Electrochemical capacitor

By optimizing the ratio of dispersant and adhesive in the negative electrode mixture layer and forming a specific layer structure on the surface, the problem of gas generation at high temperature of the lithium ion capacitor is solved, and good floating charge characteristics and resistance performance are achieved.

CN120418912APending Publication Date: 2025-08-01PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380087475.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-23
Filing Date
2023-11-06
Publication Date
2025-08-01

AI Technical Summary

Technical Problem

When the lithium-ion capacitor is used for a long time at high temperature, gas is generated due to the decomposition of the electrolyte, resulting in poor floating charging characteristics, and the gas stays between the electrodes and reduces the opposing area.

Method used

In the negative electrode mixture layer, the mass ratio of the dispersant is greater than that of the adhesive, and the negative electrode mixture layer composed of the negative electrode active material, conductive additive, adhesive and dispersant is formed on the surface of the negative electrode mixture layer, and the first layer containing lithium carbonate and the second layer of solid electrolyte are suppressed, and gas generation is maintained and good adhesion is maintained.

Benefits of technology

It effectively suppresses the gas generated by the decomposition of the electrolyte, maintains the floating charging characteristics of the electrochemical capacitor, and improves the durability and resistance performance of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120418912A_ABST
    Figure CN120418912A_ABST
Patent Text Reader

Abstract

The disclosed electrochemical capacitor comprises: a positive electrode provided with a positive electrode current collector and a positive electrode mixture layer that is supported on the positive electrode current collector and that is reversibly doped with anions; the negative electrode is provided with a negative electrode current collector and a negative electrode mixture layer that is supported on the negative electrode current collector and that is reversibly doped with lithium ions, and the negative electrode mixture layer contains a negative electrode active material, a conductive auxiliary agent, a binder, and a dispersant. The ratio of the mass of the dispersant to the mass of the negative electrode mixture layer is greater than the ratio of the mass of the binder to the mass of the negative electrode mixture layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] This disclosure claims the benefit of priority to Japanese Patent Application No. 2022-207302, filed with the Japan Patent Office on December 23, 2022, and incorporates by reference the entire contents of the above patent application into this specification. Technical field

[0003] The present invention relates to an electrochemical capacitor. Background art

[0004] In recent years, electrochemical capacitors (such as hybrid capacitors like lithium-ion capacitors) that combine the charge storage principles of lithium-ion secondary batteries and electric double-layer capacitors have received attention. Such electrochemical capacitors typically use a polarizable electrode for the positive electrode and a non-polarizable electrode for the negative electrode. As a result, it is expected that the electrochemical capacitor will have both the high energy density of a lithium-ion secondary battery and the high output characteristics of an electric double-layer capacitor.

[0005] In Patent Document 1, there has been proposed "a method for manufacturing a negative electrode active material for a lithium-ion capacitor, in which carbon black having an average particle diameter measured by an electron microscope method of 12 to 300 nm and a BET specific surface area of 200 to 1500 m 2 / g is kneaded with a carbon precursor, fired and pulverized at 800°C to 3200°C to adjust the average particle diameter (D50) to 1 to 20 μm, and the BET specific surface area is adjusted to 110 m 2 / g or more and 350 m 2 / g or less".

[0006] Prior art documents

[0007] Patent documents

[0008] Patent Document 1: Japanese Patent No. 6356145 Specification Summary of the invention

[0009] Problems to be solved by the invention

[0010] When an electrochemical capacitor such as a lithium-ion capacitor is used at high temperature for a long time, gas may be generated inside due to the decomposition of the electrolyte. In addition, such an electrochemical capacitor may have a deteriorated floating charge characteristic due to the reduction of the facing area caused by the generated gas staying between the opposed electrodes (between the positive and negative electrodes). One object of the present disclosure is to provide an electrochemical capacitor with good floating charge characteristics.

[0011] Means for solving the problems

[0012] One aspect of the present invention relates to an electrochemical capacitor, which includes a positive electrode, a negative electrode, a separator, and a lithium-ion conductive electrolyte.

[0013] The above positive electrode has a positive electrode current collector and a positive electrode mixture layer carried on the positive electrode current collector and reversibly doped with anions.

[0014] The above negative electrode has a negative electrode current collector and a negative electrode mixture layer carried on the negative electrode current collector and reversibly doped with lithium ions.

[0015] The above negative electrode mixture layer contains a negative electrode active material, a conductive additive, a binder, and a dispersant.

[0016] The proportion of the mass of the above dispersant relative to the mass of the above negative electrode mixture layer is greater than the proportion of the mass of the above binder relative to the mass of the above negative electrode mixture layer.

[0017] Advantages of the Invention

[0018] According to the present invention, an electrochemical capacitor with good floating charge characteristics can be obtained.

[0019] The new features of the present invention are described in the scope of the appended claims. However, the present invention should be more fully understood in both its constitution and content, together with other objects and features of the present invention, through the following detailed description with reference to the drawings. Description of the Drawings

[0020] Figure 1 It is a longitudinal sectional view showing the constitution of an electrochemical capacitor according to an embodiment of the present invention. Detailed Embodiments

[0021] Hereinafter, embodiments of the present disclosure will be exemplified, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials are sometimes illustrated, but as long as the invention of the present disclosure can be implemented, other numerical values and other materials can also be applied. In this specification, a description such as "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be rephrased as "not less than numerical value A and not more than numerical value B". In the following description, when the lower limit and the upper limit of a specific physical property, condition, etc. are illustrated, as long as the lower limit is not higher than the upper limit, any one of the illustrated lower limits can be arbitrarily combined with any one of the illustrated upper limits.

[0022] In addition, the present disclosure includes combinations of matters described in two or more of the multiple claims arbitrarily selected from the claims described in the appended claims. That is, as long as there is no technical contradiction, matters described in two or more of the multiple claims arbitrarily selected from the claims described in the appended claims can be combined.

[0023] In the following description, terms such as "containing ~" or "comprising ~" include expressions of "containing (or comprising) ~", "substantially consisting of ~", and "consisting of ~".

[0024] An electrochemical capacitor according to an embodiment of the present invention includes a positive electrode, a negative electrode, a separator, and a lithium ion conductive electrolyte. Generally, the positive electrode and the negative electrode together with the separator interposed therebetween form an electrode body. The electrode body is formed, for example, in the form of a columnar wound body by winding the strip-shaped positive electrode and the negative electrode with the separator interposed therebetween. Alternatively, the electrode body may be formed in the form of a laminate by laminating the plate-shaped positive electrode and the negative electrode with the separator interposed therebetween.

[0025] The positive electrode includes a positive electrode current collector and a positive electrode mixture layer supported on the positive electrode current collector and reversibly doped with anions. The positive electrode mixture layer includes at least a positive electrode active material reversibly doped with anions. The doping of anions into the positive electrode mixture layer or the positive electrode active material refers to the concept that at least includes the adsorption phenomenon of anions to the positive electrode active material, and may also include chemical interactions between anions and the positive electrode active material, etc. The positive electrode mixture layer exhibits capacitance by at least performing a non-Faraday reaction (a reaction not accompanied by oxidation or reduction) of reversibly adsorbing and desorbing anions.

[0026] The negative electrode includes a negative electrode current collector and a negative electrode mixture layer supported on the negative electrode current collector and reversibly doped with lithium ions. The negative electrode mixture layer includes at least a negative electrode active material reversibly doped with lithium ions. The doping of lithium ions into the negative electrode mixture layer or the negative electrode active material refers to the concept that at least includes the insertion phenomenon of lithium ions into the negative electrode active material, and may also include the adsorption of lithium ions to the negative electrode active material, chemical interactions between the negative electrode active material and lithium ions, etc. The negative electrode mixture layer exhibits capacitance by at least performing a Faraday reaction (a reaction accompanied by oxidation or reduction) of reversibly inserting and extracting lithium ions.

[0027] As a typical example of the electrochemical capacitor as described above, a hybrid capacitor such as a lithium ion capacitor can be cited. The positive electrode of the lithium ion capacitor is generally a polarizable electrode. The positive electrode of the polarizable electrode exhibits capacitance by the adsorption and desorption of anions to the positive electrode active material. The positive electrode active material includes, for example, a carbon material (activated carbon, etc.). However, the positive electrode may also be an electrode that, while having the properties of a polarizable electrode, a Faraday reaction also contributes to the positive electrode capacitance. That is, the positive electrode may be an electrode that exhibits capacitance by performing a Faraday reaction in addition to a non-Faraday reaction. Such an electrode includes, for example, a π-conjugated conductive polymer as a positive electrode active material. A dopant may also be doped in the conductive polymer.

[0028] (Negative electrode)

[0029] The negative electrode described above includes a negative electrode current collector and a negative electrode mixture layer supported on the negative electrode current collector and reversibly doped with lithium ions. The negative electrode mixture layer contains at least a negative electrode active material that reversibly dopes lithium ions. Such a negative electrode active material includes, for example, hard carbon (difficult-to-graphitize carbon). The thickness of the negative electrode mixture layer is not particularly limited. For example, it can be 10 μm to 300 μm on each side of the negative electrode current collector.

[0030] The above negative electrode current collector uses a sheet-like metal material. The sheet-like metal material can be a metal foil, a metal porous body, an etched metal, etc. As the metal material, copper, a copper alloy, nickel, stainless steel, etc. can be used.

[0031] The interplanar spacing (i.e., the interplanar spacing between carbon layers) d002 of the (002) plane of the difficult-to-graphitize carbon measured by X-ray diffraction method can be The above. The theoretical capacity of the difficult-to-graphitize carbon is preferably 150 mAh / g or more, for example. By using the above difficult-to-graphitize carbon, it is easy to obtain a negative electrode with a small low-temperature DCR and small expansion and contraction during charge and discharge. The difficult-to-graphitize carbon preferably accounts for 50% by mass or more of the above negative electrode active material, more preferably 80% by mass or more, and further preferably 95% by mass or more. In addition, the difficult-to-graphitize carbon preferably accounts for 40% by mass or more of the above negative electrode mixture layer, more preferably 70% by mass or more, and further preferably 90% by mass or more.

[0032] As the above negative electrode active material, difficult-to-graphitize carbon and a material other than difficult-to-graphitize carbon can be used in combination. As the material other than difficult-to-graphitize carbon that can be used as the above negative electrode active material, graphitizable carbon (soft carbon), graphite (natural graphite, artificial graphite, etc.), lithium titanium oxide (spinel-type lithium titanium oxide, etc.), silicon oxide, silicon alloy, tin oxide, tin alloy, etc. can be exemplified.

[0033] From the viewpoint of improving the filling property of the negative electrode active material in the negative electrode mixture layer and easily suppressing side reactions with the electrolyte, the average particle diameter of the negative electrode active material (especially difficult-to-graphitize carbon) is preferably 1 μm to 20 μm, more preferably 2 μm to 15 μm.

[0034] It should be noted that in this specification, the so-called average particle diameter means the volume-based median diameter (D50) in the particle size distribution measured by laser diffraction type particle size distribution measurement.

[0035] The specific surface area of the negative electrode mixture layer is 10 m 2 / g or more and 70 m 2 / g or less. When the specific surface area of the above-mentioned negative electrode mixture layer is 10 m 2 / g or more, the resistance of the negative electrode is greatly reduced, and thus the internal resistance of the electrochemical capacitor is greatly reduced. When the specific surface area of the above-mentioned negative electrode mixture layer is 70 m 2 / g or less, the reactivity of the negative electrode is not too high, and it is easy to suppress the deterioration of the negative electrode. Therefore, excellent floating charge characteristics can be obtained. Among them, the specific surface area of the above-mentioned negative electrode mixture layer is preferably 20 m 2 / g or more and 60 m 2 / g or less. It should be noted that the method for measuring the specific surface area of the above-mentioned negative electrode mixture layer will be described later.

[0036] It should be noted that the so-called floating charge characteristic is an index of the degree of deterioration of the electrochemical capacitor during floating charge in which a constant voltage is maintained using an external DC power supply. The smaller the capacity reduction during floating charge and the smaller the increase in internal resistance, the better the floating charge characteristics can be said to be.

[0037] In the case of a conventional electrochemical capacitor having a high specific surface area in the negative electrode mixture layer, since the active surface of the negative electrode active material contributing to the Faraday reaction is excessively exposed, there is a case where gas is generated inside due to the decomposition of the electrolyte. As a result, due to the gas generated staying between the opposing electrodes (between the positive and negative electrodes) and reducing the opposing area, the floating charge characteristics may deteriorate.

[0038] In order to solve this problem, the present inventors conducted in-depth research and found that by constructing the negative electrode mixture layer as described below, an electrochemical capacitor with good floating charge characteristics can be obtained even when the above-mentioned negative electrode mixture layer has a high specific surface area.

[0039] The above-mentioned negative electrode mixture layer contains a negative electrode active material, a conductive assistant, a binder, and a dispersant.

[0040] Regarding the above-mentioned negative electrode mixture layer, in order to function as an electrochemical capacitor, it is preferable to bond the above-mentioned negative electrode active material and the above-mentioned conductive assistant in a delocalized state in the negative electrode mixture layer.

[0041] The above-mentioned dispersant stabilizes the dispersion of the negative electrode slurry during the manufacturing process of the negative electrode. As a result, the negative electrode active material and the conductive assistant can be made uniform when the above-mentioned negative electrode mixture layer is formed. In addition, when there is an excess amount of the above-mentioned dispersant, it can also function as a binder, and the influence on the resistance of the above-mentioned negative electrode mixture layer is smaller than that of the binder.

[0042] On the other hand, if it is only the above-mentioned dispersant, when the electrochemical capacitor is used for a long time at a high temperature (for example, in an environment of 85°C), the durability of simply maintaining the adhesion of the above-mentioned negative electrode mixture layer is not sufficient. Therefore, in order to obtain durability, it is preferable that the above-mentioned negative electrode mixture layer contains a binder in addition to the above-mentioned dispersant. Due to its soft polymer structure, the above-mentioned binder can follow the expansion and contraction of the above-mentioned negative electrode mixture layer in the temperature environment where the electrochemical capacitor is used. Thus, the adhesion of the above-mentioned negative electrode mixture layer can be maintained.

[0043] In addition, the above-mentioned binder forms an insulating film on the surfaces of the negative electrode active material and the conductive auxiliary agent during the manufacturing process of the negative electrode. Thus, the gas generation caused by the decomposition of the electrolyte can be suppressed when the negative electrode mixture layer has a high specific surface area. On the other hand, if the mass ratio of the above-mentioned binder is too large, the resistance of the negative electrode mixture layer may increase.

[0044] The mass ratio of the above-mentioned dispersant relative to the mass of the above-mentioned negative electrode mixture layer is preferably greater than the mass ratio of the above-mentioned binder relative to the mass of the above-mentioned negative electrode mixture layer. For example, the mass ratio of the above-mentioned dispersant relative to the mass of the above-mentioned negative electrode mixture layer is preferably 1.5 times or more and 50 times or less, more preferably 2 times or more and 10 times or less, of the mass ratio of the above-mentioned binder relative to the mass of the above-mentioned negative electrode mixture layer.

[0045] By setting the mass ratios of the above-mentioned dispersant and the above-mentioned binder relative to the mass of the above-mentioned negative electrode mixture layer within the above range, the negative electrode mixture layer can be adhered with high strength while sufficiently reducing the resistance of the above-mentioned negative electrode mixture layer. On the other hand, when the mass ratio of the above-mentioned binder relative to the mass of the above-mentioned negative electrode mixture layer is greater than the mass ratio of the above-mentioned dispersant relative to the mass of the above-mentioned negative electrode mixture layer, the resistance of the above-mentioned negative electrode mixture layer becomes too large, and the floating charge characteristics may deteriorate.

[0046] The above-mentioned binder contains at least one selected from fluororesin, acrylic resin, and rubber materials, and may also contain styrene-butadiene rubber.

[0047] The mass ratio of the above-mentioned binder relative to the mass of the above-mentioned negative electrode mixture layer only needs to be 0.3% or more and less than 5%, may also be 0.5% or more and less than 3.5%, or may also be 1.0% or more and less than 2.0%. If it is within this range, the active surface of the negative electrode active material can be moderately coated by the film from the binder, so the gas generation caused by the decomposition of the electrolyte can be suppressed.

[0048] Examples of the above-mentioned binder include fluororesins, acrylic resins, rubber materials, etc. Examples of the fluororesin include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), modified PVDF, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), etc. Examples of the acrylic resin include polyacrylic acid, acrylic acid-methyl methacrylate copolymer, etc. Examples of the rubber material include styrene-butadiene rubber.

[0049] Examples of the above-mentioned dispersant include at least one selected from carboxymethyl cellulose and carboxymethyl cellulose salts (hereinafter, at least one selected from carboxymethyl cellulose and carboxymethyl cellulose salts is also referred to as "CMC").

[0050] The proportion of the mass of the above-mentioned dispersant (CMC) relative to the mass of the above-mentioned negative electrode binder layer is, for example, 1% or more, and may also be 3% or more, or may also be 4.5% or more. The proportion of the mass of the above-mentioned dispersant (CMC) relative to the mass of the above-mentioned negative electrode binder layer is, for example, 10.0% or less, and may also be 8.0% or less, or may also be 6.5% or less. If it is within this range, the above-mentioned negative electrode binder layer can be adhered to the above-mentioned negative electrode current collector with high strength while ensuring the dispersion stability of the negative electrode slurry.

[0051] When using a carboxymethyl cellulose salt as the above-mentioned CMC, sodium salt, lithium salt, potassium salt, ammonium salt, etc. can be used. Among them, it is preferable that the above-mentioned carboxymethyl cellulose salt contains an ammonium salt. The ammonium salt of the above-mentioned carboxymethyl cellulose is particularly preferable because it is particularly unlikely to increase the resistance of the negative electrode among the above-mentioned CMCs.

[0052] The specific surface area of the above-mentioned negative electrode binder layer is the BET specific surface area obtained using a measuring device in accordance with JIS Z8830 (for example, TriStarII 3020 manufactured by Shimadzu Corporation). Specifically, the BET specific surface area is obtained as follows. First, the electrochemical capacitor is disassembled and the negative electrode is taken out. Using this negative electrode as the working electrode and a Li metal foil as the counter electrode, a half-cell is assembled, and the Li in the negative electrode is de-doped until the negative electrode potential reaches 1.5V. Then, the negative electrode after de-doping of Li is washed with dimethyl carbonate (DMC) and dried. After that, the negative electrode binder layer is peeled off from the negative electrode current collector, and a sample of about 0.5 g of the above-mentioned negative electrode binder layer is collected.

[0053] Then, the collected sample is heated at 150 °C for 12 hours under reduced pressure below 95 kPa. Thereafter, nitrogen is adsorbed onto the sample with a known mass to obtain an adsorption isotherm in the range of relative pressure from 0 to 1. Thereafter, the surface area of the sample is calculated based on the monolayer adsorption amount of the gas obtained from the above adsorption isotherm. Here, the specific surface area is obtained according to the following BET equation using the BET one-point method (relative pressure is 0.3).

[0054] P / V(P0 - P) = (1 / VmC) + {(C - 1) / VmC}(P / P0) (1)

[0055] S = kVm (2)

[0056] P0: Saturated vapor pressure

[0057] P: Adsorption equilibrium pressure

[0058] V: Adsorption amount at adsorption equilibrium pressure P

[0059] Vm: Monolayer adsorption amount

[0060] C: Parameter related to adsorption heat, etc.

[0061] S: Specific surface area

[0062] k: Nitrogen monolayer occupation area 0.162 nm 2

[0063] Preferably, the peeling strength of the above negative electrode mixture layer from the above negative electrode current collector can ensure, for example, 0.015 N / mm or more. This peeling strength is sufficient from both the viewpoints of the manufacturing process and ensuring product characteristics. For example, by setting the ratio of the mass of the binder and CMC relative to the above negative electrode mixture layer within the above range, a peeling strength of 0.04 N / mm or more, and further 0.05 N / mm or more can be ensured while guaranteeing product characteristics.

[0064] The peel strength of the above-mentioned negative electrode mixture layer peeled from the above-mentioned negative electrode current collector is determined using a measuring device in accordance with JIS Z0237 (2009). Specifically, it is determined as follows. First, disassemble the electrochemical device and take out the negative electrode. Then, wash the negative electrode with dimethyl carbonate (DMC) and dry it. After that, form the negative electrode into a strip-shaped sample with a width of 10 mm and a length of 50 mm or more. Then, stick one side of a double-sided tape (for example, No. 5606 manufactured by Nitto Denko Corporation) with a width of 20 mm and a length of 130 mm on the negative electrode mixture layer of the sample. Stick the other side of the double-sided tape on a horizontal platform with a flat surface. Thereafter, fix one end of the negative electrode current collector in the longitudinal direction with a dynamometer and pull it in the vertical direction at a speed of 50 mm / minute to peel the negative electrode mixture layer stuck to the double-sided tape from the negative electrode current collector. Measure the tension at this time for 15 seconds or more, and calculate the average tension in a continuous 15-second interval.

[0065] The above-mentioned negative electrode mixture layer may contain a conductive auxiliary agent. As the above-mentioned conductive auxiliary agent, a carbon material can be used. The above-mentioned conductive auxiliary agent may be carbon black, carbon fiber, etc. As carbon black, acetylene black (AB), Ketjen black (KB), etc. can be cited. Among them, considering the large specific surface area, Ketjen black is preferably used.

[0066] The specific surface area of the above-mentioned negative electrode mixture layer can reflect the specific surface areas of the negative electrode active material and the conductive auxiliary agent. It is preferable that the specific surface area of the above-mentioned conductive auxiliary agent is large to a certain extent. By using a conductive auxiliary agent with a high specific surface area, the specific surface area of the negative electrode mixture layer can be increased, and it is easy to reduce the resistance of the negative electrode. The specific surface area of the above-mentioned conductive auxiliary agent is preferably 800 m 2 / g or more, and can also be 1000 m 2 / g or more. As such a conductive auxiliary agent, carbon black (for example, Ketjen black) can be cited.

[0067] It should be noted that by observing the cross-section of the above-mentioned negative electrode mixture layer using a scanning electron microscope (SEM), the volume fraction of the negative electrode mixture component containing the above-mentioned conductive auxiliary agent in the above-mentioned negative electrode mixture layer can be calculated respectively. Based on the obtained volume fraction and the specific surface area of the above-mentioned negative electrode mixture layer, the type, specific surface area, etc. of the conductive auxiliary agent can be inferred. In the cross-sectional image, the proportion of the area occupied by each negative electrode mixture component is regarded as the proportion of the volume to calculate the volume fraction of each negative electrode mixture component. The proportion of the area is obtained by analyzing the SEM image using image analysis software.

[0068] The proportion of the mass of the above-mentioned conductive auxiliary agent relative to the mass of the above-mentioned negative electrode mixture layer is preferably 2% or more and less than 15%, can also be 3% or more and 12% or less, and can also be 4% or more and 11% or less. If it is within this range, it is possible to sufficiently suppress the resistance of the negative electrode while easily ensuring excellent floating charge characteristics.

[0069] The above-mentioned negative electrode mixture layer is formed, for example, by the following steps: mixing a negative electrode mixture with a dispersion medium to prepare a negative electrode slurry, and after coating the negative electrode slurry on a negative electrode current collector, drying is performed. The above-mentioned negative electrode mixture contains a negative electrode active material, a binder, a conductive auxiliary agent, and the like.

[0070] Lithium ions are pre-doped in the above-mentioned negative electrode mixture layer in advance. By pre-doping lithium ions in the above-mentioned negative electrode mixture layer, the potential of the negative electrode decreases, the potential difference (i.e., voltage) between the positive electrode and the negative electrode becomes larger, and the energy density of the electrochemical capacitor is increased.

[0071] The potential of the negative electrode is, for example, 0.2 V or less based on a lithium reference (vs. Li / Li + )). This potential of the negative electrode is the potential of the negative electrode (25 °C) at the time when pre-doping is completed (or during charging). The amount of pre-doped lithium is set to match the potential of the negative electrode in the electrolyte after pre-doping is completed. The amount of pre-doped lithium can be set, for example, to about 50% to 95% of the maximum amount that can be embedded in the above-mentioned negative electrode mixture layer.

[0072] A first layer containing lithium carbonate can be formed on the surface of the above-mentioned negative electrode mixture layer. The above-mentioned first layer is mainly formed on at least a part of the surface of the negative electrode active material existing on the surface of the negative electrode mixture layer. Generally, the larger the specific surface area of the negative electrode mixture layer, the more easily the floating charge characteristics decrease, but by forming the above-mentioned first layer, the deterioration of the negative electrode can be significantly suppressed, so the decrease in the floating charge characteristics is suppressed.

[0073] A second layer containing a solid electrolyte can be formed on the surface of the above-mentioned negative electrode mixture layer. At least a part of the above-mentioned second layer can cover at least a part of the surface of the negative electrode mixture layer with the first layer interposed therebetween. Since the above-mentioned second layer has a composition different from that of the above-mentioned first layer, the above-mentioned second layer can be distinguished from the above-mentioned first layer. When the electrochemical capacitor using lithium ions is charged and discharged, a solid electrolyte interface coating film (i.e., SEI coating film) is formed on the surface of the above-mentioned negative electrode mixture layer. The above-mentioned second layer can be formed as an SEI coating film.

[0074] The above-mentioned SEI film plays an important role in the charge-discharge reaction. However, if the above-mentioned SEI film is formed too thickly, the deterioration of the negative electrode becomes larger. For example, in an electrochemical capacitor using lithium ions, the diffusion of the above-mentioned lithium ions is hindered by the above-mentioned SEI film, thereby increasing the internal resistance. On the contrary, the above-mentioned first layer containing lithium carbonate promotes the formation of a good SEI film and has the effect of maintaining the above-mentioned SEI film in a good state during repeated charge and discharge. For example, it functions as follows. That is, during repeated charge and discharge, the thickness of the above-mentioned SEI film is kept relatively constant, thereby suppressing a large change in the amount of lithium ions used in the formation of the above-mentioned SEI film. Therefore, by forming the first layer on the surface of the negative electrode binder layer, even when the specific surface area of the negative electrode binder layer is increased to reduce the resistance of the negative electrode, the deterioration of the negative electrode can be significantly suppressed.

[0075] When the above-mentioned first layer and the above-mentioned second layer are formed on the surface of the negative electrode binder layer, at least a part of the above-mentioned second layer covers at least a part of the surface of the above-mentioned negative electrode active material existing on the surface of the above-mentioned negative electrode binder layer with the above-mentioned first layer interposed therebetween. That is, at least a part of the above-mentioned first layer is covered by the above-mentioned second layer. The above-mentioned first layer is interposed between the surface of the negative electrode active material existing on the surface of the above-mentioned negative electrode binder layer and the above-mentioned second layer and serves as the base layer of the above-mentioned second layer. By making the above-mentioned first layer the base layer, the above-mentioned second layer is formed into a good state of SEI film.

[0076] The above-mentioned second layer may also contain lithium carbonate. When the above-mentioned second layer contains lithium carbonate, the content of lithium carbonate contained in the above-mentioned second layer is less than the content of lithium carbonate contained in the above-mentioned first layer. By setting the above-mentioned first layer containing a large amount of lithium carbonate as the base layer, the above-mentioned second layer is formed into an even better state of SEI film.

[0077] The above-mentioned first layer can be formed on the surface of the negative electrode binder layer before assembling the electrochemical capacitor. The electrochemical capacitor assembled using this negative electrode forms the above-mentioned second layer (SEI film) with a uniform and appropriate thickness on the surface of the negative electrode active material existing on the surface of the above-mentioned negative electrode binder layer due to subsequent charge and discharge. The SEI film is formed, for example, by the reaction of the electrolyte and the negative electrode in the electrochemical capacitor. Since the above-mentioned electrolyte can pass through not only the above-mentioned second layer but also the above-mentioned first layer, the entire layer including the above-mentioned first layer and the above-mentioned second layer can also be referred to as the SEI film. However, for convenience in this specification, the above-mentioned second layer is referred to as the SEI film to distinguish it from the above-mentioned first layer.

[0078] The existence of a region containing lithium carbonate such as the first layer described above can be confirmed, for example, by analyzing the surface of the negative electrode binder layer by X-ray photoelectron spectroscopy (XPS). It should be noted that the measurement by XPS will be described later. However, the analysis method is not limited to XPS.

[0079] The thickness of the first layer described above is, for example, 1 nm or more, and can be set to 5 nm or more when a longer-term effect is expected, and can be set to 10 nm or more when a more reliable effect is expected. However, if the thickness of the first layer is greater than 50 nm, the first layer itself may become a resistance component. Therefore, the thickness of the first layer can be set to 50 nm or less, or can be set to 30 nm or less. The thickness of the first layer is, for example, 1 nm to 50 nm.

[0080] The thickness of the second layer described above is, for example, 1 nm or more, can also be 3 nm or more, and is sufficient if it is 5 nm or more. However, if the thickness of the second layer is greater than 20 nm, the second layer itself may become a resistance component. Therefore, the thickness of the second layer can be set to 20 nm or less, or can be set to 10 nm or less.

[0081] Regarding the ratio of the thickness A of the first layer to the thickness B of the second layer: A / B, from the viewpoint of reducing the resistance of the negative electrode, it is preferably 1 or less. At this time, the thickness of the second layer is preferably 20 nm or less, and can also be 10 nm or less. However, from the viewpoint of forming a good second layer, it is preferably that A / B is 0.1 or more, and for example, A / B can be 0.2 or more.

[0082] The thicknesses of the first layer and the second layer can be measured by analyzing the surface of the negative electrode binder layer at multiple locations (at least 5 locations) of the negative electrode binder layer. In addition, the average of the thicknesses of the first layer or the second layer obtained at multiple locations can be set as the thickness of the first layer or the second layer. It should be noted that the negative electrode binder layer provided for the measurement sample can be the negative electrode binder layer peeled off from the negative electrode current collector. In this case, it is only necessary to analyze the coating film formed on the surface of the negative electrode active material near the surface of the negative electrode binder layer. Specifically, it is only necessary to collect the negative electrode active material covered with the coating film from the vicinity of the surface of the negative electrode binder layer disposed on the side opposite to the surface joined to the negative electrode current collector and use it for analysis.

[0083] The XPS analysis of the surface of the above-mentioned negative electrode mixture layer is carried out, for example, by the following operation: in the chamber of an X-ray photoelectron spectrometer, an argon beam is irradiated onto the coating film formed on the surface of the negative electrode mixture layer or on the surface of the negative electrode active material present on the surface of the negative electrode mixture layer, and the changes in each energy spectrum attributed to C1s, O1s electrons, etc. with respect to the irradiation time are observed and recorded. At this time, from the viewpoint of avoiding analysis errors, the energy spectrum of the outermost surface of the above-mentioned coating film can be ignored. The thickness of the region where the peak attributed to lithium carbonate is stably observed corresponds to the thickness of the first layer.

[0084] In the case of the negative electrode taken out from an electrochemical capacitor that has been completed and undergone a given aging or at least one charge-discharge cycle, an SEI coating film (i.e., the second layer) containing a solid electrolyte is formed on the surface of the negative electrode mixture layer. The thickness of the region where the peak attributed to the bond of the compound contained in the above-mentioned SEI coating film is stably observed corresponds to the thickness of the above-mentioned SEI coating film (i.e., the thickness of the second layer).

[0085] As the compound contained in the above-mentioned SEI coating film, a compound containing an element that can be a marker for the second layer is selected. For example, an element contained in the electrolyte and substantially not contained in the above-mentioned first layer (such as F) can be selected as the element that can be a marker for the second layer. As the compound containing the element that can be a marker for the second layer, LiF can be selected, for example.

[0086] When the above-mentioned second layer contains LiF, if the above-mentioned second layer is measured by X-ray photoelectron spectroscopy (XPS), a substantial F1s peak attributed to the LiF bond is observed. In this case, the thickness of the region where the peak attributed to the LiF bond is stably observed corresponds to the thickness of the above-mentioned second layer.

[0087] On the other hand, the above-mentioned first layer usually does not contain LiF, and a substantial F1s peak attributed to the LiF bond is not observed even when the above-mentioned first layer is measured by X-ray photoelectron spectroscopy (XPS). Therefore, the thickness of the region where the peak attributed to the LiF bond cannot be stably observed can be set as the thickness of the first layer.

[0088] An O1s peak attributed to lithium carbonate can also be observed in the above-mentioned SEI coating film. However, since the above-mentioned SEI coating film formed in the electrochemical capacitor has a different composition from the above-mentioned first layer formed in advance, the two can be distinguished. For example, in the XPS analysis of the above-mentioned SEI coating film, an F1s peak attributed to the LiF bond is observed, but a substantial F1s peak attributed to the LiF bond is not observed in the above-mentioned first layer. In addition, the lithium carbonate contained in the above-mentioned SEI coating film is in trace amounts. It should be noted that as the Li1s peak, for example, peaks from compounds such as ROCO2Li and ROLi can be detected.

[0089] When analyzing the first layer above using XPS, in addition to the first peak corresponding to O1s attributed to the C=O bond, a second peak corresponding to O1s attributed to the Li-O bond can also be observed. The region of the coating near the surface of the negative electrode active material may contain a very small amount of LiOH or Li2O.

[0090] Specifically, when analyzing the first layer formed on the surface of the negative electrode binder layer in the depth direction, in the order of increasing distance from the outermost surface of the first layer, the following regions can be observed: the first region where the first peak (O1s attributed to the C=O bond) and the second peak (O1s attributed to the Li-O bond) are observed and the intensity of the first peak (peak intensity of the first peak) is greater than the intensity of the second peak (peak intensity of the second peak); the second region where the first peak and the second peak are observed and the intensity of the second peak is greater than the intensity of the first peak. In addition, between the outermost surface of the first layer and the first region, a third region where the first peak is observed and the second peak is not observed can further exist. The third region is easily observed when the thickness of the region containing lithium carbonate is large.

[0091] It should be noted that the magnitude relationship between the intensity of the first peak and the second peak can be judged only based on the height of the peak relative to the baseline.

[0092] In the center of the thickness direction of the first layer, generally, the C1s peak attributed to the C-C bond is not substantially observed, or even if observed, it is less than half of the peak intensity attributed to the C=O bond.

[0093] Next, a method for forming the first layer containing lithium carbonate on the surface of the negative electrode binder layer will be described. The process of forming the first layer can be carried out, for example, by a vapor phase method, a coating method, a transfer method, etc.

[0094] As the above-mentioned vapor phase method, methods such as chemical vapor deposition, physical vapor deposition, and sputtering can be cited. For example, the above-mentioned lithium carbonate can be attached to the surface of the negative electrode binder layer using a vacuum evaporation device. The pressure in the device chamber during evaporation is set to 10 -2 ~10 -5 Pa, the temperature of the lithium carbonate evaporation source is 400 - 600 °C, and the temperature of the negative electrode binder layer is -20 - 80 °C.

[0095] As the above coating method, a solution or dispersion containing the above lithium carbonate is coated on the surface of the above negative electrode mixture layer using, for example, a microgravure coater and dried, whereby the above first layer can be formed. The lithium carbonate content in the solution or dispersion is, for example, 0.3 to 2% by mass, and in the case of using a solution, a concentration below the solubility (for example, about 0.9 to 1.3% by mass in the case of an aqueous solution at room temperature) is sufficient.

[0096] Subsequently, a step of forming a second layer containing a solid electrolyte in such a manner as to cover at least a part of the above first layer is performed, whereby a negative electrode can be obtained. On the surface of the negative electrode mixture layer obtained by operating in this way, the above first layer and the above second layer are formed. The above second layer is formed in such a manner as to cover at least a part of the surface of the negative electrode active material existing on the surface of the negative electrode mixture layer with at least a part of it sandwiching the above first layer (that is, with the above first layer as the base layer). The above second layer is preferably formed in such a manner as to cover the entire surface of the negative electrode mixture layer with the above first layer sandwiched therebetween.

[0097] Since the step of forming the above second layer is performed in a state where the negative electrode mixture layer on which the above first layer is formed is in contact with the electrolyte, it can also serve as at least a part of the pre-doping step of lithium ions into the above negative electrode mixture layer. As the source of lithium ions to be pre-doped, for example, metallic lithium can be used.

[0098] The above metallic lithium can be attached to the surface of the above negative electrode mixture layer. It should be noted that the negative electrode having the negative electrode mixture layer on which the above metallic lithium is attached can also be exposed to a carbon dioxide atmosphere, whereby a first layer containing lithium carbonate having a thickness of, for example, 1 nm or more and 50 nm or less can be formed on the surface of the above negative electrode mixture layer.

[0099] The step of attaching the above metallic lithium to the surface of the above negative electrode mixture layer can be performed, for example, by a vapor phase method, transfer printing, or the like. As the above vapor phase method, methods such as chemical vapor deposition, physical vapor deposition, and sputtering can be cited. For example, the above metallic lithium can be formed in a film on the surface of the above negative electrode mixture layer using a vacuum evaporation apparatus. The pressure in the apparatus chamber during evaporation is, for example, set to 10 -2 ~10 -5 Pa, the temperature of the lithium evaporation source is 400 to 600 °C, and the temperature of the above negative electrode mixture layer is -20 to 80 °C.

[0100] The carbon dioxide atmosphere is preferably a dry atmosphere that does not contain moisture. For example, a dew point of -40°C or lower, or -50°C or lower is sufficient. The above carbon dioxide atmosphere may contain gases other than carbon dioxide, but the mole fraction of carbon dioxide is preferably 80% or more, and more preferably 95% or more. The above carbon dioxide atmosphere preferably does not contain oxidizing gases. In the above carbon dioxide atmosphere, the mole fraction of oxygen is set to 0.1% or lower.

[0101] In order to form the above first layer thicker, it is effective to make the partial pressure of carbon dioxide greater than 0.5 atmospheres (5.05×10 4 Pa), for example, and it may also be 1 atmosphere (1.01×10 5 Pa) or more.

[0102] The temperature of the negative electrode exposed to the above carbon dioxide atmosphere is, for example, in the range of 15°C to 120°C. The higher the temperature, the greater the thickness of the above first layer.

[0103] By changing the time for which the negative electrode is exposed in the above carbon dioxide atmosphere, the thickness of the above first layer can be easily controlled. The exposure time is, for example, 12 hours or more, as long as it is less than 10 days.

[0104] The step of forming the above first layer is preferably carried out before forming the electrode body, but the case of carrying out after forming the electrode body is not excluded. That is, by preparing a positive electrode and a negative electrode having a negative electrode mixture layer with metallic lithium attached, and sandwiching a separator between the above positive electrode and the above negative electrode to form an electrode body, and then exposing the above electrode body to a carbon dioxide atmosphere, the above first layer can be formed on the surface of the above negative electrode mixture layer.

[0105] It should be noted that the pre-doping step of lithium ions into the above negative electrode mixture layer is further carried out, for example, by making the above negative electrode mixture layer contact with an electrolyte after forming the electrode body as described above, and is completed by leaving it for a given time. Such a step may be a step of forming the above second layer so as to cover at least a part of the above first layer. For example, by performing charge and discharge of the electrochemical capacitor at least once, the above second layer can be formed on the above negative electrode mixture layer while completing the pre-doping of lithium ions into the above negative electrode mixture layer. In addition, for example, a given charging voltage (e.g., 3.4 to 4.0 V) may be applied between the terminals of the positive electrode and the negative electrode for a given time (e.g., 1 to 75 hours), thereby completing the pre-doping of lithium ions into the above negative electrode mixture layer.

[0106] (Positive electrode)

[0107] The positive electrode contains a positive electrode active material that can be reversibly doped with anions. Examples of the above positive electrode active material include carbon materials, conductive polymers, etc. The above positive electrode may include a positive electrode mixture layer containing the above positive electrode active material and a positive electrode current collector that supports the above positive electrode mixture layer. The thickness of the above positive electrode mixture layer is not particularly limited. For example, it is 10 to 300 μm on each side of the above positive electrode current collector.

[0108] The above positive electrode current collector uses a sheet-like metal material. The above sheet-like metal material may be a metal foil, a metal porous body, an etched metal, etc. As the metal material, aluminum, aluminum alloy, nickel, titanium, etc. can be used.

[0109] As the carbon material used as the above positive electrode active material, a porous carbon material is preferred, and activated carbon is more preferred. Examples of the raw materials of the above activated carbon include wood, coconut shell, coal, pitch, phenolic resin, etc. The above activated carbon is preferably an activated carbon that has been subjected to an activation treatment.

[0110] The average particle size of the above activated carbon is not particularly limited, but it is preferably 20 μm or less, and more preferably 3 μm to 15 μm.

[0111] The specific surface area of the above positive electrode mixture layer generally reflects the specific surface area of the above positive electrode active material. The specific surface area of the above positive electrode mixture layer is, for example, 600 m 2 / g or more and 4000 m 2 / g or less, and it is preferably 800 m 2 / g or more and 3000 m 2 / g or less.

[0112] The specific surface area of the above positive electrode mixture layer is the BET specific surface area obtained using a measuring device in accordance with JIS Z8830 (for example, TriStarII 3020 manufactured by Shimadzu Corporation). Specifically, the electrochemical capacitor is disassembled and the positive electrode is taken out. Then, the positive electrode is washed with DMC and dried. After that, the positive electrode mixture layer is peeled off from the positive electrode current collector, and a sample of about 0.5 g of the positive electrode mixture layer is collected. Then, the specific surface area of the collected sample is obtained according to the above-described method for measuring the specific surface area of the negative electrode mixture layer.

[0113] It is preferred that the above activated carbon accounts for 50% by mass or more of the above positive electrode active material, more preferably 80% by mass or more, and further preferably 95% by mass or more. In addition, it is preferred that the above activated carbon accounts for 40% by mass or more of the above positive electrode mixture layer, more preferably 70% by mass or more, and further preferably 90% by mass or more.

[0114] The above-mentioned positive electrode mixture layer contains the above-mentioned positive electrode active material as an essential component, and contains a conductive assistant, a binder, a dispersant, etc. as optional components. Examples of the conductive assistant include carbon black, carbon fiber, etc. Examples of the binder include fluororesin, acrylic resin, rubber materials, etc. Examples of the dispersant include cellulose derivatives, etc.

[0115] The above-mentioned positive electrode mixture layer is formed, for example, by the following steps: preparing a positive electrode slurry by mixing a positive electrode mixture containing the above-mentioned positive electrode active material, the above-mentioned conductive assistant, etc. with a dispersion medium, and then drying the positive electrode slurry after coating it on the above-mentioned positive electrode current collector.

[0116] As the conductive polymer that can be used as the above-mentioned positive electrode active material, a π-conjugated polymer is preferred. Examples of the π-conjugated polymer include polypyrrole, polythiophene, polyfuran, polyaniline, polythiophene acetylene, polypyridine, or their derivatives. They can be used alone or in combination of two or more. The weight-average molecular weight of the above-mentioned conductive polymer is, for example, 1000 to 100000. It should be noted that the derivatives of the above-mentioned π-conjugated polymer refer to polymers having a π-conjugated polymer as a basic skeleton, such as polypyrrole, polythiophene, polyfuran, polyaniline, polythiophene acetylene, polypyridine, etc. For example, poly(3,4-ethylenedioxythiophene) (PEDOT) is included in the polythiophene derivatives.

[0117] The above-mentioned conductive polymer is formed, for example, by the following steps: immersing a positive electrode current collector having a carbon layer in a reaction solution containing a raw material monomer of the above-mentioned conductive polymer, and subjecting the raw material monomer to electrolytic polymerization in the presence of the above-mentioned positive electrode current collector. In the above-mentioned electrolytic polymerization, it is only necessary to immerse the above-mentioned positive electrode current collector and a counter electrode in the reaction solution containing the above-mentioned raw material monomer and pass an electric current between them with the above-mentioned positive electrode current collector as the anode. The above-mentioned conductive polymer can also be formed by a method other than electrolytic polymerization. For example, the above-mentioned conductive polymer can be formed by chemical polymerization of the above-mentioned raw material monomer. In the above-mentioned chemical polymerization, it is only necessary to polymerize the above-mentioned raw material monomer using an oxidizing agent, etc. in the presence of a positive electrode current collector.

[0118] The raw material monomer used in the above-mentioned electrolytic polymerization or the above-mentioned chemical polymerization only needs to be a polymerizable compound that can generate the above-mentioned conductive polymer through polymerization. The above-mentioned raw material monomer can contain oligomers. Examples of the above-mentioned raw material monomer include aniline, pyrrole, thiophene, furan, thiophene acetylene, pyridine, or their derivatives. They can be used alone or in combination of two or more. Among them, aniline is easy to grow on the surface of the carbon layer through the above-mentioned electrolytic polymerization.

[0119] The above electrolytic polymerization or the above chemical polymerization can be carried out using a reaction solution containing an anion (dopant). By doping a dopant into a π-electron conjugated polymer, excellent conductivity is exhibited. Examples of the above dopant include sulfate ion, nitrate ion, phosphate ion, borate ion, benzenesulfonate ion, naphthalenesulfonate ion, toluenesulfonate ion, methanesulfonate ion, perchlorate ion, tetrafluoroborate ion, hexafluorophosphate ion, fluorosulfate ion, etc. The above dopant may also be a polymeric ion. Examples of the above polymeric ion include ions of polyvinylsulfonic acid, polystyrenesulfonic acid, polyallylsulfonic acid, polyacrylic acid sulfonic acid, polymethacrylic acid sulfonic acid, poly(2-acrylamide-2-methylpropanesulfonic acid), polyisoprene sulfonic acid, polyacrylic acid, etc.

[0120] (Separator)

[0121] The separator is disposed between the positive electrode and the negative electrode. Preferably, the above separator contains, for example, an olefin-based resin. Hereinafter, the separator containing an olefin-based resin is also referred to as an "olefin-based separator".

[0122] Electrochemical capacitors such as lithium-ion capacitors usually use a cellulose-based separator. This is because the above cellulose-based separator has excellent electrolyte permeability and is easy to pre-dope. On the other hand, since the above cellulose-based separator has functional groups such as OH groups that are easy to react with lithium ions and is easy to contain moisture, it is easy to be damaged by side reactions. There is also a case where lithium pre-doped into the negative electrode (specifically, the negative electrode binder layer) reacts with the above separator, reducing the amount of pre-doped lithium. In an environment where lithium carbonate is generated on the surface of the negative electrode binder layer, the above cellulose-based separator tends to deteriorate severely.

[0123] In contrast, the above olefin-based separator has a low water content, and deterioration of the separator itself and the negative electrode (specifically, the negative electrode binder layer) caused by water is suppressed. The above olefin-based separator is also excellent in terms of stability to an electrolyte containing lithium ions and pre-doped lithium. The above olefin-based separator is not easily deteriorated even in an environment where lithium carbonate is generated on the surface of the negative electrode binder layer. Therefore, by using the above olefin-based separator, a state with a low internal resistance can be maintained for a long time. As a result, the floating charge characteristics of the electrochemical capacitor are improved.

[0124] It should be noted that, when pre-doping with lithium ions in the state of a wound body formed by winding a separator between a positive electrode and a negative electrode as described above, the lithium ions dissolved from the metallic lithium introduced for pre-doping are not easily diffused throughout the wound body. In this case, it is difficult to use the above-mentioned olefin-based separator. On the other hand, by bringing a negative electrode having metallic lithium pre-attached to the entire surface of the negative electrode mixture layer into contact with an electrolyte for pre-doping, it is possible to perform pre-doping on the entire wound body in a short time.

[0125] The above-mentioned olefin-based resin is a resin containing olefin units as a main component. The above-mentioned olefin-based resin contains, for example, 50 mass% or more, and further 70 mass% or more of the above-mentioned olefin units. The above-mentioned olefin units refer to monomer units derived from olefins (chain olefins) such as ethylene, propylene, and butene. Here, a divalent group (diyl) formed by monomer polymerization is called the "unit" of the monomer. At least a part of the above-mentioned olefins may also be derivatives thereof. The above-mentioned olefin-based resin may be a homopolymer or a copolymer synthesized from a plurality of olefins. A part of the hydrogen atoms of the above-mentioned olefins may be substituted by halogen atoms. Examples of the above-mentioned olefin-based resin may include polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), chlorinated polyethylene (CPE), ethylene-vinyl acetate copolymer (EVA), ethylene-ethyl acrylate copolymer (EEA), etc. Among them, it is preferably at least one selected from polypropylene (PP) and polyethylene (PE). Since the PP separator and the PE separator have high strength and are stable to an electrolyte containing lithium ions, they can be preferably used for an electrochemical capacitor having the above-mentioned first layer and the above-mentioned second layer formed on the surface of the negative electrode mixture layer.

[0126] As a separator (olefin-based separator) containing the above-mentioned olefin-based resin, for example, a microporous membrane, a woven fabric, or a non-woven fabric made of polyolefin can be used. Among them, the microporous membrane as a non-fibrous porous membrane has high strength and is suitable for thinning. The thickness of the above-mentioned separator is, for example, 8 to 40 μm, preferably 12 to 30 μm, and more preferably 14 to 25 μm or 16 to 25 μm.

[0127] (Electrolyte)

[0128] An electrolyte having lithium ion conductivity contains a lithium salt and a solvent for dissolving the lithium salt. The anion of the lithium salt reversibly repeats doping and de-doping to the positive electrode (specifically, the positive electrode active material layer). Lithium ions from the lithium salt are reversibly inserted into and extracted from the negative electrode (specifically, the negative electrode active material layer).

[0129] As the above-mentioned lithium salts, for example, LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiFSO3, LiCF3CO2, LiAsF6, LiB 10 Cl 10 , LiCl, LiBr, LiI, LiBCl4, LiN(SO2F)2, LiN(SO2CF3)2, etc. They can be used alone or in combination of two or more. Among them, from the aspects of obtaining a liquid electrolyte with high dissociation degree and low viscosity and improving the withstand voltage characteristics of the electrochemical capacitor, lithium salts with fluorine-containing anions are preferred.

[0130] The above electrolyte preferably contains an imide-based electrolyte. The above imide-based electrolyte contains an imide-based anion as the anion of the lithium salt. The above imide-based anion can be an anion containing fluorine and sulfur, and lithium bis(fluorosulfonyl)imide, that is, LiN(SO2F)2 (LiFSI), is particularly preferably used. For example, 80% by mass or more of the lithium salt can be LiFSI.

[0131] The above LiFSI is considered to have the effect of reducing the deterioration of the positive electrode active material and the negative electrode active material. Among the salts with fluorine-containing anions, the FSI anion is considered to be a substance that does not easily generate by-products due to its excellent stability, and smoothly contributes to charge and discharge without damaging the surface of the active material. In addition, the SEI film formed on the surface of the above negative electrode binder layer by using the above LiFSI contains a large amount of lithium fluoride and can reduce the lithium carbonate content ratio. Thus, a stable second layer mainly composed of lithium fluoride can be formed so as to cover the first layer mainly composed of lithium carbonate.

[0132] The concentration of the lithium salt in the non-aqueous electrolyte in the charged state (charge rate (SOC) 90 to 100%) is, for example, 0.2 to 5 mol / L.

[0133] As the solvent, cyclic carbonates such as ethylene carbonate, propylene carbonate, and butylene carbonate, chain carbonates such as dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate, aliphatic carboxylic acid esters such as methyl formate, methyl acetate, methyl propionate, and ethyl propionate, lactones such as γ-butyrolactone and γ-valerolactone, chain ethers such as 1,2-dimethoxyethane (DME), 1,2-diethoxyethane (DEE), and ethoxymethoxyethane (EME), cyclic ethers such as tetrahydrofuran and 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, acetamide, dimethylformamide, dioxolane, acetonitrile, propionitrile, nitromethane, ethyl monoethylene glycol dimethyl ether, trimethoxymethane, sulfolane, methylsulfolane, 1,3-propane sultone, etc. can be used. They can be used alone or in combination of two or more.

[0134] Various additives can be included in the above electrolyte as needed. For example, unsaturated carbonates such as vinylene carbonate, ethylene vinylene carbonate, and divinylene ethylene carbonate can be added as additives for forming a lithium-ion conductive coating film on the negative electrode surface.

[0135] Figure 1 The configuration of an electrochemical capacitor 200 according to an embodiment of the present invention is schematically shown. The electrochemical capacitor 200 includes an electrode body 100, a liquid electrolyte having lithium-ion conductivity (not shown), a metal bottomed battery case 210 for housing the electrode body 100 and the electrolyte, and a sealing plate 220 for sealing the opening of the battery case 210. The electrode body 100 is formed in the form of a columnar wound body by winding a strip-shaped positive electrode 10 and a strip-shaped negative electrode 20 with a separator 30 interposed therebetween. A gasket 221 is disposed at the peripheral portion of the sealing plate 220, and the opening end portion of the battery case 210 is riveted to the gasket 221, thereby sealing the inside of the battery case 210.

[0136] The positive electrode 10 and the negative electrode 20 each have an exposed portion of a current collector at an end along the length direction, and these exposed portions protrude from different end faces of the wound body. The exposed portion 11x of the positive electrode current collector is welded to the positive electrode current collecting plate 13 having a through hole 13h in the center. The other end of the tab 15 connected to one end of the positive electrode current collecting plate 13 is connected to the inner surface of the sealing plate 220. Therefore, the sealing plate 220 functions as an external positive terminal. On the other hand, the exposed portion 21x of the negative electrode current collector is welded to the negative electrode current collecting plate 23. The negative electrode current collecting plate 23 is directly welded to a welding member provided on the inner bottom surface of the battery case 210. Therefore, the battery case 210 functions as an external negative terminal.

[0137] The positive electrode current collecting plate 13 and the negative electrode current collecting plate 23 are substantially disk-shaped metal plates. The material of the negative electrode current collecting plate 23 is, for example, copper, copper alloy, nickel, stainless steel, etc. The material of the positive electrode current collecting plate 13 is, for example, aluminum, aluminum alloy, titanium, stainless steel, etc.

[0138] The electrochemical capacitor is not limited to Figure 1 the wound type electrochemical capacitor shown. For example, it can also be a stacked type electrochemical capacitor. That is, the electrode body can also be formed in the form of a stacked body by stacking a sheet-shaped positive electrode and a negative electrode with a separator interposed therebetween.

[0139] (Appendix)

[0140] The following technology is disclosed by the above description.

[0141] (Technology 1)

[0142] An electrochemical capacitor, comprising a positive electrode, a negative electrode, a separator, and a lithium ion-conductive electrolyte,

[0143] The positive electrode includes a positive electrode current collector and a positive electrode mixture layer supported on the positive electrode current collector and reversibly doped with anions,

[0144] The negative electrode includes a negative electrode current collector and a negative electrode mixture layer supported on the negative electrode current collector and reversibly doped with lithium ions,

[0145] The negative electrode mixture layer contains a negative electrode active material, a conductive assistant, a binder, and a dispersant,

[0146] The ratio of the mass of the dispersant to the mass of the negative electrode mixture layer is greater than the ratio of the mass of the binder to the mass of the negative electrode mixture layer.

[0147] (Technology 2)

[0148] The electrochemical capacitor according to Technology 1, wherein the binder is at least one selected from fluororesins, acrylic resins, and rubber materials.

[0149] (Technology 3)

[0150] The electrochemical capacitor according to Technology 1 or 2, wherein the binder contains styrene-butadiene rubber.

[0151] (Technology 4)

[0152] The electrochemical capacitor according to any one of Technologies 1 to 3, wherein the ratio of the mass of the binder to the mass of the negative electrode mixture layer is 0.3% or more and less than 5%.

[0153] (Technology 5)

[0154] The electrochemical capacitor according to any one of Technologies 1 to 4, wherein the dispersant is at least one selected from carboxymethyl cellulose and carboxymethyl cellulose salts.

[0155] (Technology 6)

[0156] The electrochemical capacitor according to any one of Technologies 1 to 5, wherein the dispersant contains an ammonium salt of carboxymethyl cellulose.

[0157] (Technology 7)

[0158] The electrochemical capacitor according to any one of Technologies 1 to 6, wherein the ratio of the mass of the dispersant to the mass of the negative electrode mixture layer is 1% or more and less than 10%.

[0159] (Technology 8)

[0160] The electrochemical capacitor according to any one of Technologies 1 to 7, wherein the proportion of the mass of the dispersant relative to the mass of the negative electrode mixture layer is 3% or more and less than 8%.

[0161] (Technology 9)

[0162] The electrochemical capacitor according to any one of Technologies 1 to 8, wherein the specific surface area of the negative electrode mixture layer is 10 m 2 / g or more and 70 m 2 / g or less.

[0163] (Technology 10)

[0164] The electrochemical capacitor according to any one of Technologies 1 to 9, wherein the negative electrode mixture layer contains at least one selected from Ketjen black, acetylene black, and carbon nanotubes as the conductive auxiliary agent.

[0165] (Technology 11)

[0166] The electrochemical capacitor according to any one of Technologies 1 to 10, wherein the proportion of the mass of the conductive auxiliary agent relative to the mass of the negative electrode mixture layer is 2% or more and less than 15%.

[0167] (Technology 12)

[0168] The electrochemical capacitor according to any one of Technologies 1 to 11, wherein the specific surface area of the conductive auxiliary agent is 800 m 2 / g or more.

[0169] (Technology 13)

[0170] The electrochemical capacitor according to any one of Technologies 1 to 12, wherein the negative electrode active material contains hard carbon.

[0171] (Technology 14)

[0172] The electrochemical capacitor according to any one of Technologies 1 to 13, wherein the peel strength of the negative electrode mixture layer peeled from the negative electrode current collector is 0.015 N / mm or more.

[0173] Although the current preferred embodiments of the present invention have been described, such disclosure should not be construed in a limiting sense. Various modifications and changes will be apparent to those skilled in the art belonging to the technical field of the present invention upon reading the above disclosure. Therefore, the scope of the appended claims should be construed to include all modifications and changes without departing from the true spirit and scope of the present invention.

[0174] Examples

[0175] Hereinafter, the present invention will be described in more detail based on embodiments, but the present invention is not limited to the embodiments.

[0176] "Electrochemical Capacitors A1 - A7, B1 - B2"

[0177] (1) Fabrication of the positive electrode

[0178] An aluminum foil (positive electrode current collector) with a thickness of 30 μm was prepared. On the other hand, 88 mass parts of activated carbon (average particle size 5.5 μm) as the positive electrode active material, 6 mass parts of acetylene black (AB) as the conductive assistant, 4 mass parts of carboxymethyl cellulose (CMC) as the dispersant, and 2 mass parts of polytetrafluoroethylene (PTFE) as the binder were dispersed in water to prepare a positive electrode paste. The obtained positive electrode paste was coated on both sides of the above aluminum foil, and the coating film was dried and calendered to form a positive electrode mixture layer. Thus, the positive electrode was obtained. At the end of the above positive electrode current collector along the length direction, a positive electrode current collector exposed portion with a width of 10 mm was formed.

[0179] (2) Fabrication of the negative electrode

[0180] A copper foil (negative electrode current collector) with a thickness of 10 μm was prepared. On the other hand, the negative electrode active material, conductive assistant, binder, and dispersant were dispersed in water at the compounding ratios shown in Table 1 to prepare a negative electrode paste. The obtained negative electrode paste was coated on both sides of the copper foil, and the coating film was dried and calendered to form a negative electrode mixture layer. Thus, the negative electrode was obtained. The above negative electrode active material used hard carbon (HC: average particle size 5 μm). It should be noted that Ketjen black (KB) was used as the above conductive assistant, the ammonium salt of carboxymethyl cellulose (CMC) was used as the above dispersant, and styrene - butadiene rubber (SBR) was used as the above binder. In addition, by changing the compounding ratio of the above negative electrode active material and the above conductive assistant, the specific surface area of the above negative electrode mixture layer was adjusted to the value shown in Table 1.

[0181] After that, a thin film of lithium metal for pre - doping was formed on the entire surface of the above negative electrode mixture layer by vacuum evaporation. The amount of pre - doped lithium was set such that the negative electrode potential in the electrolyte after the completion of pre - doping was 0.2 V or less with respect to lithium metal.

[0182] After that, the chamber of the device was purged with carbon dioxide to form a carbon dioxide atmosphere, and thus a first layer containing lithium carbonate was formed on the surface of the negative electrode mixture layer. The dew point of the carbon dioxide atmosphere was set to - 40 °C, the mole fraction of carbon dioxide was set to 100%, and the pressure in the chamber was set to 1 atmospheric pressure (1.01×10 5Pa). The temperature of the negative electrode exposed to a carbon dioxide atmosphere at 1 atm was set at 25°C. The time for exposing the negative electrode in the carbon dioxide atmosphere was set at 22 hours. Substantially no F (or LiF) was contained in the first layer.

[0183] The peel strength of the above negative electrode mixture layer peeled from the above negative electrode current collector was measured, and the results were all 0.04 N / mm or more.

[0184] (Fabrication of electrode body)

[0185] As the separator, a microporous membrane (thickness 25 μm) having a single-layer structure made of polypropylene (PP), which is an olefin-based separator, was used.

[0186] The above positive electrode and the above negative electrode were wound around the above separator into a columnar shape to form an electrode body. At this time, the exposed portion of the above positive electrode current collector protruded from one end face of the above electrode body, and the exposed portion of the above negative electrode current collector protruded from the other end face of the above electrode body. A disk-shaped positive electrode current collector plate and a negative electrode current collector plate were welded to the exposed portions of the above positive electrode current collector and the above negative electrode current collector, respectively.

[0187] (Preparation of electrolyte)

[0188] A non-aqueous electrolyte was prepared by dissolving LiFSI as a lithium salt in a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) (volume ratio 3:5:2). The concentration of LiFSI in the non-aqueous electrolyte was set at 1.2 mol / L.

[0189] (Assembly of electrochemical capacitor)

[0190] The above electrode body was housed in a bottomed battery case having an opening, and the tab connected to the above positive electrode current collector plate was connected to the inner surface of the sealing plate. Subsequently, the above negative electrode current collector plate was welded to the inner bottom surface of the above battery case. After adding the above non-aqueous electrolyte into the battery case, the opening of the above battery case was sealed with the above sealing plate to assemble an electrochemical capacitor as shown in Figure 1 In Table 1, A1 to A10 are the electrochemical capacitors of Examples 1 to 10, and B1 to B2 are the electrochemical capacitors of Comparative Examples 1 to 2.

[0191] Thereafter, while applying a charging voltage of 3.8 V between the terminals of the positive electrode and the negative electrode, aging was performed at 60°C to complete the pre-doping of lithium ions into the negative electrode (specifically, the negative electrode active material layer).

[0192] The following evaluations were performed on the electrochemical capacitors of the examples and comparative examples.

[0193] [Evaluation 1: Evaluation of the reliability (floating charge characteristics) of the electrochemical capacitor]

[0194] The electrochemical capacitor just after aging was tested at -30°C with a current of 2 mA / cm per unit positive electrode area. 2 After constant current charging at a current density of 1000 nm to a voltage of 3.8 V, the voltage of 3.8 V was maintained for 10 minutes. Then, the battery was charged at a current density of 2 mA / cm per unit positive electrode area at -30°C. 2 The battery was discharged at a constant current density until the voltage reached 2.2 V.

[0195] The height H1 (mm) of the electrochemical capacitor at this time was measured using a vernier caliper. Figure 1 The cylindrical electrochemical capacitor 200 shown has a maximum axial dimension H of its main body.

[0196] Then, a constant voltage of 3.8 V was applied to the electrochemical capacitor for a long time at 85°C. After 1000 hours, the electrochemical capacitor was taken out. Thereafter, a constant voltage of 2 mA / cm2 per unit positive electrode area was applied to the electrochemical capacitor at -30°C. 2 The capacitor was discharged at a constant current density of 1.5 volts to a voltage of 2.2 V. The height H2 (mm) of the electrochemical capacitor at this time was measured using a vernier caliper.

[0197] The value obtained by subtracting H1 from H2 is calculated as the expansion (mm) of the electrochemical capacitor. A small expansion indicates that gas generation during float charge is suppressed. If the expansion value is less than 0.6 (mm), the float charge performance is good.

[0198] Table 1 shows the evaluation results.

[0199] Table 1

[0200]

[0201] Electrochemical capacitor B1 produced very large amounts of gas, resulting in inadequate float charge characteristics. Electrochemical capacitor B2 had poor dispersibility of the negative electrode slurry, making it impossible to apply it to the negative electrode current collector. Meanwhile, electrochemical capacitors A1-A10 produced low amounts of decomposition gas and exhibited excellent float charge characteristics. Details regarding electrochemical capacitors A8-A10 will be discussed later.

[0202] Furthermore, a comparison of electrochemical capacitors A1 to A4 and B1 confirmed that, when the specific surface area of the negative electrode mixture layer and the mixing ratio of the conductive additive in the negative electrode mixture layer were set to the same, the use of a binder reduced gas generation and improved float charge characteristics.

[0203] Electrochemical Capacitor A8

[0204] Except that 91 parts by mass in total of the negative electrode active material and the conductive assistant, 5 parts by mass of the ammonium salt of carboxymethyl cellulose (CMC) as a dispersant, and 4 parts by mass of polyacrylic acid (PAA: binder) are dispersed in water in the preparation of the above-mentioned negative electrode paste, the operation is carried out in the same manner as in the case of the electrochemical capacitors A1 to A7 to produce the electrochemical capacitor A8 and evaluate it. The results are shown in Table 1.

[0205] "Electrochemical Capacitor A9"

[0206] Except that sodium salt (CMC-Na) is used instead of the ammonium salt of carboxymethyl cellulose in the production of the negative electrode, the operation is carried out in the same manner as in the case of the electrochemical capacitors A1 to A7 to produce the electrochemical capacitor A9 and evaluate it. The results are shown in Table 1.

[0207] "Electrochemical Capacitor A10"

[0208] Except that acetylene black (AB: specific surface area 70 m 2 / g) is used instead of Ketjen black (KB) in the production of the negative electrode, the operation is carried out in the same manner as in the case of the electrochemical capacitors A1 to A7 to produce the electrochemical capacitor A10 and evaluate it. The results are shown in Table 1.

[0209] From the comparison between the electrochemical capacitors A1 to A3 and A8, it was confirmed that: by using PAA as a binder instead of styrene-butadiene rubber (SBR), the gas generation amount is reduced, and good floating charge characteristics can be obtained.

[0210] From the comparison between the electrochemical capacitors A1 and A9, it was confirmed that: by using CMC-Na, the gas generation amount and the floating charge characteristics can be obtained to be generally good.

[0211] From the comparison between the electrochemical capacitors A1 and A10, it was confirmed that: by using acetylene black (AB) instead of Ketjen black (KB), the specific surface area of the negative electrode binder layer is reduced by about more than 1 / 2. It is considered that the difference in the specific surface area between AB and KB and the difference in the structure between AB and KB have an impact on such a difference in results.

[0212] It should be noted that in the electrochemical capacitor A10, it can be considered that even when AB is increased so as to achieve the same specific surface area as A1, the gas generation amount is suppressed equally to that of A1. In other words, it can be said that even when using AB (furthermore, when using a conductive assistant other than AB and KB), by using it to such an extent that the mass ratio of the binder relative to the mass of the negative electrode binder layer is not greater than the mass ratio of the dispersant, it is possible to suppress the generation of decomposition gas and improve the floating charge characteristics at the same time.

[0213] [Evaluation 2: XPS Analysis of the Surface of the Negative Electrode Mix Layer]

[0214] The C1s spectrum, O1s spectrum, and Li1s spectrum of the surface of the negative electrode mix layer after exposure to a carbon dioxide atmosphere were analyzed by XPS. An X-ray photoelectron spectroscopy apparatus (trade name: Model 5600, manufactured by ULVAC-PHI, Inc.) was used in the analysis. The measurement conditions are shown below.

[0215] X-ray source: Al-mono (1486.6 eV) 14 kV / 200 W

[0216] Measurement diameter: 800 μmφ

[0217] Photoelectron extraction angle: 45°

[0218] Etching conditions: acceleration voltage of 3 kV, etching rate of approximately 3.1 nm / min (SiO2 conversion), grid area of 3.1 mm × 3.4 mm

[0219] The analysis results of the C1s spectrum, O1s spectrum, and Li1s spectrum confirmed that the thickness of the first layer was approximately 18 nm. Specifically, peaks such as C-C bonds presumably belonging to impurity carbon were observed on the outermost surface of the first layer, but they decreased sharply near a depth of 1 - 2 nm from the outermost surface of the first layer. On the other hand, a first peak attributed to C=O bonds was observed from the outermost surface of the first layer to a depth of 18 nm. A peak attributed to Li-O bonds was also observed near a depth of 18 nm. In addition, the presence of Li was constantly confirmed from the outermost surface of the first layer to a depth of 18 nm. No peak attributed to LiF was observed.

[0220] The surface of the negative electrode mix layer of the negative electrode taken out from the electrochemical capacitor was subjected to XPS analysis in the same manner as above, and the results confirmed that a SEI coating film (second layer) with a thickness of 10 nm, which had a different composition from the first layer and was distinguishable from the first layer, was formed. In addition, a peak attributed to LiF was observed.

[0221] Industrial Applicability

[0222] The electrochemical capacitor of the present invention is suitable for use in in-vehicle applications, for example.

[0223] Explanation of Reference Numerals

[0224] 100 Electrode body, 10 Positive electrode, 11x Exposed portion of the positive electrode current collector, 13 Positive electrode current collecting plate, 15 Terminal tab, 20 Negative electrode, 21x Exposed portion of the negative electrode current collector, 23 Negative electrode current collecting plate, 30 Separator, 200 Electrochemical capacitor, 210 Battery case, 220 Sealing plate, 221 Gasket.

Claims

1. An electrochemical capacitor, which comprises a positive electrode, a negative electrode, a separator, and a lithium-ion conductive electrolyte, The positive electrode includes a positive electrode current collector and a positive electrode mixture layer carried on the positive electrode current collector and reversibly doped with anions, The negative electrode includes a negative electrode current collector and a negative electrode mixture layer carried on the negative electrode current collector and reversibly doped with lithium ions, The negative electrode mixture layer contains a negative electrode active material, a conductive additive, a binder, and a dispersant, The proportion of the mass of the dispersant relative to the mass of the negative electrode mixture layer is greater than the proportion of the mass of the binder relative to the mass of the negative electrode mixture layer.

2. The electrochemical capacitor according to claim 1, wherein, The binder is at least one selected from fluororesin, acrylic resin, and rubber material.

3. The electrochemical capacitor according to claim 1, wherein, The binder contains styrene-butadiene rubber.

4. The electrochemical capacitor according to claim 1, wherein, The proportion of the mass of the binder relative to the mass of the negative electrode mixture layer is 0.3% or more and less than 5%.

5. The electrochemical capacitor according to claim 1, wherein, The dispersant is at least one selected from carboxymethyl cellulose and carboxymethyl cellulose salts.

6. The electrochemical capacitor according to claim 1, wherein, The dispersant contains an ammonium salt of carboxymethyl cellulose.

7. The electrochemical capacitor according to claim 1, wherein, The proportion of the mass of the dispersant relative to the mass of the negative electrode mixture layer is 1% or more and less than 10%.

8. The electrochemical capacitor according to claim 1, wherein, The proportion of the mass of the dispersant relative to the mass of the negative electrode mixture layer is 3% or more and less than 8%.

9. The electrochemical capacitor according to claim 1, wherein, The specific surface area of the negative electrode mixture layer is 10 m 2 / g or more and 70 m 2 / g or less.

10. The electrochemical capacitor according to claim 1, wherein, The negative electrode mixture layer contains at least one selected from Ketjen black, acetylene black, and carbon nanotubes as the conductive additive.

11. The electrochemical capacitor according to claim 1, wherein, The proportion of the mass of the conductive additive relative to the mass of the negative electrode mixture layer is 2% or more and less than 15%.

12. The electrochemical capacitor according to claim 1, wherein, The specific surface area of the conductive additive is 800 m 2 / g or more.

13. The electrochemical capacitor according to claim 1, wherein, The negative electrode active material contains hard carbon.

14. The electrochemical capacitor according to claim 1, wherein, The peeling strength of the negative electrode mixture layer peeled from the negative electrode current collector is 0.015 N / mm or more.

Citation Information

Patent Citations

  • Protective device for generator

    JP1988056145A