Smelting method for improving cleanliness of austenitic stainless steel
Through the multi-step smelting process of electric furnace melting and AOD and LF refining, the problem of high inclusion level of 304 stainless steel is solved, and the production of high cleanliness of stainless steel is achieved, meeting the quality requirements of high-end products.
Patent Information
- Application Number
- CN202510372148.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-27
- Publication Date
- 2025-06-20
- Estimated Expiration
- 2045-03-27
AI Technical Summary
In the prior art, the immature process of 304 stainless steel leads to a high level of inclusions, which cannot meet the high requirements for cleanliness of high-end 304 stainless steel products.
The raw materials are melted by electric furnaces, and multiple reduction and deoxygenation are carried out through the AOD and LF refining process to control the alkalinity of the slag, the temperature of the molten steel, argon blowing and stirring process parameters to ensure the cleanliness of the finished product.
Through this smelting method, the inclusion level of stainless steel can be significantly reduced, so that it reaches ≤1.0, and meets the cleanliness requirements of high-end 304 stainless steel products.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the field of smelting, and particularly to a smelting method for improving the cleanliness of austenitic stainless steel. Background Art
[0002] The control of steel cleanliness is an inevitable trend in the development of steel materials. Cleanliness is an important indicator reflecting the overall quality level of steel, usually evaluated by the content of harmful elements in molten steel and the quantity, morphology, and size of non-metallic inclusions. Among them, non-metallic inclusions are an important factor affecting the cleanliness of molten steel. Austenitic stainless steel refers to stainless steel with austenite structure at room temperature. When the steel contains about 18% Cr, 8% - 25% Ni, and about 0.1% C, it has a stable austenite structure. As the stainless steel grade with the largest output in China, 304 austenitic stainless steel has been widely used in people's daily lives. Some high-end 304 austenitic stainless steel products are used in the production of mobile phone cases and watch chains, so there are high requirements for the surface quality of stainless steel products. At present, there are problems such as surface line scale defects and dot-like defects after polishing in the high-end 304 stainless steel independently produced in China, which seriously affect the surface aesthetics of its finished products. This is mainly caused by inclusions in the stainless steel. For high-end 304 steel, the requirements for various types of inclusions A, B, C, and D are all ≤ 1.0 grade. However, due to immature processes in current production, the inclusion level often ranges from 1.5 to 2.0 grades, and in severe cases, 2.5-grade inclusions will appear, which cannot meet the current production requirements. The control of inclusions in 304 stainless steel is of great significance for Chinese enterprises to achieve the production of high-end 304 stainless steel. Summary of the Invention
[0003] In order to solve the problem of high inclusion levels caused by immature processes of 304 stainless steel in the prior art, the present invention proposes a smelting method for improving the purity of austenitic stainless steel.
[0004] In order to achieve the above-mentioned invention purpose, the present invention provides the following technical solutions: A smelting method for improving the cleanliness of austenitic stainless steel, comprising the following steps: melting raw materials in an electric furnace and tapping; AOD refining; LF refining; In the AOD refining, adding reducing slag materials such as quicklime and fluorite to make slag, controlling the target requirement of the basicity of the reducing slag (R = CaO / SiO2) at 2.1 - 2.2, and adding 0.5 - 0.8 kg / t of steel of aluminum pellets; In the LF refining, using CaSi powder for diffusion deoxidation, and controlling the soft blowing argon time at 15 - 20 min.
[0005] Preferably, in the steps of the smelting method for improving the cleanliness of austenitic stainless steel, when tapping, the C element content is 1.9 - 2.2%, and the Si element content ≤ 0.8%.
[0006] Further preferably, the tapping temperature is 1640 - 1660 °C.
[0007] Preferably, the AOD refining includes the following steps: (1) AOD oxygen blowing for decarburization; (2) Primary reduction with FeSi; (3) After the primary reduction is completed, tilt the furnace to remove the slag. For the secondary reduction, add flux materials such as quicklime and fluorite to form slag. Control the basicity of the reducing slag (R = CaO / SiO2) to the target requirement of 2.1 - 2.2. Add 0.5 - 0.8 kg / t of steel with aluminum pellets, and the rest is reduced with calcium-silicon blocks.
[0008] Further preferably, during the AOD oxygen blowing for decarburization in step (1), the temperature of the molten steel is maintained at 1680 - 1730 °C while adding flux materials.
[0009] Further preferably, the target control of Si in the primary reduction in step (2) is 0.25 - 0.45%.
[0010] Preferably, the LF refining includes the following steps: (1) After the LF arrives, turn on the argon gas. Stir with high-flow argon to break the slag crust. After the ladle car is moved to the heating station, measure the temperature, take samples, and adjust the argon gas flow rate before energizing to raise the temperature; (2) Use CaSi powder for diffusion deoxidation, do not use Al for deoxidation, and control the oxygen content to ≤25 ppm; (3) Take samples after the slag is fully white and the temperature ≥1560 °C. Precisely adjust the composition according to the analysis results according to the internal control composition standard, and maintain the white slag for ≥20 minutes; (4) After the composition meets the internal control standard range, start stirring with high-flow argon. After stirring for 8 - 10 minutes, the diameter of the Ar gas ring ≥300 mm without exposing the molten steel surface. Start feeding calcium wire at 4 - 6 m / t. After feeding, start soft argon blowing operation for 15 - 20 minutes, and then lift the ladle for casting.
[0011] Further preferably, the internal control composition standard is: C: ≤0.020%; Si: 0.30 - 0.50%; Mn: 0.95 - 1.05%; P: ≤0.035%; S: ≤0.001%; Ni: 8.05 - 8.12%; Cr: 18.15 - 18.35%; Fe: balance.
[0012] Further preferably, the casting temperature is 1530 - 1540 °C.
[0013] The raw materials described in step (1) include scrap steel, high-carbon ferrochrome, aluminum pellets, nickel plates, and high-carbon ferromanganese or ferrosilicon.
[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) By selecting and adjusting the dosage of deoxidizers in the refining processes of AOD and LF furnaces, and taking into account various adjustments such as the basicity of slag making, molten steel temperature control, argon blowing, and stirring, the final smelted product achieves the purpose of the present invention.
[0015] (2) The present invention can meet the requirements for inclusions in current high-end 304 austenitic stainless steel, reducing the inclusions from grade 1.5 or 2.0 to ≤1.0 grade. Specific Embodiments
[0016] The present invention will be further described below in conjunction with specific embodiments. The advantages and features of the present invention will be more clearly reflected in the description. However, the embodiments are only for demonstration and do not constitute any limitation to the scope of the present invention. Those skilled in the art should understand that without departing from the spirit and scope of the present invention, they can modify or replace the details and forms of its technical solutions, and these modifications and replacements all fall within the protection scope of the present invention.
[0017] Embodiment 1 A smelting method for improving the cleanliness of austenitic stainless steel, comprising the following steps: (1) Melting raw materials in an electric furnace, including scrap steel, high-carbon ferrochrome, aluminum pellets, nickel plates, and high-carbon ferromanganese. The C content of the tapped steel is 1.9%, the Si content is 0.6%, and the tapped temperature is 1648°C; (2) Refining in an AOD furnace: 1) During AOD oxygen blowing for decarburization, adding slag materials to blow and refine the molten steel temperature to 1688°C; 2) Primary reduction process: Reducing with FeSi, controlling Si at 0.28%; 3) Secondary reduction: After the primary reduction is completed, tilting the furnace to remove slag. For secondary reduction, adding reducing slag materials such as quicklime and fluorite to make slag, controlling the target requirement of the basicity of the reducing slag (R = CaO / SiO2) at 2.1, adding 0.6 kg / t of molten steel of aluminum pellets, and using calcium silicide blocks for the rest of the reduction; (3) Refining in an LF furnace: 1) After the LF furnace arrives, turn on the argon gas, stir with large argon gas to break the slag crust. After the ladle car is driven to the heating station, measure the temperature, take samples, and adjust the argon gas flow rate and then send power to raise the temperature.
[0018] 2) Using CaSi powder for diffusion deoxidation, not using Al for deoxidation, controlling oxygen at 23 ppm.
[0019] 3) Sampling when the furnace slag is fully white and the temperature is 1562°C, accurately adjusting the composition according to the analysis results according to the internal control composition, and maintaining the white slag for 25 minutes.
[0020] 4) After the components meet the internal control standard range, start large argon stirring. After stirring for 8 minutes (the diameter of the Ar gas circle is 350 mm without exposing the molten steel surface), the calcium treatment process: feed 4 m / t of calcium wire; after feeding, start soft argon blowing operation, the soft blowing time is 18 minutes, and then lift the ladle for casting, the casting temperature: 1532 °C.
[0021] In this embodiment, the component control is carried out according to the internal control standard in Table 1.
[0022] Table 1. Component control standard of austenitic stainless steel in Example 1
[0023] Example 2 A smelting method for improving the cleanliness of austenitic stainless steel, comprising the following steps: (1) The electric furnace melts raw materials including scrap steel, high-carbon ferrochrome, aluminum pellets, nickel plates, and high-carbon ferromanganese. The C content of the molten steel tapped: 2.1%, the Si content 0.8%, and the tapping temperature: 1658 °C; (2) AOD furnace: 1) During the AOD oxygen blowing decarburization, add slag materials and blow the molten steel at a temperature of 1708 °C; 2) Primary reduction process: FeSi reduction, with Si controlled at 0.3%; 3) Secondary reduction: After the primary reduction is completed, tilt the furnace to remove the slag. During the secondary reduction, add reducing slag materials such as quicklime and fluorite to make slag, and control the target requirement of the reduction slag basicity (R = CaO / SiO2) at 2.2. Add 0.7 kg / t of molten steel of aluminum pellets, and the rest is reduced with calcium silicide blocks; (3) LF furnace: 1) After the LF arrives, turn on the argon gas, and use large argon stirring to break the slag crust. After the ladle car is driven to the heating station, measure the temperature, take samples, and adjust the argon gas flow rate and then power on to raise the temperature.
[0024] 2) Use CaSi powder for diffusion deoxidation and do not use Al for deoxidation. The oxygen control target is 20 ppm.
[0025] 3) Take samples when the furnace slag is fully white and the temperature is 1568 °C. According to the analysis results, accurately adjust the components according to the internal control components (the same as in Example 1), and keep the white slag for 30 minutes.
[0026] 4) Argon stirring process: After the components meet the internal control standard range, start large argon stirring. After stirring for 9 minutes (the diameter of the Ar gas circle is 320 mm without exposing the molten steel surface), the calcium treatment process: feed 4.5 m / t of calcium wire; the soft blowing time is 18 minutes.
[0027] Lift the ladle for casting, the casting temperature: 1535 °C.
[0028] Comparative Example 1 A smelting method for austenitic stainless steel, comprising the following steps: (1)The raw materials melted in the electric furnace include scrap steel, high-carbon ferrochrome, aluminum pellets, nickel plates, and high-carbon ferromanganese. The C content of the molten steel tapped is 2.0%, the Si content is 0.3%, and the tapping temperature is 1648°C; (2)AOD furnace: 1) During the AOD oxygen blowing for decarburization, slag materials are added and the molten steel temperature is blown to 1690°C; 2) Primary reduction process: Si is controlled at 0.3%; 3) Secondary reduction: The target requirement for controlling the basicity of the reducing slag (R = CaO / SiO2) is 1.7, and 0.6 kg / t of molten steel of aluminum pellets is added; (3)LF furnace: 1) After the LF arrives, argon is turned on, and the large argon stirring breaks the slag crust. After the ladle car is driven to the heating station, the temperature is measured, samples are taken, and the argon flow rate is adjusted and power is supplied to raise the temperature; 2) CaSi powder is used for diffusion deoxidation, and Al is not used for deoxidation; the oxygen control target is 20 ppm; 3) The white slag holding time is 24 minutes; 4) Argon stirring process: After the composition meets the internal control standard range, large argon stirring starts. After stirring for 8 minutes (the Ar gas ring diameter is 350 mm without exposing the molten steel surface), the calcium treatment process: 4 m / t of calcium wire is fed; the soft blowing time is 10 minutes. The ladle is lifted for pouring, and the pouring temperature is: 1535°C.
[0029] Comparative Example 2 A smelting method for austenitic stainless steel, comprising the following steps: (1)The raw materials are melted in the electric furnace. The C content of the molten steel tapped is 1.9%, the Si content is 0.4%, and the tapping temperature is 1645°C; (2)AOD furnace: 1) During the AOD oxygen blowing for decarburization, slag materials are added and the molten steel temperature is blown to 1700°C; 2) Primary reduction process: FeSi reduction, Si is controlled at 0.40%; 3) Secondary reduction: The target requirement for controlling the basicity of the reducing slag (R = CaO / SiO2) is 2.0, and 1 kg / t of molten steel of aluminum pellets is added; (3)LF furnace: 1) After the LF arrives, argon is turned on, and the large argon stirring breaks the slag crust. After the ladle car is driven to the heating station, the temperature is measured, samples are taken, and the argon flow rate is adjusted and power is supplied to raise the temperature; 2) Al is used for deoxidation, and the oxygen control target is 21 ppm; 3) The white slag holding time is 24 minutes; 4) Argon stirring process: After the composition meets the internal control standard range, start large argon stirring. After stirring for 8 minutes (the diameter of the Ar gas ring is 310 mm without exposing the molten steel surface), calcium treatment process: Feed 6 m / t of calcium wire; soft blowing time is 15 minutes. Lift the ladle for pouring, pouring temperature: 1535 °C.
[0030] The head and tail positions of the ingots produced according to the steps described in Examples 1 and 2 and Comparative Examples 1 and 2 were inspected and analyzed, and the results are shown in Table 2.
[0031] Table 2. Inspection and analysis results of the head and tail positions of the ingots produced in the examples and comparative examples
[0032] Note: The upper and lower rows in the above table are the inspection results of the relative head and tail positions of the ingot respectively.
[0033] Through the comparison of the inclusion inspection results between the above examples and comparative examples, the inclusion results of the examples produced according to the process set in this scheme are all ≤ 1.0 grade, meeting the requirements of high-end 304 steel that the inclusion levels of types A, B, C, and D are all required to be ≤ 1.0 grade. However, the inclusion levels of the finished products produced in the comparative examples have B and D types exceeding 1.0 grade, not meeting the requirements.
Claims
1. A smelting method for improving the cleanliness of austenitic stainless steel, characterized in that: The following steps are involved: The electric furnace melts the raw materials and produces steel; AOD refining; LF refining; In the AOD refining, lime and fluorite are added to make slag, the basicity R of the reduced slag is controlled to be 2.1-2.2, and 0.5-0.8 kg / t of aluminum particles are added; In the LF refining, CaSi powder is used for diffusion deoxidation, and the soft argon blowing time is controlled at 15-20 minutes.
2. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 1, characterized in that: When the steel is tapped, the C content is 1.9-2.2%, and the Si content is ≤0.8%.
3. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 1, characterized in that: The temperature of the steel tapping is 1640-1660°C.
4. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 1, characterized in that: The AOD refining comprises the following steps: (1) AOD oxygen decarburization; (2) Perform a reduction with FeSi; (3) After the first reduction, the furnace is shaken and the slag is removed. For the second reduction, lime and fluorite are added to make slag. The basicity of the reducing slag (R=CaO / SiO2) is controlled at a target of 2.1-2.
2. 0.5-0.8 kg / t of aluminum particles are added, and the rest is reduced with silicon-calcium blocks.
5. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 4, characterized in that: During the AOD oxygen decarburization process, the temperature of the molten steel is maintained at 1680-1730°C by adding slag.
6. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 4, characterized in that: Step (2) The primary reduction Si control target is 0.25-0.45%.
7. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 1, characterized in that: The LF refining comprises the following steps: (1) After the LF is in place, the argon gas is connected, and the large amount of argon gas is stirred to break the slag shell. After the ladle car drives to the heating station, the temperature is measured and sampled, and the argon gas flow is adjusted before power is supplied to increase the temperature; (2) Use CaSi powder for diffusion deoxidation, do not use Al for deoxidation, and the oxygen control target is ≤25ppm; (3) After the slag has fully turned white and the temperature is ≥1560°C, take a sample and accurately adjust the composition according to the internal control composition standard based on the analysis results. The white slag should be kept for ≥20 minutes; (4) After the composition meets the internal control standard range, start large argon stirring. After stirring for 8-10 minutes, the diameter of the Ar gas ring is ≥300mm and does not expose the steel liquid surface. Start feeding the calcium wire at 4-6m / t. After feeding, start soft argon blowing operation. The soft blowing time is 15-20 minutes, and then pouring by hanging ladle.
8. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 7, characterized in that: The internal control component standards are: C: ≤0.020%; Si: 0.30~0.50%; Mn: 0.95~1.05%; P: ≤0.035%; S: ≤0.001%; Ni:8.05~8.12%; Cr: 18.15~18.35%; Fe: balance.
9. The smelting method for improving the cleanliness of austenitic stainless steel according to claim 7, characterized in that: The pouring temperature is 1530~1540℃.
Citation Information
Patent Citations
Method for controlling plastic inclusions of austenitic stainless steel
CN105567907A
Smelting method of high-purity austenitic stainless steel
CN111910045A
Austenite stainless steel with good weldability
JP1978071616A
Argon oxygen decarburization refining method for molten austenitic stainless steel
US20170175212A1
Stainless steel with good mirror polishability and method for producing same
US20230115048A1
Cited By
Smelting process of high-purity 304 stainless steel bar
CN120945169A