Corrosion-resistant and wear-resistant copper insert and preparation method thereof
By electroplating on the surface of the copper insert with ionic liquid, and performing sealing liquid treatment, the shortcomings of the copper insert in corrosion resistance and wear resistance are solved, and a higher service life and environmental protection are achieved.
Patent Information
- Application Number
- CN202510573913.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-06
- Publication Date
- 2025-06-13
AI Technical Summary
The existing copper inserts have shortcomings in corrosion resistance and wear resistance, and the traditional electroless plating process has problems such as environmental pollution and easy plating.
Ion liquid electroplating technology is used to deposit nickel-copper-Elosite nanotube layers on the surface of copper inserts, and the bonding strength of the plating is improved by the sealing liquid treatment.
It significantly improves the corrosion resistance, wear resistance and service life of copper inserts, while reducing the risk of environmental pollution.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of corrosion resistance, and particularly to a corrosion-resistant and wear-resistant copper insert and a preparation method thereof. Background Art
[0002] Copper inserts are a common type of hardware component, generally used for embedding in substrates such as plastics to improve the strength, wear resistance and other properties of the substrates, and are widely used in fields such as communication, electronic appliances, automobiles, mechanical equipment, etc.
[0003] Currently, most copper inserts are processed from environmental protection copper, H59 copper, H62 copper, H3604 copper. However, metal components have problems such as limited corrosion resistance and wear resistance, which limit the scope of use and service life of copper inserts. In the existing industry, electroplating and coating methods are usually used to improve the corrosion resistance of copper inserts. However, traditional electroless plating generally uses water as a solvent, and its complex plating solution components are likely to cause environmental pollution and other problems. Single coatings also have problems such as easy peeling. Summary of the Invention
[0004] The purpose of the present invention is to provide a corrosion-resistant and wear-resistant copper insert and a preparation method thereof to solve the problems in the prior art.
[0005] To solve the above technical problems, the present invention provides the following technical solutions:
[0006] A preparation method of a corrosion-resistant and wear-resistant copper insert, comprising the following steps:
[0007] S1: The formed copper insert is successively subjected to alkali washing, water washing, acid washing, ultrasonic water washing, and drying to obtain a pretreated copper insert;
[0008] S2: Prepare an ionic liquid electroplating solution containing composite halloysite nanotubes, put the pretreated copper insert into the ionic liquid electroplating solution, and perform ultrasonic-assisted electroplating treatment to obtain an electroplated copper insert;
[0009] S3: Mix composite halloysite nanotubes, silane-modified polyurethane, additives, and solvents to obtain a sealing solution;
[0010] S4: Coat the sealing solution on the surface of the electroplated copper insert and dry it to obtain a corrosion-resistant and wear-resistant copper insert.
[0011] Further, the working conditions of the ultrasonic-assisted electroplating treatment are: the temperature is 68 - 72 °C, the time is 30 - 40 min, and the ultrasonic power is 280 W.
[0012] Further, the composition of the ionic liquid electroplating solution is: using choline chloride - ethylene glycol ionic liquid as a solvent, which contains nickel chloride hexahydrate 48 g / L, copper chloride dihydrate 17 g / L, and composite halloysite nanotubes (4 - 6) g / L.
[0013] Further, the choline chloride-ethylene glycol ionic liquid is prepared by mixing choline chloride and ethylene glycol in a molar ratio of 1:2.
[0014] Further, by mass, the composition of the sealing liquid is: 1-5 parts of composite halloysite nanotubes, 12-24 parts of silane-modified polyurethane, 0.5-1 part of auxiliary agent, and 11-16 parts of solvent.
[0015] Further, the solvent is prepared by mixing N,N-dimethylformamide, ethanol, and deionized water in a mass ratio of 3:2:1; the auxiliary agent is one of formic acid and acetic acid.
[0016] Further, the preparation of the composite halloysite nanotubes includes the following steps:
[0017] (1) Mix the corrosion inhibitor and ethanol, add halloysite nanotubes, ultrasonically treat for 10-20 min, transfer to a vacuum drying oven, evacuate for 1-2 h and then take out, repeat the process of evacuation and taking out 3-5 times, centrifuge, wash, and dry to obtain pretreated halloysite nanotubes;
[0018] (2) Mix the tris(hydroxymethyl)aminomethane hydrochloride solution, pretreated halloysite nanotubes, and dopamine hydrochloride, stir in the dark for 10-12 h, centrifuge, wash with water, and dry to obtain composite halloysite nanotubes.
[0019] 8. The preparation method of a corrosion-resistant and wear-resistant copper insert according to claim 7, wherein the corrosion inhibitor is one of 2-(1,3-benzothiazol-2-ylthio)succinic acid, sodium gluconate, and benzotriazole.
[0020] Further, the preparation of the silane-modified polyurethane includes the following steps:
[0021] 1) Mix octylamine and 3-(2,3-epoxypropoxy)propyltrimethoxysilane, stir at 18-25 °C for 22-24 h to obtain a silane chain extender;
[0022] 2) Under a nitrogen atmosphere, mix polytetramethylene ether glycol, isophorone diisocyanate, and methyl ethyl ketone, add dibutyltin dilaurate, raise the temperature to 68-72 °C and keep warm for 3-4 h, lower the temperature to 18-25 °C, add the chain extender, raise the temperature to 68-72 °C and stir for 2-3 h, add 2-(perfluorodecyl)ethanol and aminopropyltriethoxysilane and stir for 1-2 h to obtain silane-modified polyurethane.
[0023] Compared with the prior art, the beneficial effects of the present invention are:
[0024] The present invention provides a corrosion-resistant and wear-resistant copper insert and a preparation method thereof. Through composition and process limitations, the copper insert is subjected to plating treatment by means of ionic liquid electroplating, and then the surface of the plating layer is subjected to sealing treatment, so as to prepare a copper insert with hydrophobicity, good corrosion resistance and high wear resistance, greatly improving the appearance aesthetics and service life of the copper insert.
[0025] In order to improve the problems existing in the existing aqueous solution electroplating process, such as hydrogen embrittlement prone to occur in the plating layer, easy passivation of the metal anode and troublesome waste liquid treatment, choline chloride-ethylene glycol ionic liquid with good conductivity and high chemical stability is selected as the solvent in the present invention, and a nickel-copper-halloysite nanotube layer is electrodeposited on the surface of the formed copper insert. The introduction of halloysite nanotubes can effectively reduce the residual stress of the plating layer, and at the same time improve the hardness, wear resistance and corrosion resistance of the plating layer. In order to further improve the corrosion resistance of the plating layer, taking advantage of the unique hollow tubular structure, large specific surface area and high reaction activity of halloysite nanotubes, etc., it is used as a nano loader for corrosion inhibitors, and then coated with dopamine to obtain composite halloysite nanotubes, which are introduced into the copper insert plating layer, so as to provide long-term corrosion protection for the copper insert, and at the same time improve the bonding strength between the sealing liquid and the plating layer, preventing the sealing layer formed by the sealing liquid from falling off.
[0026] In the sealing liquid, composite halloysite nanotubes are used as fillers and silane-modified polyurethane is used as the base material. The silane-modified polyurethane is prepared by using isophorone diisocyanate and polytetramethylene ether glycol as raw materials to synthesize a prepolymer, using octylamine to ring-open 3-(2,3-epoxypropoxy)propyltrimethoxysilane as a chain extender, and using 2-(perfluorodecyl)ethanol and aminopropyltriethoxysilane as end-capping agents. The structure of the polyurethane prepolymer is modified by functionalized siloxane, and then in the sealing layer, the hydrolysis and condensation of siloxane are used to achieve compatibility with the substrate and firm mechanical properties, endowing the sealing layer with excellent water resistance and high temperature resistance, and extending the service life of the copper insert. Specific embodiments
[0027] The following will clearly and completely describe the technical solutions in the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative efforts shall fall within the protection scope of the present invention.
[0028] It should be noted that if there are directional indications in the embodiments of the present invention, such as up, down, left, right, front, and back, these directional indications are only used to explain the relative positional relationship and movement conditions between components in a specific posture. If the specific posture changes, the directional indications will also change accordingly. In addition, the technical solutions between various embodiments can be combined with each other, but it must be based on the ability of those of ordinary skill in the art to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0029] The technical solutions of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0030] Embodiment 1: A preparation method of a corrosion-resistant and wear-resistant copper insert, comprising the following steps:
[0031] S1: The formed copper insert is successively subjected to alkali washing, water washing, acid washing, ultrasonic water washing, and drying to obtain a pretreated copper insert;
[0032] S2: Prepare an ionic liquid electroplating solution containing composite halloysite nanotubes, put the pretreated copper insert into the ionic liquid electroplating solution, and perform ultrasonic-assisted electroplating treatment to obtain an electroplated copper insert;
[0033] The working conditions of the ultrasonic-assisted electroplating treatment are: the temperature is 68 °C, the time is 40 min, and the ultrasonic power is 280 W;
[0034] The composition of the ionic liquid electroplating solution is: using choline chloride-ethylene glycol ionic liquid as a solvent, which contains 48 g / L of nickel chloride hexahydrate, 17 g / L of copper chloride dihydrate, and 4 g / L of composite halloysite nanotubes;
[0035] The choline chloride-ethylene glycol ionic liquid is prepared by mixing choline chloride and ethylene glycol in a molar ratio of 1:2;
[0036] The preparation of the composite halloysite nanotubes includes the following steps:
[0037] (1) Mix 2 g of corrosion inhibitor and 50 mL of ethanol, add 1 g of halloysite nanotubes, perform ultrasonic treatment for 10 min, transfer to a vacuum drying oven, evacuate for 1 h and then take out, repeat the process of evacuating and taking out 3-5 times, centrifuge, wash, dry, and grind to obtain pretreated halloysite nanotubes;
[0038] (2) Mix 20 mL of tris(hydroxymethyl)aminomethane hydrochloride solution (pH = 8.5), 40 mg of pretreated halloysite nanotubes, and 80 mg of dopamine hydrochloride, stir in the dark for 10 h, centrifuge, wash with water, and dry to obtain composite halloysite nanotubes;
[0039] The corrosion inhibitor is 2-(1,3-benzothiazole-2-thio) succinic acid;
[0040] S3: Mix the composite halloysite nanotubes, silane-modified polyurethane, additives, and solvent to obtain a sealing solution;
[0041] By mass, the composition of the sealing solution is: 1 part of composite halloysite nanotubes, 12 parts of silane-modified polyurethane, 0.5 part of additives, and 11 parts of solvent;
[0042] The solvent is a compound obtained by mixing N,N-dimethylformamide, ethanol, and deionized water in a mass ratio of 3:2:1; the additive is acetic acid;
[0043] The preparation of the silane-modified polyurethane includes the following steps:
[0044] 1) Mix 1 mmol of octylamine and 1 mmol of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, and stir at 18 °C for 24 h to obtain a silane chain extender;
[0045] 2) Under a nitrogen atmosphere, mix 0.02 mol of polytetramethylene ether glycol, 0.04 mol of isophorone diisocyanate, and 50 mL of butanone, add 2 drops of dibutyltin dilaurate, heat to 68 °C and keep warm for 4 h, cool to 18 °C, add 5 mmol of chain extender, heat to 68 °C and stir for 3 h, add 0.01 mol of 2-(perfluorodecyl)ethanol and 0.01 mol of aminopropyltriethoxysilane and stir for 1 h to obtain silane-modified polyurethane;
[0046] S4: Coat the sealing solution on the surface of the electroplated copper insert, and dry to obtain a corrosion-resistant and wear-resistant copper insert.
[0047] Example 2: A method for preparing a corrosion-resistant and wear-resistant copper insert, including the following steps:
[0048] S1: Alkaline wash, water wash, acid wash, ultrasonic water wash, and dry the formed copper insert in sequence to obtain a pretreated copper insert;
[0049] S2: Prepare an ionic liquid electroplating solution containing composite halloysite nanotubes, put the pretreated copper insert into the ionic liquid electroplating solution, and perform ultrasonic-assisted electroplating treatment to obtain an electroplated copper insert;
[0050] The working conditions of the ultrasonic-assisted electroplating treatment are: temperature is 70 °C, time is 35 min, and ultrasonic power is 280 W;
[0051] The composition of the ionic liquid electroplating solution is: using choline chloride-ethylene glycol ionic liquid as the solvent, which contains 48 g / L of nickel chloride hexahydrate, 17 g / L of copper chloride dihydrate, and 5 g / L of composite halloysite nanotubes;
[0052] The choline chloride-ethylene glycol ionic liquid is prepared by mixing choline chloride and ethylene glycol in a molar ratio of 1:2;
[0053] The preparation of the composite halloysite nanotubes includes the following steps:
[0054] (1) Mix 2 g of corrosion inhibitor and 50 mL of ethanol, add 1 g of halloysite nanotubes, ultrasonically treat for 15 min, transfer to a vacuum drying oven, evacuate for 1.5 h and then take out, repeat the process of evacuating and taking out 4 times, centrifuge, wash, dry, and grind to obtain pretreated halloysite nanotubes;
[0055] (2) Mix 20 mL of tris(hydroxymethyl)aminomethane hydrochloride solution (pH = 8.5), 40 mg of pretreated halloysite nanotubes, and 80 mg of dopamine hydrochloride, stir under dark conditions for 11.5 h, centrifuge, wash with water, and dry to obtain composite halloysite nanotubes;
[0056] The corrosion inhibitor is 2-(1,3-benzothiazol-2-ylthio)succinic acid;
[0057] S3: Mix the composite halloysite nanotubes, silane-modified polyurethane, additives, and solvent to obtain a sealing solution;
[0058] By mass, the composition of the sealing solution is: 3 parts of composite halloysite nanotubes, 17 parts of silane-modified polyurethane, 0.7 part of additives, and 13 parts of solvent;
[0059] The solvent is prepared by mixing N,N-dimethylformamide, ethanol, and deionized water in a mass ratio of 3:2:1; the additive is acetic acid;
[0060] The preparation of the silane-modified polyurethane includes the following steps:
[0061] 1) Mix 1 mmol of octylamine and 1 mmol of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, stir at 20 °C for 23 h to obtain a silane chain extender;
[0062] 2) Under a nitrogen atmosphere, mix 0.02 mol of polytetramethylene ether glycol, 0.04 mol of isophorone diisocyanate, and 50 mL of butanone, add 2 drops of dibutyltin dilaurate, raise the temperature to 70 °C and keep it warm for 3.5 h, lower the temperature to 20 °C, add 5 mmol of chain extender, raise the temperature to 70 °C and stir for 2.5 h, add 0.01 mol of 2-(perfluorodecyl)ethanol and 0.01 mol of aminopropyltriethoxysilane and stir for 1.5 h to obtain silane-modified polyurethane;
[0063] S4: Coat the sealing solution on the surface of the electroplated copper insert, dry to obtain a corrosion-resistant and wear-resistant copper insert.
[0064] Example 3: A preparation method of a corrosion-resistant and wear-resistant copper insert, comprising the following steps:
[0065] S1: The formed copper insert is successively subjected to alkali washing, water washing, acid washing, ultrasonic water washing, and drying to obtain a pretreated copper insert;
[0066] S2: Prepare an ionic liquid electroplating solution containing composite halloysite nanotubes, put the pretreated copper insert into the ionic liquid electroplating solution, and perform ultrasonic-assisted electroplating treatment to obtain an electroplated copper insert;
[0067] The working conditions of the ultrasonic-assisted electroplating treatment are: the temperature is 72 °C, the time is 30 min, and the ultrasonic power is 280 W;
[0068] The composition of the ionic liquid electroplating solution is: using choline chloride-ethylene glycol ionic liquid as the solvent, which contains 48 g / L of nickel chloride hexahydrate, 17 g / L of copper chloride dihydrate, and 6 g / L of composite halloysite nanotubes;
[0069] The choline chloride-ethylene glycol ionic liquid is prepared by mixing choline chloride and ethylene glycol in a molar ratio of 1:2;
[0070] The preparation of the composite halloysite nanotubes includes the following steps:
[0071] (1) Mix 2 g of corrosion inhibitor and 50 mL of ethanol, add 1 g of halloysite nanotubes, perform ultrasonic treatment for 20 min, transfer to a vacuum drying oven, evacuate for 1 h and then take out, repeat the process of evacuating and taking out 5 times, centrifuge, wash, dry, and grind to obtain pretreated halloysite nanotubes;
[0072] (2) Mix 20 mL of tris(hydroxymethyl)aminomethane hydrochloride solution (pH = 8.5), 40 mg of pretreated halloysite nanotubes, and 80 mg of dopamine hydrochloride, stir in the dark for 12 h, centrifuge, wash with water, and dry to obtain composite halloysite nanotubes;
[0073] The corrosion inhibitor is 2-(1,3-benzothiazol-2-ylthio)succinic acid;
[0074] S3: Mix the composite halloysite nanotubes, silane-modified polyurethane, additives, and solvent to obtain a sealing solution;
[0075] By mass, the composition of the sealing solution is: 5 parts of composite halloysite nanotubes, 24 parts of silane-modified polyurethane, 1 part of additives, and 16 parts of solvent;
[0076] The solvent is prepared by mixing N,N-dimethylformamide, ethanol, and deionized water in a mass ratio of 3:2:1; the additive is acetic acid;
[0077] The preparation of the silane-modified polyurethane includes the following steps:
[0078] 1) Mix 1 mmol of octylamine and 1 mmol of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, and stir at 25 °C for 22 h to obtain a silane chain extender;
[0079] 2) Under a nitrogen atmosphere, mix 0.02 mol of polytetramethylene ether glycol, 0.04 mol of isophorone diisocyanate, and 50 mL of methyl ethyl ketone, add 2 drops of dibutyltin dilaurate, heat to 72 °C and keep warm for 3 h, cool to 25 °C, add 5 mmol of chain extender, heat to 72 °C and stir for 2 h, add 0.01 mol of 2-(perfluorodecyl)ethanol and 0.01 mol of aminopropyltriethoxysilane and stir for 2 h to obtain a silane-modified polyurethane;
[0080] S4: Coat the sealing liquid on the surface of the electroplated copper insert, and dry it to obtain a corrosion-resistant and wear-resistant copper insert.
[0081] Comparative Example 1: Using Example 3 as a control group, replace the composite halloysite nanotubes with halloysite nanotubes, and other processes are normal;
[0082] A preparation method of a corrosion-resistant and wear-resistant copper insert, comprising the following steps:
[0083] S1: The formed copper insert is successively subjected to alkali washing, water washing, acid washing, ultrasonic water washing, and drying to obtain a pretreated copper insert;
[0084] S2: Prepare an ionic liquid electroplating solution containing halloysite nanotubes, put the pretreated copper insert into the ionic liquid electroplating solution, and perform ultrasonic-assisted electroplating treatment to obtain an electroplated copper insert;
[0085] The working conditions of the ultrasonic-assisted electroplating treatment are: the temperature is 72 °C, the time is 30 min, and the ultrasonic power is 280 W;
[0086] The composition of the ionic liquid electroplating solution is: using choline chloride-ethylene glycol ionic liquid as a solvent, which contains 48 g / L of nickel chloride hexahydrate, 17 g / L of copper chloride dihydrate, and 6 g / L of halloysite nanotubes;
[0087] The choline chloride-ethylene glycol ionic liquid is prepared by mixing choline chloride and ethylene glycol in a molar ratio of 1:2;
[0088] S3: Mix halloysite nanotubes, silane-modified polyurethane, additives, and solvents to obtain a sealing liquid;
[0089] By mass, the composition of the sealing liquid is: 5 parts of halloysite nanotubes, 24 parts of silane-modified polyurethane, 1 part of additives, and 16 parts of solvents;
[0090] The solvent is prepared by mixing N,N-dimethylformamide, ethanol, and deionized water in a mass ratio of 3:2:1; the additive is acetic acid;
[0091] The preparation of the silane-modified polyurethane comprises the following steps:
[0092] 1) Mix 1 mmol of octylamine and 1 mmol of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, and stir at 25 °C for 22 h to obtain a silane chain extender;
[0093] 2) Under a nitrogen atmosphere, mix 0.02 mol of polytetramethylene ether glycol, 0.04 mol of isophorone diisocyanate, and 50 mL of methyl ethyl ketone, add 2 drops of dibutyltin dilaurate, raise the temperature to 72 °C and keep it warm for 3 h, then lower the temperature to 25 °C, add 5 mmol of the chain extender, raise the temperature to 72 °C and stir for 2 h, add 0.01 mol of 2-(perfluorodecyl)ethanol and 0.01 mol of aminopropyltriethoxysilane and stir for 2 h to obtain the silane-modified polyurethane;
[0094] S4: Coat the sealing solution on the surface of the electroplated copper insert, and dry it to obtain a corrosion-resistant and wear-resistant copper insert.
[0095] Comparative Example 2: Taking Example 3 as the control group, the silane chain extender was not prepared, and other processes were normal;
[0096] A preparation method of a corrosion-resistant and wear-resistant copper insert comprises the following steps:
[0097] S1: Perform alkali washing, water washing, acid washing, ultrasonic water washing on the formed copper insert in sequence, and dry it to obtain a pretreated copper insert;
[0098] S2: Prepare an ionic liquid electroplating solution containing composite halloysite nanotubes, put the pretreated copper insert into the ionic liquid electroplating solution, and perform ultrasonic-assisted electroplating treatment to obtain an electroplated copper insert;
[0099] The working conditions of the ultrasonic-assisted electroplating treatment are: the temperature is 72 °C, the time is 30 min, and the ultrasonic power is 280 W;
[0100] The composition of the ionic liquid electroplating solution is: using choline chloride-ethylene glycol ionic liquid as the solvent, which contains 48 g / L of nickel chloride hexahydrate, 17 g / L of copper chloride dihydrate, and 6 g / L of composite halloysite nanotubes;
[0101] The choline chloride-ethylene glycol ionic liquid is prepared by mixing choline chloride and ethylene glycol in a molar ratio of 1:2;
[0102] The preparation of the composite halloysite nanotubes comprises the following steps:
[0103] (1) Mix 2 g of corrosion inhibitor and 50 mL of ethanol, add 1 g of halloysite nanotubes, ultrasonically treat for 20 min, transfer to a vacuum drying oven, evacuate for 1 h and then take out. Repeat the process of evacuation and taking out 5 times, centrifuge, wash, dry, and grind to obtain pretreated halloysite nanotubes;
[0104] (2) Mix 20 mL of tris(hydroxymethyl)aminomethane hydrochloride solution (pH = 8.5), 40 mg of pretreated halloysite nanotubes, and 80 mg of dopamine hydrochloride, stir in the dark for 12 h, centrifuge, wash with water, and dry to obtain composite halloysite nanotubes;
[0105] The corrosion inhibitor is 2-(1,3-benzothiazol-2-ylthio)succinic acid;
[0106] S3: Mix the composite halloysite nanotubes, silane-modified polyurethane, additives, and solvent to obtain a sealing solution;
[0107] By mass, the composition of the sealing solution is: 5 parts of composite halloysite nanotubes, 24 parts of silane-modified polyurethane, 1 part of additives, and 16 parts of solvent;
[0108] The solvent is a compound prepared from N,N-dimethylformamide, ethanol, and deionized water in a mass ratio of 3:2:1; the additive is acetic acid;
[0109] The preparation of the silane-modified polyurethane includes the following steps:
[0110] 1) Under a nitrogen atmosphere, mix 0.02 mol of polytetramethylene ether glycol, 0.04 mol of isophorone diisocyanate, and 50 mL of butanone, add 2 drops of dibutyltin dilaurate, raise the temperature to 72 °C and hold for 3 h, cool to 25 °C, then raise the temperature to 72 °C, add 0.01 mol of 2-(perfluorodecyl)ethanol and 0.01 mol of aminopropyltriethoxysilane, and stir for 2 h to obtain silane-modified polyurethane;
[0111] S4: Coat the sealing solution on the surface of the electroplated copper insert, dry to obtain a corrosion-resistant and wear-resistant copper insert.
[0112] The thickness formed after the sealing solution is cured on the surface of the electroplated copper insert is 5 μm.
[0113] Sources of the raw materials used (only for demonstration examples):
[0114] Copper inlay: H3604 copper; choline chloride C108896, ethylene glycol E103319, nickel chloride hexahydrate N112126, cupric chloride dihydrate C111680, halloysite nanotubes H431905, tris(hydroxymethyl)aminomethane hydrochloric acid solution (pH=8.5) T301494, dopamine hydrochloride D103111, 2-(1,3-benzothiazole-2-thio)succinic acid S709757, octylamine O110 545, 3-(2,3-Epoxypropoxy)propyltrimethoxysilane G134407, polytetramethylene ether glycol P118599, isophorone diisocyanate I109582, dibutyltin dilaurate D100274, 2-(perfluorodecyl)ethanol P346518, aminopropyltriethoxysilane A107147: Aladdin reagent; N,N-dimethylformamide, ethanol, acetic acid, butanone, analytical grade, commercially available.
[0115] Performance test: The copper inlays prepared in the embodiments and comparative examples were tested:
[0116] Hydrophobicity: Characterized by water contact angle, tested with a contact angle meter and a 2μL deionized water droplet;
[0117] Wear resistance: Place the copper inlay downward on 800-grit silicon carbide sandpaper, place a 500-gram weight on the copper inlay, and move it back and forth in a straight line for 10 cm per cycle. After 10 cycles, measure the water contact angle again. If the change rate of the water contact angle is between 0-1% (including 1%), it is qualified, otherwise it is unqualified.
[0118] Corrosion resistance: The copper insert was kept at 300℃ for 6h, cooled and placed in a 6% sodium chloride aqueous solution, and immersed at 25℃ for 72h. The surface corrosion morphology was observed. If there was no discoloration or corrosion, it was qualified. Otherwise, it was unqualified. The results are shown in Table 1.
[0119] Table 1
[0120] Water contact angle (°) Wear resistance Corrosion resistance Example 1 154.1 Qualified Qualified Example 2 154.3 Qualified Qualified Example 3 154.8 Qualified Qualified Comparative example 1 149.3 Unqualified Unqualified Comparative example 2 142.7 Unqualified Unqualified
[0121] The present invention provides a corrosion-resistant and wear-resistant copper inlay and a preparation method thereof. By limiting the composition and process, the copper inlay is plated by ionic liquid electroplating, and then the surface of the plated layer is sealed to prepare a hydrophobic, corrosion-resistant and wear-resistant copper inlay, thereby greatly improving the appearance and service life of the copper inlay.
[0122] Comparing Example 3 with Comparative Example 1, it can be seen that in order to improve the problems existing in the existing aqueous solution electroplating process, such as hydrogen embrittlement prone to occur in the coating, easy passivation of the metal anode, and troublesome waste liquid treatment, choline chloride-ethylene glycol with good electrical conductivity and high chemical stability is selected as the solvent in the present invention, and a nickel-copper-halloysite nanotube layer is electrodeposited on the surface of the formed copper insert. The introduction of halloysite nanotubes can effectively reduce the residual stress of the coating, and at the same time improve the hardness, wear resistance and corrosion resistance of the coating. In order to further improve the corrosion resistance of the coating, taking advantage of the unique hollow tubular structure, large specific surface area and high reaction activity of halloysite nanotubes, they are used as nano-loaders of corrosion inhibitors, and then coated with dopamine to obtain composite halloysite nanotubes, which are introduced into the copper insert coating, thereby providing long-term corrosion protection for the copper insert, and at the same time improving the bonding strength between the sealing liquid and the coating to prevent the sealing layer formed by the sealing liquid from falling off.
[0123] Comparing Example 3 with Comparative Example 2, it can be seen that in the sealing liquid, composite halloysite nanotubes are used as fillers and silane-modified polyurethane is used as the base material. The silane-modified polyurethane is a prepolymer synthesized from isophorone diisocyanate and polytetramethylene ether glycol, and 3-(2,3-epoxypropoxy)propyltrimethoxysilane is used as the chain extender with octylamine to open the ring, and 2-(perfluorodecyl)ethanol and aminopropyltriethoxysilane are used as end-capping agents. The structure of the polyurethane prepolymer is modified by functionalized siloxane, and then in the sealing layer, the hydrolysis and condensation of siloxane are used to achieve compatibility with the substrate and strong mechanical properties, endowing the sealing layer with excellent water resistance and high temperature resistance and prolonging the service life of the copper insert.
[0124] The above are only the embodiments of the present invention, and do not limit the patent scope of the present invention accordingly. All equivalent structural transformations made using the description of the present invention under the inventive concept of the present invention, or direct / indirect applications in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a corrosion-resistant and wear-resistant copper inlay, characterized in that: The following steps are involved: S1: sequentially alkali-washing, water-washing, acid-washing, ultrasonic-washing and drying the formed copper insert to obtain a pretreated copper insert; S2: preparing an ionic liquid electroplating solution containing composite halloysite nanotubes, placing the pretreated copper inlay in the ionic liquid electroplating solution, and performing ultrasonic assisted electroplating treatment to obtain an electroplated copper inlay; S3: mixing the composite halloysite nanotubes, silane-modified polyurethane, additives, and solvent to obtain a sealing liquid; S4: coating the sealing liquid on the surface of the electroplated copper inlay and drying it to obtain a corrosion-resistant and wear-resistant copper inlay.
2. The method for preparing a corrosion-resistant and wear-resistant copper inlay according to claim 1, characterized in that: The working conditions of ultrasonic assisted electroplating treatment are: temperature of 68-72°C, time of 30-40min, and ultrasonic power of 280W.
3. The method for preparing a corrosion-resistant and wear-resistant copper insert according to claim 1, characterized in that: The composition of the ionic liquid electroplating solution is: choline chloride-ethylene glycol ionic liquid as solvent, containing 48g / L nickel chloride hexahydrate, 17g / L copper chloride dihydrate, and g / L composite halloysite nanotubes (4-6).
4. The method for preparing a corrosion-resistant and wear-resistant copper insert according to claim 3, characterized in that: The choline chloride-ethylene glycol ionic liquid is prepared by compounding choline chloride and ethylene glycol in a molar ratio of 1:
2.
5. The method for preparing a corrosion-resistant and wear-resistant copper insert according to claim 1, characterized in that: The sealing liquid comprises, by weight, 1-5 parts of composite halloysite nanotubes, 12-24 parts of silane-modified polyurethane, 0.5-1 parts of auxiliary agent and 11-16 parts of solvent.
6. The method for preparing a corrosion-resistant and wear-resistant copper insert according to claim 1, characterized in that: The solvent is prepared by mixing N,N-dimethylformamide, ethanol and deionized water in a mass ratio of 3:2:1; the auxiliary agent is one of formic acid and acetic acid.
7. The method for preparing a corrosion-resistant and wear-resistant copper insert according to claim 1, characterized in that: The preparation of the composite halloysite nanotubes comprises the following steps: (1) mixing a corrosion inhibitor and ethanol, adding halloysite nanotubes, ultrasonically treating for 10-20 min, transferring to a vacuum drying oven and evacuating for 1-2 h before taking out, repeating the evacuation and taking out process 3-5 times, centrifuging, washing, and drying to obtain pretreated halloysite nanotubes; (2) The tris(hydroxymethyl)aminomethane hydrochloric acid solution, the pretreated halloysite nanotubes and dopamine hydrochloride are mixed, stirred for 10-12 hours in the dark, centrifuged, washed with water and dried to obtain composite halloysite nanotubes.
8. The method for preparing a corrosion-resistant and wear-resistant copper insert according to claim 7, characterized in that: The corrosion inhibitor is one of 2-(1,3-benzothiazole-2-thio)succinic acid, sodium gluconate and benzotriazole.
9. The method for preparing a corrosion-resistant and wear-resistant copper insert according to claim 1, characterized in that: The preparation of the silane-modified polyurethane comprises the following steps: 1) octylamine and 3-(2,3-epoxypropoxy)propyltrimethoxysilane are mixed, and stirred at 18-25° C. for 22-24 hours to obtain a silane chain extender; 2) Under a nitrogen atmosphere, polytetramethylene ether glycol, isophorone diisocyanate and butanone are mixed, dibutyltin dilaurate is added, the temperature is raised to 68-72°C and kept for 3-4 hours, the temperature is lowered by 18-25°C, a chain extender is added, the temperature is raised to 68-72°C and stirred for 2-3 hours, 2-(perfluorodecyl)ethanol and aminopropyltriethoxysilane are added and stirred for 1-2 hours to obtain a silane-modified polyurethane.
10. A corrosion-resistant and wear-resistant copper insert, characterized in that: Prepared by the method according to any one of claims 1 to 9.
Citation Information
Cited By
PPO / PPE chip packaging test tray material
CN121758952A
Low-VOC (volatile organic compound) waterborne epoxy anticorrosive paint and production process thereof
CN122080732A
Low-voc water-based epoxy anticorrosive coating and production process thereof
CN122080732B