Application method of micro-phase separated polyimide sizing agent for carbon fibers

By applying a micro-phase separated polyimide sizing agent on the surface of the carbon fiber, the problem of poor compatibility between carbon fiber and matrix material is solved, and the interface binding performance is improved and the mechanical properties are optimized.

CN120211117APending Publication Date: 2025-06-27DONGHUA UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202510341821.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-21
Publication Date
2025-06-27

AI Technical Summary

Technical Problem

The poor compatibility of carbon fiber and matrix materials leads to weak interface bonding force, affecting the mechanical properties of carbon fiber reinforced composite materials.

Method used

Using a micro-phase separated polyimide sizing agent, a polyamic acid arranged alternately in rigid and flexible segments is synthesized by dianhydride monomer and diamine monomer as raw materials, and a body self-assembled by heat treatment to form a micro-phase separated polyimide coating.

Benefits of technology

It effectively improves the interface combination performance between carbon fiber and matrix material, balances the strength and toughness of the interface layer, and improves the mechanical properties of the composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120211117A_ABST
    Figure CN120211117A_ABST
Patent Text Reader

Abstract

The invention relates to a use method of a micro-phase separated polyimide sizing agent for carbon fibers, which comprises the following steps: synthesizing polyamide acid with rigid and flexible chain segments alternately arranged by using a dianhydride monomer and a diamine monomer as raw materials, coating the polyamide acid on the surface of the carbon fibers, carrying out heat treatment, carrying out thermal cyclization on the polyamide acid to form polyimide, and carrying out body self-assembly at the same time, thereby obtaining the micro-phase separated polyimide sizing agent for the carbon fibers. And thus, the micro-phase separated polyimide coating is obtained. According to the method, the interface performance of the carbon fibers and the base material in the carbon fiber composite material can be improved, the thermal cyclization process of the sizing agent and microphase separation of the obtained surface coating are achieved at the same time through the heat treatment one-step method, and procedures and energy are saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of material surface treatment and modification, and particularly relates to a method for using a polyimide sizing agent for microphase-separated carbon fibers. Background Art

[0002] Carbon fibers have the advantages of high specific strength, high specific modulus, high temperature resistance, corrosion resistance, etc., and are widely used in many fields such as aerospace, weaponry, rail transit, electronic communication, and cultural and sports products. They are one of the important materials that affect national security and development, as well as national economic life. Carbon fibers are often used as a reinforcing phase, and carbon fiber reinforced composites are obtained by compounding with matrix materials such as resins. However, the chemical composition of carbon fibers is non-polar, and their surface is relatively inert. This results in poor compatibility and weak interfacial bonding force between carbon fibers and resins, ultimately leading to unsatisfactory mechanical properties of carbon fiber reinforced composites.

[0003] To solve the compatibility problem between carbon fibers and matrix materials, various methods have been developed to modify the surface of carbon fibers. Among them, sizing treatment of fibers is one of the most widely used methods in industry. By forming a coating on the surface of carbon fibers with a sizing agent, which serves as the interface between the fiber and the matrix during compounding, the interfacial properties can be effectively improved, and ultimately the mechanical properties of the resulting composite materials can be enhanced. This method has the advantages of not damaging the fibers, simple process, and easy operation.

[0004] The key to the sizing method lies in the preparation and selection of the sizing agent. Commonly used sizing agent materials include epoxy resins, polyimides, and their composites with various nanomaterials (such as titanium dioxide nanoparticles, graphene, carbon nanotubes, etc.). As the "intermediate layer" between the carbon fiber reinforcing phase and the matrix material, factors such as the chemical composition, molecular arrangement form, and thickness of the coating formed by the sizing agent on the fiber surface directly determine key processes such as stress bearing and transfer in the composite material, and thus affect the macroscopic mechanical properties of the material. When the strength of the sizing agent coating is relatively high, the strength of the composite material is also relatively high, but the brittleness also increases accordingly; when the toughness of the sizing agent coating increases, the toughness of the composite material also increases, but the strength will decrease. That is to say, the sizing agent coating also faces the contradiction between strength and toughness. Bai Yongping et al. reported a "soft-hard" combined sizing agent interface coating, which was coated on the surface of carbon fibers by blending flexible polyethyleneimine (PEI) with rigid metal-organic framework / graphene oxide composite (MOF / GO), effectively improving the interfacial properties of carbon fiber reinforced polymer materials (Composites Part B, 2022, 236, 109846.). However, its soft and hard parts are obtained by blending and do not have an ordered arrangement. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a method for using a polyimide sizing agent for microphase-separated carbon fibers to enhance the interfacial bonding performance between the carbon fibers and the matrix material of the material.

[0006] The present invention provides a method for using a polyimide sizing agent for microphase-separated carbon fibers. Using dianhydride monomers and diamine monomers as raw materials, polyamic acid with alternating rigid and flexible chain segments is synthesized. It is coated on the surface of carbon fibers and heat-treated. While the polyamic acid undergoes thermal cyclization to become polyimide, bulk self-assembly occurs, thereby obtaining a microphase-separated polyimide coating.

[0007] Preferably, the molar ratio of the dianhydride monomer to the diamine monomer is 0.9 - 1.1:1.

[0008] Preferably, the dianhydride monomer includes but is not limited to at least one of the following compounds:

[0009]

[0010] Furthermore, the above compounds (a-1) - (a-6) are pyromellitic dianhydride (PMDA), 3,3′,4,4′-biphenyltetracarboxylic dianhydride (BPDA), 2,3,3′,4-biphenyltetracarboxylic dianhydride (α-BPDA), 3,3′,4,4′-benzophenone tetracarboxylic dianhydride (BTDA), diphenyl ether tetracarboxylic dianhydride (ODPA), 1,2,4,5-cyclohexanetetracarboxylic dianhydride (CHTDA) in sequence.

[0011] Preferably, the diamine monomer includes but is not limited to at least one of the following compounds:

[0012]

[0013] Among them, the value of n in compound (b-1) is 1, 2, 3, 4 or 5; the molecular weight of compound (b-2) is 400 - 2000 Da.

[0014] Furthermore, the above compounds (b-1) - (b-2) are amino-terminated polyethylene glycol vinyl ether (PEGBA), amino-terminated polypropylene glycol vinyl ether (PPGBA) in sequence.

[0015] Preferably, the thickness of the polyimide coating is 20 - 500 nm.

[0016] Preferably, the polyamic acid is diluted with an organic solvent to 0.2 wt% - 2 wt% and coated on the surface of carbon fibers by the dipping method, and the dipping time is 5 - 30 s.

[0017] Preferably, the heat treatment temperature is 180 - 250 °C, and the heat treatment time is 2 - 12 h.

[0018] Preferably, the above sizing agent is prepared by the following method: completely dissolve diamine monomers in an organic solvent under nitrogen protection, then place it in an ice-water bath to cool, and then add dianhydride monomers under stirring. React the reaction system under nitrogen protection to obtain a viscous polyamic acid solution.

[0019] Preferably, the solid content of the reaction system is 10 wt% - 30 wt%; the reaction time is 8 - 24 h.

[0020] Preferably, the organic solvent includes any one of N,N-dimethylacetamide (DMAc) or N-methylpyrrolidone (NMP).

[0021] The present invention provides a polyimide sizing agent based on the alternating arrangement of hard and soft segments. After coating it on the surface of carbon fiber as a sizing agent, during the heat treatment process, it undergoes bulk self-assembly, and the hard and soft segments will undergo microphase separation to obtain an orderly arranged "soft phase" and "hard phase" respectively. Figure 1 It is a schematic diagram of the formation of a microphase separation coating of the polyimide sizing agent on the surface of carbon fiber. The highly regular structure will effectively alleviate the contradiction between the strength and toughness of the composite material interface layer and improve the mechanical properties of the composite material.

[0022] Beneficial effects

[0023] (1) Through the optimized design of the molecular structure, the present invention obtains a polyimide sizing agent with an alternating arrangement of hard and soft segments. After sizing by the impregnation method and heat treatment, the polyimide on the surface of carbon fiber will not only complete the cyclization reaction but also undergo bulk self-assembly to obtain a microphase separation coating. The relatively rigid and relatively soft microphases coexist, effectively balancing the strength and toughness of the interface layer, thereby improving the interfacial performance between carbon fiber and matrix material in the carbon fiber composite material.

[0024] (2) Through heat treatment, the present invention simultaneously realizes the thermal cyclization process of the sizing agent and the microphase separation of the obtained surface coating in one step, effectively reducing equipment requirements and saving processes and energy.

[0025] (3) The raw materials of the present invention are easily available, the operation is simple, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the formation of a microphase separation coating of the polyimide sizing agent in the present invention on the surface of carbon fiber. DETAILED DESCRIPTION OF THE INVENTION

[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and not to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of this application.

[0028] The raw materials used in the following examples and comparative examples of the present invention are all commercially available products. The carbon fibers used are all carbon fibers of model T700SC produced by Toray Industries, Inc. of Japan, and are subjected to desizing treatment by Soxhlet extraction before sizing.

[0029] The interfacial shear strength (IFSS) of the composites of the sized carbon fibers in the examples and comparative examples of the present invention was tested. The matrix material in the composites was selected as epoxy resin E51.

[0030] Example 1

[0031] PEGBA (n = 2) (14.6 g) was dissolved in anhydrous DMAc (100 mL, 93.7 g) at room temperature and stirred thoroughly under nitrogen protection for dissolution. After 1 h, the reaction system was immersed in an ice-water bath for cooling, and then stoichiometric PMDA (21.6 g) was added to the flask while stirring. The mixture was stirred in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0032] A portion of the polyamic acid solution was taken and diluted with DMAc to a solid content of 1 wt%. Then, the carbon fibers were sized by the dipping method. The dipping time was 30 s, and after taking out, it was heat-treated at 180 °C for 12 h.

[0033] Example 2

[0034] PEGBA (n = 2) (16.1 g) was dissolved in anhydrous DMAc (100 mL, 93.7 g) at room temperature and stirred thoroughly under nitrogen protection for dissolution. After 1 h, the reaction system was immersed in an ice-water bath for cooling, and then stoichiometric PMDA (23.8 g) was added to the flask while stirring. The mixture was stirred in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0035] A portion of the polyamic acid solution was taken and diluted with DMAc to a solid content of 1 wt%. Then, the carbon fibers were sized by the dipping method. The dipping time was 20 s, and after taking out, it was heat-treated at 230 °C for 12 h.

[0036] Example 3

[0037] Dissolve PEGBA (n = 2) (14.6 g) in anhydrous NMP (100 mL, 103 g) at room temperature, and stir well to dissolve under nitrogen protection. After 1 h, immerse the reaction system in an ice-water bath for cooling, and then add stoichiometric PMDA (21.6 g) to the flask while stirring. Stir the mixture in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0038] Take a part of the polyamic acid solution and dilute it with NMP to a solid content of 0.5 wt%. Then, size the carbon fiber by the dipping method. The dipping time is 30 s, and after taking it out, heat-treat it at 180 °C for 12 h.

[0039] Example 4

[0040] Dissolve PEGBA (n = 2) (14.6 g) in anhydrous DMAc (150 mL, 140.6 g) at room temperature, and stir well to dissolve under nitrogen protection. After 1 h, immerse the reaction system in an ice-water bath for cooling, and then add stoichiometric BPDA (29.4 g) to the flask while stirring. Stir the mixture in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0041] Take a part of the polyamic acid solution and dilute it with DMAc to a solid content of 1.5 wt%. Then, size the carbon fiber by the dipping method. The dipping time is 25 s, and after taking it out, heat-treat it at 180 °C for 10 h.

[0042] Example 5

[0043] Dissolve PEGBA (n = 3) (19.2 g) in anhydrous DMAc (120 mL, 112.5 g) at room temperature, and stir well to dissolve under nitrogen protection. After 1 h, immerse the reaction system in an ice-water bath for cooling, and then add stoichiometric PMDA (21.6 g) to the flask while stirring. Stir the mixture in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0044] Take a part of the polyamic acid solution and dilute it with DMAc to a solid content of 0.8 wt%. Then, size the carbon fiber by the dipping method. The dipping time is 30 s, and after taking it out, heat-treat it at 180 °C for 12 h.

[0045] Example 6

[0046] Dissolve PPGBA (n = 2) (13.2 g) in anhydrous DMAc (100 mL, 93.7 g) at room temperature, and stir well to dissolve under nitrogen protection. After 1 h, immerse the reaction system in an ice-water bath for cooling, and then add stoichiometric PMDA (21.6 g) to the flask while stirring. Stir the mixture in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0047] Take a portion of the polyamic acid solution and dilute it with DMAc to a solid content of 2 wt%. Then, the carbon fibers are sized by the dipping method. The dipping time is 10 s, and after taking out, it is heat-treated at 220 °C for 12 h.

[0048] Comparative Example 1

[0049] Dissolve p-phenylenediamine PDA (10.8 g) in anhydrous DMAc (100 mL, 93.7 g) at room temperature, and stir well to dissolve under nitrogen protection. After 1 h, immerse the reaction system in an ice-water bath for cooling, and then add stoichiometric PMDA (21.6 g) to the flask while stirring. Stir the mixture in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0050] Take a portion of the polyamic acid solution and dilute it with DMAc to a solid content of 1 wt%. Then, the carbon fibers are sized by the dipping method. The dipping time is 30 s, and after taking out, it is heat-treated at 180 °C for 12 h.

[0051] Comparative Example 2

[0052] Dissolve 4′,4-diaminodiphenyl ether ODA (15.2 g) in anhydrous DMAc (100 mL, 93.7 g) at room temperature, and stir well to dissolve under nitrogen protection. After 1 h, immerse the reaction system in an ice-water bath for cooling, and then add stoichiometric PMDA (21.6 g) to the flask while stirring. Stir the mixture in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0053] Take a portion of the polyamic acid solution and dilute it with DMAc to a solid content of 1 wt%. Then, the carbon fibers are sized by the dipping method. The dipping time is 30 s, and after taking out, it is heat-treated at 180 °C for 12 h.

[0054] Comparative Example 3

[0055] Dissolve PEGBA (n = 2) (14.6 g) in anhydrous DMAc (100 mL, 93.7 g) at room temperature, and stir well to dissolve under nitrogen protection. After 1 h, immerse the reaction system in an ice-water bath for cooling, and then add stoichiometric PMDA (21.6 g) to the flask while stirring. Stir the mixture in a nitrogen atmosphere for 12 h to obtain a viscous polyamic acid solution.

[0056] Take a portion of the polyamic acid solution and dilute it with DMAc to a solid content of 1 wt%. Then, the carbon fibers are sized by the dipping method. The dipping time is 30 s, and after taking out, it is left to stand and dry at room temperature.

[0057] Table 1 shows the test results of the interfacial shear strength of the composites of the sized carbon fibers in the above-mentioned examples and comparative examples. It can be seen from Table 1 that compared with the sizing agent in the comparative example, the sizing agent in the examples of the present invention can significantly improve the interfacial bonding performance between the carbon fiber and the matrix material.

[0058] Table 1 Interfacial Shear Strength of Sized Carbon Fiber Composites in Examples and Comparative Examples

[0059]

Claims

1. A method for using a polyimide sizing agent for microphase-separated carbon fiber, characterized in that: Polyamic acid with alternating rigid and flexible segments is synthesized using dianhydride monomers and diamine monomers as raw materials, which is then coated on the surface of carbon fiber and heat-treated. The polyamic acid is thermally cyclized into polyimide and bulk self-assembles to obtain a microphase-separated polyimide coating.

2. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 1, characterized in that: The molar ratio of the dianhydride monomer to the diamine monomer is 0.9-1.1:

1.

3. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 2, characterized in that: The dianhydride monomer includes at least one of the following compounds:

4. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 2, characterized in that: The diamine monomer includes at least one of the following compounds: The value of n in compound (b-1) is 1, 2, 3, 4 or 5; the molecular weight of compound (b-2) is 400 to 2000 Da.

5. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 1, characterized in that: The thickness of the polyimide coating is 20-500 nm.

6. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 1, characterized in that: The polyamic acid is diluted with an organic solvent to 0.2 wt% to 2 wt% and coated on the surface of the carbon fiber by an immersion method, and the immersion time is 5 to 30 seconds.

7. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 1, characterized in that: The heat treatment temperature is 180-250° C., and the heat treatment time is 2-12 hours.

8. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 1, characterized in that: The sizing agent is prepared by the following method: a diamine monomer is completely dissolved in an organic solvent under nitrogen protection, then placed in an ice water bath for cooling, then a dianhydride monomer is added under stirring, and the reaction system is reacted under nitrogen protection to obtain a viscous polyamic acid solution.

9. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to claim 8, characterized in that: The solid content of the reaction system is 10wt% to 30wt%; and the reaction time is 8 to 24h.

10. The method for using the polyimide sizing agent for microphase-separated carbon fiber according to any one of claims 6 or 8, characterized in that: The organic solvent includes any one of N,N-dimethylacetamide and N-methylpyrrolidone.

Citation Information

Cited By

  • Hyperbranched polyimide modified carbon fiber resin-based composite material as well as preparation method and application thereof

    CN121182200A

  • High-temperature-resistant water-based sizing agent as well as preparation method and application thereof

    CN122103571A

  • Imide derivative monomer containing electroactive group as well as preparation method and application of imide derivative monomer

    CN122355915A