Covalent organic framework / melamine-based sponge composite material as well as preparation method and application thereof
By uniformly coating the covalent organic frame on the surface of melamine sponge, composite materials are prepared, which solves the problems of cumbersome preparation and insufficient mechanical strength of existing oil-water separation materials, and achieves efficient and stable oil-water separation effects, which are suitable for environmental protection and industrial production.
Patent Information
- Application Number
- CN202510562036.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-30
- Publication Date
- 2025-08-05
AI Technical Summary
The existing oil-water separation materials have problems such as cumbersome preparation, poor environmental protection of raw materials, insufficient mechanical strength, and difficulty in recycling. The traditional methods are inefficient, high cost or secondary pollution.
Through the impregnation-curing process, the covalent organic frame is uniformly coated on the surface of the melamine sponge to form a composite material based on the covalent organic frame/melamine sponge. Combining the hydrophobicity of the covalent organic frame and the mechanical properties of the melamine sponge, oil-water separation is achieved.
It realizes efficient oil-water separation, the materials have good stability in the water environment, are easy to recycle, reduces treatment costs, and are widely used in environmental protection and industrial production.
Smart Images

Figure CN120420957A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional materials, and in particular to a covalent organic framework / melamine sponge composite material and a preparation method and application thereof. Background Art
[0002] In modern industry and daily life, large amounts of oily wastewater enter water bodies, causing serious pollution, particularly in the petrochemical industry, water transportation, and mechanical processing. Globally, nearly 10 million tons of various oils enter the ocean each year, either directly or through water transport. This oil often floats on the water surface, hindering gas exchange between the interior and exterior of the water, leading to oxygen depletion and severely impacting aquatic life. Due to its relatively stable chemical properties, oil is difficult to break down and degrade naturally. Once this oily wastewater enters the water cycle, it can cause illness in humans and animals, disrupt aquatic ecosystems, and contribute to a host of environmental and social problems.
[0003] Traditional oil-water separation methods, such as gravity separation, centrifugal separation, and chemical treatment, often suffer from low efficiency, high cost, or secondary pollution. In recent years, adsorption separation technology based on porous materials has attracted widespread attention due to its high efficiency and environmental protection.
[0004] At present, most researchers in this field usually use chemical treatment of the surface of melamine sponge (MA sponge), such as introducing fluorine-containing, sulfur-containing and other organic groups, or using grafting polymerization on the surface of melamine sponge to prepare adsorbent oil and moisture materials. However, these materials still have the disadvantages of cumbersome preparation, poor environmental protection of raw materials, and difficulty in control.
[0005] Covalent organic frameworks (COFs) show great potential for oil-water separation due to their ordered pore structure, tunable chemical properties, and excellent stability. However, pure COFs often face challenges in practical applications, such as insufficient mechanical strength and difficulty in recycling. Melamine sponge, with its high porosity, excellent mechanical properties, and ease of processing, is an ideal support for the preparation of composite materials. Summary of the Invention
[0006] In order to solve the above technical problems, the present invention provides a covalent organic framework / melamine sponge composite material and its preparation method and application. Through a simple impregnation-curing process, the covalent organic framework is uniformly coated on the surface of the melamine sponge. The obtained covalent organic framework / melamine sponge composite material combines the excellent hydrophobicity of the covalent organic framework and the excellent mechanical properties of the melamine sponge, has excellent adsorption performance for a variety of oils and organic solvents, maintains high stability in an aqueous environment, can be reused multiple times without degrading the performance, and improves the overall performance and oil-water separation efficiency of the composite material.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a covalent organic framework / melamine sponge composite material, wherein the covalent organic framework / melamine sponge composite material comprises melamine sponge and a covalent organic framework material.
[0009] The covalent organic framework material is prepared by reacting an amino monomer with an aldehyde monomer.
[0010] The aldehyde monomer is an aldehyde monomer containing a hydroxyl group.
[0011] The present invention uses melamine sponge as a carrier and a covalent organic framework as a coating material to prepare a covalent organic framework / melamine sponge composite material. This composite material combines the excellent hydrophobicity of the covalent organic framework with the excellent mechanical properties of the melamine sponge. The composite material utilizes the surface dominance of the hydrophobic skeleton of the covalent organic framework and the shielding effect of the hydroxyl groups to encapsulate the hydroxyl groups within the framework, while the hydrophobic aromatic ring skeleton (such as benzene rings and imine bonds) is exposed on the surface of the material, forming a "hydrophobic shell." The present invention also utilizes the intramolecular interactions of the covalent organic framework and regulates its macrostructure, achieving a hydrophobic-lipophilic function. The composite material has a strong adsorption capacity for oils while repelling water, exhibiting excellent oil-water separation effect and enabling efficient oil-water separation.
[0012] Preferably, the aldehyde monomer containing a hydroxyl group includes any one of 2,5-dihydroxyterephthalaldehyde, 2,4-dihydroxybenzaldehyde or 5-hydroxyfuran-2-carbaldehyde, or a combination of at least two thereof, and more preferably 2,5-dihydroxyterephthalaldehyde.
[0013] Preferably, the amino monomer includes any one or a combination of at least two of 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 4',4"',4""'-(1,3,5-triazine ring-2,4,6-triyl)tris(([1,1'-biphenyl]-4-amine)) or 5"-(4'-amino[1,1'-biphenyl]-4-yl)[1,1':4',1":3",1"':4"',1""-pentaphenyl]-4,4""-diamine, and 1,3,5-tris(4-aminophenyl)benzene is further preferred.
[0014] Preferably, the molar ratio of the amino monomer to the aldehyde monomer containing a hydroxyl group is 1:(4-5), for example, 1:4, 1:4.2, 1:4.4, 1:4.6, 1:4.8 or 1:5.
[0015] Preferably, the reaction is carried out in the presence of a catalyst.
[0016] Preferably, the catalyst comprises glacial acetic acid.
[0017] Preferably, the catalyst is a glacial acetic acid solution with a glacial acetic acid concentration of 10-15 mol / L, for example, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L.
[0018] Preferably, based on the mass of the solute in the catalyst, the mass ratio of the aldehyde monomer to the catalyst is 1:(18-20), for example, 1:18, 1:18.5, 1:19, 1:19.5, or 1:20.
[0019] Preferably, the reaction is carried out in a solvent.
[0020] Preferably, based on the mass of the amino monomer, each gram of the amino monomer is dissolved in 1-2 L of solvent, for example, 1 L, 1.2 L, 1.4 L, 1.6 L, 1.8 L or 2 L.
[0021] Preferably, the solvent comprises dimethyl sulfoxide.
[0022] Preferably, the temperature for reacting the amino monomer and the aldehyde monomer is 20-30°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, and the time is 5-15 min, for example, 5 min, 7 min, 9 min, 10 min, 12 min, 14 min or 15 min.
[0023] In a second aspect, the present invention provides a method for preparing the covalent organic framework / melamine sponge composite material according to the first aspect, the preparation method comprising the following steps:
[0024] (1) Immersing the melamine sponge in a solution containing a covalent organic framework material;
[0025] (2) curing the impregnated melamine sponge to obtain the composite material.
[0026] The present invention prepares a covalent organic framework / melamine sponge composite material through a simple impregnation-curing process, using melamine sponge as a carrier and a covalent organic framework as a coating material. This preparation method achieves uniform coating of the covalent organic framework on the surface of the melamine sponge, is simple to operate and environmentally friendly, and does not require the use of harmful solvents or complex post-processing steps.
[0027] Preferably, the melamine sponge in step (1) is subjected to impurity removal and drying treatments.
[0028] Preferably, the impurity removal treatment is to soak the melamine sponge in ethanol for 1-2 hours, for example, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours, and then wash with water.
[0029] Preferably, the drying temperature is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C or 70°C, and the drying time is 20-30h, for example, 20h, 22h, 24h, 26h, 28h or 30h.
[0030] Preferably, the solvent of the solution containing the covalent organic framework material comprises dimethyl sulfoxide and / or acetonitrile.
[0031] Preferably, the concentration of the covalent organic framework material in the solution containing the covalent organic framework material is 1.5-3 g / L, for example, 1.5 g / L, 1.8 g / L, 2 g / L, 2.2 g / L, 2.5 g / L, 2.7 g / L or 3 g / L.
[0032] Preferably, the curing treatment temperature in step (3) is 20-30°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, and the curing time is 6-24h, for example, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24.
[0033] Preferably, the curing treatment further includes a washing step and a drying step.
[0034] Preferably, the solvent used in the washing step comprises ethanol.
[0035] Preferably, the temperature of the drying step is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C or 70°C, and the time is 30-40h, for example, 30h, 32h, 34h, 36h, 38h or 40h.
[0036] In a third aspect, the present invention provides an application of the covalent organic framework / melamine sponge composite material as described in the first aspect in oil-water separation.
[0037] Compared with the prior art, the present invention has at least the following beneficial effects:
[0038] (1) The covalent organic framework / melamine sponge composite material prepared by the present invention combines the excellent hydrophobicity of the covalent organic framework with the high porosity of the melamine sponge, so that the composite material has a strong adsorption capacity for oils while repelling water, and has an excellent oil-water separation effect, thereby achieving efficient oil-water separation.
[0039] (2) The present invention uses melamine sponge as a carrier to provide the composite material with good mechanical properties and stability. The covalent organic framework as a coating material enhances the overall strength of the composite material, allowing it to maintain high stability in an aqueous environment and not easily deformed or damaged. The material is easy to recycle and has excellent recycling performance, which reduces processing costs and reduces pollution to the environment.
[0040] (3) The present invention achieves uniform coating of the covalent organic framework material on the surface of the melamine sponge through a simple impregnation-curing process, and the operation is simple and environmentally friendly, without the need for the use of harmful solvents or complicated post-processing steps.
[0041] (4) The covalent organic framework / melamine sponge composite material prepared in the present invention is not only suitable for separating oil-water mixtures, but can also effectively treat complex systems such as oil-water emulsions and oily wastewater. The wide range of applications makes this composite material have great potential in the fields of environmental protection, industrial production and water treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a scanning electron microscope test image of melamine sponge;
[0043] Figure 2 This is a scanning electron microscope test image of the covalent organic framework-based melamine sponge composite material prepared in Example 1;
[0044] Figure 3 This is a water contact angle test graph based on the covalent organic framework / melamine sponge composite material prepared in Example 1;
[0045] Figure 4 This is a test diagram of oil-water separation of simulated heavy oil based on the covalent organic framework / melamine sponge composite material prepared in Example 1;
[0046] Figure 5 This is a test diagram of oil-water separation of simulated light oil based on the covalent organic framework / melamine sponge composite material prepared in Example 1;
[0047] Figure 6 This is a test chart of the adsorption results of different oil samples based on the covalent organic framework / melamine sponge composite material prepared in Example 1. DETAILED DESCRIPTION
[0048] The technical solution of the present invention will be further described below with reference to the accompanying drawings and through specific embodiments. However, the following examples are merely simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0049] The chemical reagents and solvents used in the following examples were all of analytical grade, and the raw materials were all available from chemical reagent companies or biopharmaceutical companies.
[0050] Example 1
[0051] A covalent organic framework / melamine sponge composite material, wherein the covalent organic framework / melamine sponge composite material is prepared by the following preparation method:
[0052] (1) Take a melamine sponge and cut it into pieces with a length of 3 cm, a width of 3 cm, a height of 3 cm and a volume of 27 cm. 3 After soaking the cubes in ethanol for 1.5 hours to remove impurities on the sponge, the melamine sponge was washed three times with deionized water to remove residual ethanol. The cubes were dried in an oven at 60°C for 22 hours to obtain the pretreated melamine sponge for later use.
[0053] Take a clean beaker, add 22.4 mg of 2,5-dihydroxyterephthalaldehyde, 10.5 mg of 1,3,5-tris(4-aminophenyl)benzene and 15 mL of dimethyl sulfoxide (the molar ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dihydroxyterephthalaldehyde is 1:4.5) into the beaker, sonicate the solution until it is clear, add 600 μL of 12 mol / L glacial acetic acid solution, and stir for 10 minutes to obtain a covalent organic framework precursor solution for later use.
[0054] (2) Immersing the pretreated melamine sponge into the covalent organic framework precursor solution, so that the liquid evenly submerges the entire melamine sponge.
[0055] (3) Seal the beaker with sealing film and let it stand at 25°C to cure for 12 hours.
[0056] (4) After complete curing, the excess solvent on the upper layer was removed, the melamine sponge was washed three times with ethanol, the excess ethanol was drained, and the melamine sponge was placed in a vacuum drying oven and vacuum dried at 60°C for 22 hours to obtain a covalent organic framework / melamine sponge composite material.
[0057] Example 2
[0058] A covalent organic framework / melamine sponge composite material, wherein the covalent organic framework / melamine sponge composite material is prepared by the following preparation method:
[0059] (1) Take a melamine sponge and cut it into pieces with a length of 2 cm, a width of 2 cm, a height of 2 cm and a volume of 8 cm. 3After soaking the cubes in ethanol for 2.5 hours to remove impurities on the sponge, the melamine sponge was washed three times with deionized water to remove residual ethanol. The cubes were dried in an oven at 60°C for 24 hours to obtain the pretreated melamine sponge for later use.
[0060] Take a clean beaker, add 11.2 mg of 2,5-dihydroxyterephthalaldehyde, 5.3 mg of 1,3,5-tris(4-aminophenyl)benzene and 9 mL of dimethyl sulfoxide (the molar ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dihydroxyterephthalaldehyde is 1:4.5) into the beaker, sonicate the solution until it is clear, add 300 μL of 12 mol / L glacial acetic acid solution, and stir for 10 minutes to obtain a covalent organic framework precursor solution for later use.
[0061] (2) Immersing the pretreated melamine sponge into the covalent organic framework precursor solution, so that the liquid evenly submerges the entire melamine sponge.
[0062] (3) Seal the beaker with sealing film and let it stand at 25°C for 6 hours to cure.
[0063] (4) After complete curing, the excess solvent on the upper layer was removed, the melamine sponge was washed three times with ethanol, the excess ethanol was drained, and the melamine sponge was placed in a vacuum drying oven and vacuum dried at 60°C for 24 hours to obtain a covalent organic framework / melamine sponge composite material.
[0064] Example 3
[0065] A covalent organic framework / melamine sponge composite material, wherein the covalent organic framework / melamine sponge composite material is prepared by the following preparation method:
[0066] (1) Take a melamine sponge and cut it into pieces with a length of 4 cm, a width of 4 cm, a height of 4 cm and a volume of 64 cm. 3 After soaking the cubes in ethanol for 1.5 hours to remove impurities on the sponge, the melamine sponge was washed three times with deionized water to remove residual ethanol. The cubes were dried in an oven at 60°C for 24 hours to obtain the pretreated melamine sponge for later use.
[0067] Take a clean beaker, add 33.6 mg of 2,5-dihydroxyterephthalaldehyde, 15.6 mg of 1,3,5-tris(4-aminophenyl)benzene and 20 mL of dimethyl sulfoxide (the molar ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dihydroxyterephthalaldehyde is 1:4.6) into the beaker, ultrasonicate the solution until it is clear, add 900 μL of 12 mol / L glacial acetic acid solution, and stir for 20 minutes to obtain a covalent organic framework precursor solution for later use.
[0068] (2) Immersing the pretreated melamine sponge into the covalent organic framework precursor solution, so that the liquid evenly submerges the entire melamine sponge.
[0069] (3) Seal the beaker with sealing film and let it stand at 25°C to cure for 12 hours.
[0070] (4) After complete curing, the excess solvent on the upper layer was removed, the melamine sponge was washed three times with ethanol, the excess ethanol was drained, and the melamine sponge was placed in a vacuum drying oven and vacuum dried at 60°C for 24 hours to obtain a covalent organic framework / melamine sponge composite material.
[0071] Example 4
[0072] A covalent organic framework / melamine sponge composite material, wherein the covalent organic framework / melamine sponge composite material is prepared by the following preparation method:
[0073] (1) Take a melamine sponge and cut it into pieces with a length of 5 cm, a width of 5 cm, a height of 5 cm and a volume of 125 cm. 3 After soaking the cubes in ethanol for 2.5 hours to remove impurities on the sponge, the melamine sponge was washed three times with deionized water to remove residual ethanol. The cubes were dried in an oven at 60°C for 36 hours to obtain the pretreated melamine sponge for later use.
[0074] Take a clean beaker, add 44.8 mg of 2,5-dihydroxyterephthalaldehyde, 21.2 mg of 1,3,5-tris(4-aminophenyl)benzene and 25 mL of dimethyl sulfoxide (the molar ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dihydroxyterephthalaldehyde is 1:4.5) into the beaker, sonicate the solution until it is clear, add 1.2 mL of 12 mol / L glacial acetic acid solution, and stir for 20 minutes to obtain a covalent organic framework precursor solution for later use.
[0075] (2) Immersing the pretreated melamine sponge into the covalent organic framework precursor solution, so that the liquid evenly submerges the entire melamine sponge.
[0076] (3) Seal the beaker with sealing film and let it stand at 25°C to cure for 12 hours.
[0077] (4) After complete curing, the excess solvent on the upper layer was removed, the melamine sponge was washed three times with ethanol, the excess ethanol was drained, and the melamine sponge was placed in a vacuum drying oven and vacuum dried at 60°C for 36 hours to obtain a covalent organic framework / melamine sponge composite material.
[0078] Example 5
[0079] A covalent organic framework / melamine sponge composite material, wherein the covalent organic framework / melamine sponge composite material is prepared by the following preparation method:
[0080] (1) Take a melamine sponge and cut it into pieces with a length of 6 cm, a width of 6 cm, a height of 6 cm and a volume of 216 cm. 3 After soaking the cubes in ethanol for 1.5 hours to remove impurities on the sponge, the melamine sponge was washed three times with deionized water to remove residual ethanol. The cubes were dried in an oven at 60°C for 24 hours to obtain the pretreated melamine sponge for later use.
[0081] Take a clean beaker, add 56 mg of 2,5-dihydroxyterephthalaldehyde, 26.5 mg of 1,3,5-tris(4-aminophenyl)benzene and 30 mL of dimethyl sulfoxide (the molar ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dihydroxyterephthalaldehyde is 1:4.5) into the beaker, sonicate the solution until it is clear, add 1.5 mL of 12 mol / L glacial acetic acid solution, and stir for 20 minutes to obtain a covalent organic framework precursor solution for later use.
[0082] (2) Immersing the pretreated melamine sponge into the covalent organic framework precursor solution, so that the liquid evenly submerges the entire melamine sponge.
[0083] (3) Seal the beaker with sealing film and let it stand at 25°C for 24 hours to cure.
[0084] (4) After complete curing, the excess solvent on the upper layer was removed, the melamine sponge was washed three times with ethanol, the excess ethanol was drained, and the melamine sponge was placed in a vacuum drying oven and vacuum dried at 60°C for 36 hours to obtain a covalent organic framework / melamine sponge composite material.
[0085] Example 6
[0086] A covalent organic framework / melamine sponge composite material, wherein the covalent organic framework / melamine sponge composite material is prepared by the following preparation method:
[0087] (1) Take a melamine sponge and cut it into pieces with a length of 9 cm, a width of 9 cm, a height of 9 cm and a volume of 729 cm. 3 After soaking the cubes in ethanol for 2 hours to remove impurities on the sponge, the melamine sponge was washed three times with deionized water to remove residual ethanol. The cubes were dried in an oven at 60°C for 36 hours to obtain the pretreated melamine sponge for later use.
[0088] Take a clean beaker, add 78.4 mg of 2,5-dihydroxyterephthalaldehyde, 37.1 mg of 1,3,5-tris(4-aminophenyl)benzene and 40 mL of dimethyl sulfoxide (the molar ratio of 1,3,5-tris(4-aminophenyl)benzene to 2,5-dihydroxyterephthalaldehyde is 1:4.5) into the beaker, ultrasonicate the solution until it is clear, add 2.1 mL of 12 mol / L glacial acetic acid solution, and stir for 20 minutes to obtain a covalent organic framework precursor solution for later use.
[0089] (2) Immersing the pretreated melamine sponge into the covalent organic framework precursor solution, so that the liquid evenly submerges the entire melamine sponge.
[0090] (3) Seal the beaker with sealing film and let it stand at 25°C for 24 hours to cure.
[0091] (4) After complete curing, the excess solvent on the upper layer was removed, the melamine sponge was washed three times with ethanol, the excess ethanol was drained, and the melamine sponge was placed in a vacuum drying oven and vacuum dried at 60°C for 36 hours to obtain a covalent organic framework / melamine sponge composite material.
[0092] Example 7
[0093] A covalent organic framework / melamine sponge composite material is different from Example 1 in that 1,3,5-tris(4-aminophenyl)benzene is replaced by an equimolar amount of 4',4"',4""'-(1,3,5-triazine ring-2,4,6-triyl)tris(([1,1'-biphenyl]-4-amine)).
[0094] Example 8
[0095] A covalent organic framework / melamine sponge composite material is different from Example 1 in that 1,3,5-tris(4-aminophenyl)benzene is replaced by an equimolar amount of 5"-(4'-amino[1,1'-biphenyl]-4-yl)[1,1':4',1":3",1"':4"',1""-pentaphenyl]-4,4""-diamine.
[0096] Example 9
[0097] A covalent organic framework / melamine sponge composite material is different from Example 1 in that 2,5-dihydroxyterephthalaldehyde is replaced by an equal molar amount of 5-hydroxyfuran-2-carboxaldehyde.
[0098] Example 10
[0099] A covalent organic framework / melamine sponge composite material is different from Example 1 in that the added amount of 2,5-dihydroxyterephthalaldehyde is 10.5 mg, and the molar ratio of 2,5-dihydroxyterephthalaldehyde to 1,3,5-tris(4-aminophenyl)benzene is 2.1:1.
[0100] Example 11
[0101] A covalent organic framework / melamine sponge composite material is different from Example 1 in that the added amount of 2,5-dihydroxyterephthalaldehyde is 52.5 mg, and the molar ratio of 2,5-dihydroxyterephthalaldehyde to 1,3,5-tris(4-aminophenyl)benzene is 10.6:1.
[0102] Comparative Example 1
[0103] A covalent organic framework / melamine sponge composite material is different from Example 1 in that 2,5-dihydroxyterephthalaldehyde is replaced by an equimolar amount of 2,5-bis(2-propyn-1-yloxy)-1,4-benzenedicarbaldehyde.
[0104] Test Method
[0105] (1) Water contact angle: The covalent organic framework / melamine sponge composite materials obtained in Examples 1-11 and Comparative Example 1 were placed in a contact angle meter to test their contact angles to water.
[0106] (2) Adsorption capacity test: The covalent organic framework / melamine sponge composite materials obtained in Examples 1-11 and Comparative Example 1 were subjected to adsorption capacity tests on silicone oil, pump oil, soybean oil, and n-hexane, respectively.
[0107] The weight of the covalent organic framework / melamine sponge composite material was recorded as M0 (g), and the weight of the material after it was placed in oil or organic solvent until adsorption saturation was recorded as M1 (g).
[0108] Qm / m=(M1-M0) / M0×100%;
[0109] Calculate mass adsorption capacity;
[0110] QV / V=(Qm / m)×(ds / dl);
[0111] Calculate the volumetric adsorption capacity, where ds and dl are the bulk density of the absorbent and the density of the absorbed liquid, respectively.
[0112] (3) Compression strength: Tested in accordance with GB / T 8813-2020 Determination of compression properties of rigid foam plastics.
[0113] (4) Resilience: The sample (20 mm × 20 mm × 20 mm) was tested using a universal material testing machine (Instron 5967) at a compression rate of 10 mm / min to test the compression deformation under maximum stress and the recovery rate after unloading.
[0114] (4) Cyclic performance: Refer to ASTM F726-17 Test for Oil Adsorption Capacity of Adsorbent Materials. The number of repetitions when the adsorption volume first drops below 95% is used as the cyclic performance test result.
[0115] (5) Stability: Solvent tolerance test solvent: Soak in ethanol, acetone, and n-hexane (representing polar / non-polar solvents) at room temperature for 24 hours and observe the structural collapse or dissolution phenomenon. No collapse or dissolution phenomenon is excellent, slight collapse or dissolution phenomenon is good, and obvious collapse or dissolution phenomenon in any solvent is poor.
[0116] Test results
[0117] The covalent organic framework / melamine sponge composite materials obtained in Examples 1-11 and Comparative Example 1 were tested, and the test results are shown in Table 1 below:
[0118] Table 1
[0119]
[0120] The test results show that:
[0121] (1) It can be seen from Examples 1 to 6 that the covalent organic framework / melamine sponge composite material prepared by the present invention combines the excellent hydrophobicity of the covalent organic framework and the excellent mechanical properties of the melamine sponge, with a water contact angle greater than 130°, an adsorption capacity for silicone oil, pump oil, soybean oil, and n-hexane of more than 85%, a compressive strength of more than 10 KPa, a rebound resilience of more than 90%, can be reused more than 45 times, and has excellent solvent tolerance.
[0122] (2) It can be seen from Examples 1 to 7-11 that the present invention achieves better adsorption effect and mechanical properties by further optimizing 2,5-dihydroxyterephthalaldehyde as the aldehyde monomer, 1,3,5-tris(4-aminophenyl)benzene as the amino monomer, and the molar ratio of the aldehyde monomer to the amino monomer.
[0123] (3) It can be seen from Example 1 and Comparative Example 1 that the present invention realizes the hydrophobic-lipophilic function by utilizing the surface dominance of the covalent organic framework hydrophobic skeleton and the shielding effect of the hydroxyl group, has a strong adsorption capacity for oils, and repels water at the same time, has an excellent oil-water separation effect, and realizes efficient oil-water separation.
[0124] Figure 1This is a scanning electron microscope test image of melamine sponge. From the image, we can observe that the melamine sponge has three-dimensional layers and smooth, porous structural characteristics.
[0125] Figure 2 This is a scanning electron microscope test image of the covalent organic framework / melamine sponge composite material prepared in Example 1. It can be observed from the figure that after modification with the covalent organic framework material, the skeleton structure of the sponge has not changed, and the original porous three-dimensional structure is retained. The sponge skeleton is covered with a layer of rough structure (covalent organic framework), which increases the hydrophobicity of the sponge.
[0126] Figure 3 This is a water contact angle test diagram of the covalent organic framework / melamine sponge composite material prepared in Example 1. The left contact angle of the material is 138.2°, and the right contact angle is 141.0°, which shows excellent hydrophobic properties.
[0127] Figure 4 This is an oil-water separation test diagram of the simulated heavy oil based on the covalent organic framework / melamine sponge composite material prepared in Example 1. Chloroform was used to simulate the heavy oil and dyed with Sudan III. From the figure, it can be observed that the red chloroform sinks to the bottom of the liquid. The material can completely adsorb the chloroform at the bottom and does not absorb water.
[0128] Figure 5 This image shows the oil-water separation test of the simulated light oil based on the covalent organic framework / melamine sponge composite prepared in Example 1. The simulated light oil was dyed with Sudan III using n-hexadecane. The image shows red n-hexadecane floating on the top of the liquid, indicating that the material completely absorbs the top n-hexadecane without absorbing water.
[0129] Figure 6 The adsorption test results of different oil samples based on the covalent organic framework / melamine sponge composite material prepared in Example 1 are shown. The mass and volume adsorption capacities of the superhydrophobic covalent organic framework sponge composite material for silicone oil, pump oil, soybean oil, and n-hexane samples were tested. It was observed that the adsorption capacity of the material for each oil sample was higher than 0.7 mL / cm 3 , indicating that the superhydrophobic covalent organic framework sponge composite material has good adsorption capacity for the four oil samples.
[0130] The applicant declares that the above is only a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention fall within the scope of protection and disclosure of the present invention.
Claims
1. A covalent organic framework / melamine sponge composite material, characterized in that: The covalent organic framework / melamine sponge composite material comprises melamine sponge and a covalent organic framework material; The covalent organic framework material is prepared by reacting an amino monomer with an aldehyde monomer; The aldehyde monomer is an aldehyde monomer containing a hydroxyl group.
2. The composite material according to claim 1, characterized in that The aldehyde monomer containing a hydroxyl group includes any one of 2,5-dihydroxyterephthalaldehyde, 2,4-dihydroxybenzaldehyde or 5-hydroxyfuran-2-carboxaldehyde, or a combination of at least two thereof, and 2,5-dihydroxyterephthalaldehyde is more preferred; Preferably, the amino monomer includes any one or a combination of at least two of 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 4',4"',4""'-(1,3,5-triazine ring-2,4,6-triyl)tris(([1,1'-biphenyl]-4-amine)) or 5"-(4'-amino[1,1'-biphenyl]-4-yl)[1,1':4',1":3",1"':4"',1""-pentaphenyl]-4,4""-diamine, and 1,3,5-tris(4-aminophenyl)benzene is further preferred.
3. The covalent organic framework / melamine sponge composite material according to claim 1 or 2, characterized in that: The molar ratio of the amino monomer to the aldehyde monomer containing a hydroxyl group is 1:(4-5).
4. The covalent organic framework / melamine sponge composite material according to any one of claims 1 to 3, characterized in that: The reaction is carried out in the presence of a catalyst; Preferably, the catalyst comprises glacial acetic acid; Preferably, the catalyst is a glacial acetic acid solution with a glacial acetic acid concentration of 10-15 mol / L; Preferably, based on the mass of the solute in the catalyst, the mass ratio of the aldehyde monomer to the catalyst is 1:(18-20).
5. The covalent organic framework / melamine sponge composite material according to any one of claims 1 to 4, characterized in that: The reaction is carried out under the conditions of a solvent; Preferably, based on the mass of the amino monomer, each gram of the amino monomer is dissolved in 1-2 L of solvent; Preferably, the solvent comprises dimethyl sulfoxide.
6. The covalent organic framework / melamine sponge composite material according to any one of claims 1 to 5, characterized in that: The temperature for reacting the amino monomer and the aldehyde monomer is 20-30° C., and the time is 5-15 minutes.
7. A method for preparing a covalent organic framework / melamine sponge composite material according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) Immersing the melamine sponge in a solution containing a covalent organic framework material; (2) curing the impregnated melamine sponge to obtain the composite material.
8. The method for preparing the covalent organic framework / melamine sponge composite material according to claim 7, characterized in that: The melamine sponge in step (1) is subjected to impurity removal and drying treatments; Preferably, the impurity removal treatment is to soak the melamine sponge in ethanol for 1-2 hours and then wash it with water; Preferably, the drying temperature is 50-70° C. and the drying time is 20-30 h.
9. The method for preparing the covalent organic framework / melamine sponge composite material according to claim 7 or 8, characterized in that: The solvent of the solution containing the covalent organic framework material includes dimethyl sulfoxide and / or acetonitrile; Preferably, the concentration of the covalent organic framework material in the solution containing the covalent organic framework material is 1.5-3 g / L; Preferably, the curing treatment temperature in step (3) is 20-30°C and the time is 6-24h; Preferably, the curing treatment further includes a washing step and a drying step; Preferably, the solvent used in the washing step comprises ethanol; Preferably, the temperature of the drying step is 50-70° C. and the time is 30-40 hours.
10. Use of the covalent organic framework / melamine sponge composite material according to any one of claims 1 to 6 in oil-water separation.
Citation Information
Cited By
Hydrophobic oleophylic modified sponge, preparation method thereof and application of hydrophobic oleophylic modified sponge in oil-water separation
CN119240857A
Hydrophobic and lipophilic modified sponge, preparation method and application thereof in oil-water separation
CN119240857B
Functionalized super-hydrophobic melamine sponge as well as preparation method and application thereof
CN122124504A