300 90×10 -7 / ℃~110×10 -7 / ℃, preferably 95×10 -7 / ℃~105×10 -7 / ℃; and / or, The glass transition temperature of the microcrystalline glass powder composition for packaging a mica window GM counter is 400° C. to 450° C., preferably 410° C. to 430° C.; and / or, The expansion softening temperature of the microcrystalline glass powder composition for packaging a mica window GM counter is 420° C. to 480° C., preferably 430° C. to 460° C.; and / or, The crystallization temperature of the microcrystalline glass powder composition for packaging a mica window GM counter is 520°C to 620°C, preferably 580°C to 600°C.
6. A method for preparing the microcrystalline glass powder composition for packaging a mica window GM counter according to any one of claims 1 to 5, characterized in that: include: Step S1, mixing the raw materials of the microcrystalline glass powder composition for packaging the mica window GM counter to obtain a mixture; Step S2, the mixed material is melted and rolled in sequence to obtain a rolled material; Step S3, the rolled material is ball-milled and sieved in sequence to obtain the microcrystalline glass powder composition for packaging the mica window GM counter.
7. The method for preparing the microcrystalline glass powder composition for packaging a mica window GM counter according to claim 6, characterized in that: In the step S2, The melting is performed at 850°C to 1200°C until the mixed material is melted; and / or the rolling roller temperature used in the rolling is 5°C to 30°C; Preferably, the melting is carried out at 900°C to 1000°C until the mixed material is melted; and / or the rolling roller temperature used in the rolling is 10°C to 25°C.
8. The method for preparing the microcrystalline glass powder composition for packaging a mica window GM counter according to claim 6 or 7, characterized in that: In the step S3, the rotation speed of the ball mill is 100 rap / min to 500 rap / min, and the time is 0.5 h to 3 h.
9. A mica window GM counter, comprising a metal shell, a ceramic column, an air-filled glass tube and a mica sheet, wherein the connection between the metal shell and the ceramic column, the connection between the metal shell and the air-filled glass tube, and the connection between the metal shell and the mica sheet are all achieved by coating and sintering sealing glass, characterized in that: The sealing glass is the microcrystalline glass powder composition for packaging a mica window GM counter according to any one of claims 1 to 5.
10. The mica window GM counter according to claim 9, characterized in that: The assembly process of the mica window GM counter includes the following steps: preparing the microcrystalline glass powder composition for packaging the mica window GM counter with an organic solvent into a bonding slurry with a viscosity of 100,000 CP to 200,000 CP; applying the bonding slurry to the connection between the metal shell and the gas-filling glass tube, and forming a first seal after a first sintering; applying the bonding slurry to the connection between the metal shell and the ceramic column, and forming a second seal after a second sintering; applying the bonding slurry to the connection between the metal shell and the mica sheet, and forming a third seal after a third sintering; Preferably, the air tightness of the mica window GM counter is 2.0×10 -9 Pa·m 3 / s~10 -8 Pa·m 3 / s.