Preparation method and application of amorphous nickel-cobalt-iron phosphate anode catalyst

The amorphous nickel-cobalt iron phosphate catalyst was synthesized at room temperature by the solution method, which solved the stability and preparation energy consumption of traditional nickel-iron-based oxide anode catalyst in the electrolytic hydrogen production technology of anion exchange membrane, and achieved high-efficiency and low-cost large-scale application of catalysts, improving the oxygen evolution reaction performance and the efficiency of electrolyzed hydrogen production.

CN120553668APending Publication Date: 2025-08-29NANJING DAQUAN ZHONGKE HYDROGEN ENERGY TECHNOLOGY CO LTD +1
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202510801395.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-16
Publication Date
2025-08-29

AI Technical Summary

Technical Problem

The existing non-precious metal nickel-ferro-based oxide/hydroxide anode catalysts have problems such as attenuation of active site caused by Fe3+ dissolution at high potentials, interface defects caused by lattice mismatch, and high energy consumption and difficulty in batching of traditional preparation processes, which limit their application in the anion exchange membrane electrolysis hydrogen production technology.

Method used

Amorphous nickel-cobalt iron phosphate catalyst was prepared by the solution method. Through the co-precipitation reaction of nickel, cobalt, iron salt and phosphate, combined with ultrasonic spraying and hot pressing technology, it was loaded on the surface of nickel felt or anion exchange membrane to form a high-performance anode assembly.

Benefits of technology

It has achieved large-scale green preparation of catalysts, reduced energy consumption, improved catalytic activity and stability, and exceeded the large-scale application of traditional catalysts in anion exchange membrane electrolytic cells, demonstrated excellent oxygen evolution reaction performance and low charge transfer resistance, and had significant industrial prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120553668A_ABST
    Figure CN120553668A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an amorphous nickel-cobalt-iron phosphate anode catalyst, and belongs to the technical field of alkaline water electrolysis hydrogen production, the preparation method comprises the following steps: (1) dissolving transition metal salt in a solvent, and stirring to obtain a metal salt solution; (2) dissolving phosphate in a solvent, and stirring to obtain a phosphate solution; and (3) adding the phosphate solution into the metal salt solution for reaction, washing with deionized water and ethanol, centrifugally separating, and drying to obtain the amorphous nickel-cobalt-iron phosphate anode catalyst. According to the preparation method and application of the amorphous nickel-cobalt-iron phosphate anode catalyst, process safety improvement and environmental friendliness optimization are achieved through an all-water-phase green synthesis system, the obtained catalyst shows excellent performance in an AEM electrolytic cell, the cell voltage is only 1.87 V under the current density of 2 A / cm, and the method has remarkable industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogen production by alkaline water electrolysis, and in particular relates to a preparation method and application of an amorphous nickel-cobalt-iron phosphate anode catalyst. Background Art

[0002] In the process of building a new power system dominated by renewable energy, developing water electrolysis hydrogen production technology capable of adapting to wide power fluctuations is one of the core paths to achieving carbon neutrality. Anion exchange membrane water electrolysis (AEMWE) technology achieves a breakthrough balance between material cost and system efficiency by creatively coupling the technological advantages of alkaline electrolysis and proton exchange membrane electrolysis. On the one hand, it inherits the low-cost characteristics of alkaline systems using non-precious metal catalysts, and on the other hand, it integrates the technical characteristics of proton membrane systems, such as high current density, rapid start-stop response, and high gas purity. It is particularly suitable for direct coupling hydrogen production scenarios with fluctuating power sources such as wind power and photovoltaics. This cross-generational technological integration solves the dual dilemma of the low efficiency of traditional alkaline electrolyzers and the high cost of proton membrane electrolyzers.

[0003] The performance of the anode catalyst in the membrane electrode assembly (MEA) directly determines the hydrogen production efficiency and commercialization process of the AEMWE system. The anode oxygen evolution reaction (OER) involves a four-electron transfer pathway. Its slow kinetic characteristics lead to a high reaction overpotential, which has become a core bottleneck restricting the improvement of the system's energy efficiency. Current commercial catalysts are mainly precious metal oxides such as IrO2 / RuO2, but their scarcity and price volatility severely limit the large-scale application of the technology. Although non-precious metal nickel-iron-based oxides / hydroxides have shown substitution potential in alkaline OER, they face three major challenges: ① Fe at high potential 3+ ① The dynamic decay of active sites caused by preferential dissolution leads to a high decay rate during the stability test; ② The NiOOH / FeOOH heterojunction generated by surface reconstruction produces high-density interface defects due to lattice mismatch, resulting in a decrease in electron mobility (poor conductivity); ③ The traditional preparation process relies on high-temperature hydrothermal, inert atmosphere protection and organic template assistance, which has high energy consumption, difficulty in batch preparation, poor batch consistency and safety hazards. Therefore, it is necessary to develop a new preparation method and application of amorphous nickel cobalt iron phosphate anode catalyst to solve the existing problems. Summary of the Invention

[0004] The purpose of the present invention is to provide a preparation method and application of an amorphous nickel-cobalt-iron phosphate anode catalyst to solve the above problems.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing an amorphous nickel-cobalt-iron phosphate anode catalyst, comprising the following steps: (1) Adding a transition metal salt in a specific ratio into a reaction vessel, adding a solvent, placing the reaction vessel on a magnetic stirrer, and stirring until the transition metal salt is completely dissolved to obtain a metal salt solution; (2) Weigh an appropriate amount of phosphate and dissolve it in a solvent. Place it on a magnetic stirrer and stir until it is completely dissolved to obtain a phosphate solution. (3) The completely dissolved phosphate solution is quickly poured into the metal salt solution in step (1). After a certain reaction time, the solution is washed with deionized water and ethanol for multiple times, centrifuged, and dried in an oven to obtain an amorphous nickel cobalt iron phosphate anode catalyst.

[0006] Preferably, the transition metal salts include nickel salts, cobalt salts and iron salts.

[0007] Preferably, the nickel salt is selected from one or more of nickel nitrate, nickel sulfate, nickel chloride and nickel acetate.

[0008] Preferably, the cobalt salt is selected from one or more of cobalt nitrate, cobalt sulfate, cobalt chloride and cobalt acetate.

[0009] Preferably, the iron salt is selected from one or more of ferric nitrate, ferric sulfate, ferric chloride and ferric acetate.

[0010] Preferably, the solvent is selected from one or more of deionized water, ethanol, ethylene glycol, and isopropanol.

[0011] Preferably, the phosphate is selected from one or more of trisodium phosphate, tripotassium phosphate, triammonium phosphate, and sodium hypophosphite.

[0012] Preferably, the total mass ratio of the iron salt to the nickel salt and the cobalt salt is 1:(10-2), wherein the molar ratio of the nickel salt to the cobalt salt is 1:1-1:3.

[0013] Preferably, the molar ratio of the phosphate to the metal salt is 1:1 to 1:3, and the metal salt includes nickel salt, cobalt salt, and iron salt.

[0014] Preferably, the reaction is carried out at room temperature for 1 to 3 hours.

[0015] Preferably, the reaction is carried out at room temperature for 1 to 2 hours.

[0016] Preferably, the drying is carried out in an oven at a drying temperature of 50-80°C.

[0017] Preferably, the drying temperature is 60-80°C Preferably, the total mass ratio of the iron salt to the nickel salt and the cobalt salt is 1:(10~3), wherein the molar ratio of the nickel salt to the cobalt salt is 1:1~1:2.

[0018] Preferably, the phosphate is one or more of trisodium phosphate, tripotassium phosphate and ammonium phosphate.

[0019] Preferably, the molar ratio of the phosphate to the transition metal salt is 1:1 to 1:2.

[0020] Preferably, the selected transition metal salt is one or more of nitrates, sulfates, hydrochlorides and acetates of nickel, cobalt and iron.

[0021] The present invention further provides an amorphous nickel-cobalt-iron phosphate anode catalyst obtained by the above-mentioned preparation method for use in anion exchange membrane water electrolysis to produce hydrogen, comprising the following steps: Preparation of catalyst slurry: Place amorphous nickel cobalt iron phosphate powder anode catalyst, ball milling medium and solvent in a certain proportion in the ball mill jar of a ball mill and grind in sections; The ground amorphous nickel cobalt iron phosphate slurry is transferred to a mixed solvent containing an ionomer, and ultrasonically dispersed in a high-power ultrasonic instrument to obtain an amorphous nickel cobalt iron phosphate anode catalyst dispersion; Preparation of anion exchange membrane anode membrane electrode: Place the cut nickel felt substrate or anion exchange membrane on the heating plate of an ultrasonic sprayer, and use the ultrasonic sprayer to spray the catalyst slurry on the nickel felt substrate or anion exchange membrane to make a catalyst coated substrate (CCS) membrane electrode or catalyst coated membrane (CCM) membrane electrode; hot press the sprayed catalyst coated substrate membrane electrode or catalyst coated membrane membrane electrode on a hot press and use it as the anode of the anion exchange membrane (AEM) water electrolysis hydrogen production device for AEM water electrolysis performance testing.

[0022] Preferably, the mass ratio of the amorphous nickel cobalt iron phosphate anode catalyst, the ball milling medium, and the solvent is 1:40:5; and the ball milling medium is zirconia ball milling beads.

[0023] Preferably, the grinding process is segmented grinding, using a four-stage series ball milling device, with the rotation speed of each ball mill being 750 rpm and the ball milling time of each segment being 5 minutes.

[0024] Preferably, during the preparation of the amorphous nickel cobalt iron phosphate catalyst dispersion, the mass ratio of the ionomer to the amorphous nickel cobalt iron phosphate anode catalyst is 1:(4-5); Preferably, the mixed solvent consists of isopropanol and water, and the volume ratio of water to isopropanol is 1:(1-2); the mass concentration of the catalyst dispersion is 7.5-10 mg / mL.

[0025] Preferably, the nickel felt substrate or the anion exchange membrane is placed on a heating plate of an ultrasonic spray coating apparatus, and the heating temperature of the heating plate is 60-80°C.

[0026] Preferably, the spraying speed of the ultrasonic sprayer is set to 0.11 ml / time.

[0027] Preferably, the hot pressing temperature of the catalyst-coated substrate membrane electrode or the catalyst-coated membrane electrode is 100-150° C., the hot pressing time is 5-20 minutes, and the hot pressing pressure is 50-100 kPa.

[0028] Preferably, during the milling process, the mass ratio of the amorphous nickel cobalt iron phosphate anode catalyst, the ball milling medium, and the solvent is 1:(30-50):(4-6).

[0029] Preferably, the grinding process includes: using a four-stage series ball milling device, the rotation speed of each stage of the ball mill is 700-800 rpm, and the ball milling time of each stage is 4-6 minutes.

[0030] Preferably, during the preparation of the dispersion, the mass ratio of the ionomer to the amorphous nickel cobalt iron phosphate anode catalyst is 1:(3~5); the mixed solvent consists of isopropanol and water, and the volume ratio of water to isopropanol is 1:(1~3); the mass concentration of the finally prepared catalyst dispersion is 7.5~15 mg / mL.

[0031] Preferably, the hot pressing temperature is 100-160° C., the hot pressing time is 5-30 minutes, and the hot pressing pressure is 50 kPa-100 kPa.

[0032] The technical effects and advantages of the present invention are as follows: the preparation method and application of the amorphous nickel cobalt iron phosphate anode catalyst achieves improved process safety and optimized environmental friendliness through an all-aqueous green synthesis system, abandons the use of toxic solvents and controlled reagents, and can achieve large-scale preparation of the catalyst at room temperature and pressure; experiments show that the obtained catalyst exhibits excellent performance in the AEM electrolytic cell, and the cell voltage only requires 1.87V at a current density of 2A / cm², which has significant prospects for industrial application; the green synthesis of the catalyst is achieved through a mild room-temperature aqueous reaction system, and its simplified process flow greatly reduces the energy consumption of preparation; it exhibits excellent scalability, with a single batch output of up to 100 grams, and the catalyst crystal structure and active component distribution remain highly uniform during the scale-up production process, effectively solving the performance attenuation problem that is common in the scale-up process of traditional catalysts; in terms of catalytic performance, the prepared amorphous nickel cobalt iron phosphate catalyst exhibits excellent oxygen evolution reaction activity (OER); more importantly, through the coordinated regulation of the ternary metal cobalt, the charge transfer resistance of the catalyst is significantly reduced. This optimization of the electronic structure not only improves the intrinsic catalytic activity, but also enhances the kinetic characteristics of the catalytic process; the breakthrough provides a new anode catalytic material with both high performance and industrialization potential for large-scale hydrogen production applications of anion exchange membrane electrolyzers; through a room-temperature controllable synthesis process and a multi-metal coordinated optimization strategy, the technical barriers of activity attenuation and complex processes in the large-scale preparation of traditional amorphous catalysts are broken through; the stable preparation of a single batch of 100-gram-level high-activity nickel cobalt iron phosphate catalysts is achieved, and its OER overpotential and charge transfer resistance are greatly reduced compared with the amorphous nickel iron phosphate materials prepared by existing technologies; it not only provides a solution with high-efficiency catalytic activity, excellent amplification characteristics and process universality for the low-cost industrialization of anion exchange membrane water electrolysis hydrogen production technology, but also has important engineering application value for promoting the large-scale production of green hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 X-ray diffraction (XRD) patterns of the amorphous nickel-iron salt prepared in Comparative Example 1 of the present invention and the amorphous nickel-cobalt-iron phosphate powder samples prepared in Example 1; Figure 2a This is a transmission electron microscope (TEM) image of the amorphous nickel iron phosphate prepared in Comparative Example 1 of the present invention; Figure 2b This is a transmission electron microscope (TEM) image of the amorphous nickel-cobalt-iron phosphate prepared in Example 1 of the present invention; Figure 3a Polarization curves of the oxygen evolution reaction (OER) of the amorphous nickel iron phosphate prepared in Comparative Example 1 of the present invention, the nickel cobalt phosphate prepared in Comparative Example 2, and the amorphous nickel cobalt iron phosphate prepared in Examples 1 to 3 in a three-electrode system; Figure 3bElectrochemical impedance spectroscopy (EIS) spectra of the amorphous nickel iron phosphate prepared in Comparative Example 1 of the present invention, the nickel cobalt phosphate prepared in Comparative Example 2, and the amorphous nickel cobalt iron phosphate prepared in Examples 1 to 3 under a three-electrode system; Figure 4 The performance curves of the membrane electrode using the amorphous nickel iron phosphate prepared in comparative example 1 of the present invention, the nickel cobalt phosphate prepared in comparative example 2, and the amorphous nickel cobalt iron phosphate prepared in Examples 1 to 3 as anodes in an anion exchange membrane (AEM) water electrolysis device are shown. DETAILED DESCRIPTION

[0034] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0035] The invention provides a preparation method of an amorphous nickel-cobalt-iron-phosphate anode catalyst, which adopts a solution method and room temperature synthesis process. The specific steps include: dissolving a nickel salt, a cobalt salt, and an iron salt in a solvent according to a predetermined molar ratio to form a mixed metal salt solution; adding a potassium phosphate precipitant to the solution to carry out a coprecipitation reaction, and stirring at room temperature to obtain an amorphous nickel-cobalt-iron-phosphate powder catalyst; preparing the obtained catalyst powder, an ionomer, and a solvent according to an optimized ratio to form a uniform dispersion liquid, and loading it on the surface of a nickel felt or an anion exchange membrane through an ultrasonic spraying process to form an anode assembly; and the anode and a carbon paper cathode coated with commercial Pt / C through the anion exchange membrane to form a membrane electrode assembly for testing hydrogen production by electrolysis of water.

[0036] The present invention further provides an amorphous nickel-cobalt-iron phosphate anode catalyst obtained by the above preparation method for use in anion exchange membrane water electrolysis to produce hydrogen.

[0037] Preparation of catalyst slurry: Place amorphous nickel cobalt iron phosphate powder anode catalyst, ball milling medium and solvent in a certain proportion in the ball mill jar of a ball mill and grind in sections; The ground amorphous nickel cobalt iron phosphate slurry is transferred to a mixed solvent containing an ionomer, and ultrasonically dispersed in a high-power ultrasonic instrument to obtain an amorphous nickel cobalt iron phosphate anode catalyst dispersion; Preparation of anion exchange membrane anode membrane electrode: Place the cut nickel felt substrate or anion exchange membrane on the heating plate of an ultrasonic sprayer, and use the ultrasonic sprayer to spray the catalyst slurry on the nickel felt substrate or anion exchange membrane to make a catalyst coated substrate (CCS) membrane electrode or catalyst coated membrane (CCM) membrane electrode; hot press the sprayed catalyst coated substrate membrane electrode or catalyst coated membrane membrane electrode on a hot press and use it as the anode of the anion exchange membrane (AEM) water electrolysis hydrogen production device for AEM water electrolysis performance testing.

[0038] Control Example 1; A preparation method of amorphous nickel iron phosphate: 30 mmol of nickel chloride and 10 mmol of ferric chloride were weighed and dissolved in 10 mL of water and magnetically stirred until completely dissolved to form a metal salt mixed solution. Subsequently, 40 mmol of tripotassium phosphate was weighed and dissolved in 10 mL of water and ultrasonically treated until completely dissolved. The tripotassium phosphate solution was poured into the metal salt mixed solution and magnetically stirred for 2 hours. After the reaction was completed, the mixture was washed with deionized water several times, centrifuged, dried, and ground to obtain a yellow-green product.

[0039] Alkaline OER performance test method of the amorphous nickel iron phosphate catalyst prepared above in a three-electrode system: Preparation of the dispersion (ink): 5 mg of the catalyst prepared above was weighed and dispersed in a mixture of 380 μL of deionized water and 600 μL of isopropanol. 20 μL of Nafion solution (5% by mass) was then added and ultrasonicated for 60 minutes to form a uniform slurry (ink). 10 μL of the catalyst ink was measured with a pipette and dispersed on a 5 mm diameter glassy carbon electrode. After natural drying, it was used as the working electrode. A mercury / mercuric oxide electrode and a platinum sheet were used as the reference electrode and the counter electrode, respectively. In a standard three-electrode system, the prepared catalyst was tested for OER performance in a 1 M KOH solution using an electrochemical workstation (CHI660e) and a rotating disk electrode (RDE). Test method: Electrochemical polarization curve (LSV) test was performed in the voltage range of 0~0.8 V vs. Hg / HgO, with a scan rate of 0.01 V·s -1 , the rotation speed is 2500 rpm. All potentials in LSV are corrected for ir compensation.

[0040] Preparation and testing method of the above-prepared amorphous nickel iron phosphate catalyst in AEM membrane electrode: Preparation of membrane electrode: amorphous nickel iron phosphate powder, zirconium oxide ball milling beads and solvent were placed in the ball mill of a ball mill in a ratio of 1:40:5, and ground in four stages, each for 5 minutes, with a ball mill speed of 750 rpm; the ground amorphous nickel iron phosphate slurry was transferred to a mixed solvent containing ionomer (the mass ratio of catalyst to ionomer was 4:1, and the volume ratio of water to isopropanol in the mixed solvent was 1:2) to prepare an amorphous nickel iron phosphate catalyst dispersion with a mass concentration of 7.5 mg / mL, and ultrasonically dispersed in a high-power ultrasonic instrument to obtain an amorphous nickel iron phosphate anode catalyst dispersion; then, the catalyst dispersion was sprayed on the nickel fiber felt substrate using an ultrasonic sprayer (the spraying rate was 0.11 ml / time, each time took 14 seconds, the membrane electrode heating plate temperature was 80°C, and the loading amount was 3 mg / cm 2 The obtained nickel fiber felt-supported amorphous nickel iron phosphate electrode was placed in a hot press and hot pressed at 120°C and 100 kPa for 30 minutes to obtain a membrane electrode as the anode of the AEM water electrolysis device; the cathode was similarly sprayed with commercial platinum carbon loaded on carbon fiber paper (loading amount 2 mg / cm 2 ); An anion exchange membrane water electrolysis (AEMWE) device was assembled using commercial anion exchange membranes, and its water electrolysis performance was tested; experimental results show that at an operating temperature of 60°C, when the current density reaches 2 A / cm², the operating potential of the device is only 1.81 V; this excellent electrochemical performance indicates that this material has significant industrial application prospects as a cathode oxygen evolution reaction (OER) catalyst in AEMWE water electrolysis.

[0041] Preparation method of nickel cobalt phosphate: Control Example 2; 30 mmol of nickel chloride and 10 mmol of cobalt chloride were weighed and dissolved in 10 mL of water and magnetically stirred until completely dissolved to form a metal salt mixed solution. Subsequently, 40 mmol of tripotassium phosphate was weighed and dissolved in 10 mL of water and ultrasonically treated until completely dissolved. The tripotassium phosphate solution was poured into the metal salt mixed solution and magnetically stirred for 2 hours. After the reaction was completed, the mixture was washed with deionized water several times, centrifuged, dried, and ground to obtain a gray product.

[0042] The preparation method of the nickel cobalt phosphate catalyst dispersion prepared in Comparative Example 2 and the alkaline OER performance test method in the three-electrode system are the same as those in Comparative Example 1.

[0043] The preparation process of the membrane electrode based on the nickel cobalt phosphate catalyst obtained in Comparative Example 2 and its application in the AEM water electrolysis device are the same as those in Comparative Example 1.

[0044] A method for preparing an amorphous nickel-cobalt-iron phosphate anode catalyst for anion exchange membrane water electrolysis to produce hydrogen: Example

[0045] 30 mmol of nickel chloride, 7 mmol of cobalt chloride and 3 mmol of ferric chloride were weighed and dissolved in 10 mL of water and magnetically stirred until completely dissolved to form a metal salt mixed solution; then, 40 mmol of tripotassium phosphate was weighed and dissolved in 10 mL of water and ultrasonically treated until completely dissolved; the tripotassium phosphate solution was poured into the metal salt mixed solution and magnetically stirred for 2 hours; after the reaction was completed, the mixture was washed with deionized water several times, centrifuged, dried and ground to obtain a synthesized amorphous nickel cobalt iron phosphate solid powder, the apparent color of which was gray-green.

[0046] The preparation method of the amorphous nickel cobalt iron phosphate catalyst dispersion prepared in Example 1 and the alkaline OER performance test method in a three-electrode system are the same as those in Comparative Example 1.

[0047] The preparation process of the membrane electrode based on the amorphous nickel cobalt iron phosphate catalyst obtained in Example 1 and its application in the AEM water electrolysis device are the same as those in Comparative Example 1. Example

[0048] 30 mmol of nickel chloride, 8 mmol of cobalt chloride, and 2 mmol of ferric chloride were weighed and dissolved in 10 mL of water and magnetically stirred until completely dissolved to form a metal salt mixed solution. Subsequently, 40 mmol of tripotassium phosphate was weighed and dissolved in 10 mL of water and ultrasonically treated until completely dissolved. The tripotassium phosphate solution was poured into the metal salt mixed solution and magnetically stirred for 2 hours. After the reaction was completed, the mixture was washed with deionized water several times and centrifuged to obtain a gray-green precipitate.

[0049] The preparation method of the amorphous nickel cobalt iron phosphate catalyst dispersion prepared in Example 2 and the alkaline OER performance test method in a three-electrode system are the same as those in Comparative Example 1.

[0050] The preparation process of the membrane electrode based on the amorphous nickel cobalt iron phosphate catalyst obtained in Example 1 and its application in the AEM water electrolysis device are the same as those in Comparative Example 1. Example

[0051] 30 mmol of nickel chloride, 9 mmol of cobalt chloride, and 1 mmol of ferric chloride were weighed and dissolved in 10 mL of water and magnetically stirred until completely dissolved to form a metal salt mixed solution. Subsequently, 40 mmol of tripotassium phosphate was weighed and dissolved in 10 mL of water and ultrasonically treated until completely dissolved. The tripotassium phosphate solution was poured into the metal salt mixed solution and magnetically stirred for 2 hours. After the reaction was completed, the mixture was washed with deionized water several times and centrifuged to obtain a gray-green precipitate.

[0052] The preparation method of the amorphous nickel cobalt iron phosphate catalyst dispersion prepared in Example 1 and the alkaline OER performance test method in a three-electrode system are the same as those in Comparative Example 1.

[0053] The preparation process of the membrane electrode based on the amorphous nickel cobalt iron phosphate catalyst obtained in Example 1 and its application in the AEM water electrolysis device are the same as those in Comparative Example 1.

[0054] like Figure 1 From the XRD patterns of the samples, it can be seen that the nickel iron phosphate and nickel cobalt iron phosphate prepared in Control Example 1 and Example 1 are both amorphous structures.

[0055] like Figure 2a 、 Figure 2b From the TEM images of the samples, it can be seen that the nickel iron phosphate prepared in Control Example 1 presents agglomerated nanoparticles, while the nickel cobalt iron phosphate prepared in Example 1 presents uniformly dispersed nanoparticles.

[0056] like Figure 3a 、 Figure 3b From the LSV curve of the sample, it can be seen that compared with the nickel iron phosphate prepared in Control Example 1, the oxygen evolution (OER) performance of the nickel cobalt iron phosphate prepared in Example 1 is significantly improved, and the nickel cobalt iron phosphate has a smaller charge transfer resistance.

[0057] Based on the AEMWE polarization curve test results, at 60°C, the membrane electrode (nickel iron phosphate coated nickel felt) prepared in Control Example 1, as an AEMWE anode catalyst, has a potential of 1.96 V when the current density reaches 2 A / cm². The membrane electrode (nickel cobalt iron phosphate coated nickel felt) prepared in Example 1, as an AEMWE anode catalyst, exhibits higher catalytic activity, lower cell voltage, and smaller resistance. When the current density reaches 2 A / cm², its potential is 1.87 V; Figure 4 As shown; PO4 3- The strong coordination bond formed with the Ni / Fe metal center has a dual optimization effect: at the electronic level, the d-band electronic structure of the metal center is regulated by pd orbital hybridization, effectively reducing the adsorption energy barrier of the key OER intermediate (*OOH) and improving the intrinsic catalytic activity; at the structural level, the phosphate skeleton inhibits the migration and agglomeration of metal atoms through chemical bond anchoring, while forming an anti-corrosion protective layer to reduce the metal dissolution rate at high potential. In addition, the conductivity of the nickel-iron catalyst can be improved by introducing the transition metal cobalt into the nickel-iron-based catalyst. Therefore, the prepared amorphous nickel-cobalt-iron phosphate catalyst exhibits high intrinsic catalytic activity and AEM water electrolysis performance, and a 2A / cm 2 When the current density is 2.5V, the cell voltage is only 1.87V.

[0058] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing an amorphous nickel-cobalt-iron phosphate anode catalyst, characterized by: The following steps are involved: (1) dissolving a transition metal salt in a solvent and stirring to obtain a metal salt solution; (2) dissolving phosphate in a solvent and stirring to obtain a phosphate solution; (3) Adding the phosphate solution to the metal salt solution for reaction, washing with deionized water and ethanol, centrifuging, and drying to obtain an amorphous nickel cobalt iron phosphate anode catalyst.

2. The method for preparing an amorphous nickel-cobalt-iron phosphate anode catalyst according to claim 1, characterized in that: The transition metal salts include nickel salts, cobalt salts and iron salts; The total mass ratio of the iron salt to the nickel salt and the cobalt salt is 1:(10-2), wherein the molar ratio of the nickel salt to the cobalt salt is 1:1-1:3; The nickel salt is selected from one or more of nickel nitrate, nickel sulfate, nickel chloride, and nickel acetate; The cobalt salt is selected from one or more of cobalt nitrate, cobalt sulfate, cobalt chloride, and cobalt acetate; The iron salt is selected from one or more of ferric nitrate, ferric sulfate, ferric chloride and ferric acetate.

3. The method for preparing an amorphous nickel-cobalt-iron phosphate anode catalyst according to claim 1, characterized in that: The solvent is selected from one or more of deionized water, ethanol, ethylene glycol, and isopropanol; The phosphate is selected from one or more of trisodium phosphate, tripotassium phosphate, triammonium phosphate, and sodium hypophosphite.

4. The method for preparing an amorphous nickel-cobalt-iron phosphate anode catalyst according to claim 1, wherein: The phosphate solution is added to the metal salt solution for reaction, wherein the molar ratio of the phosphate to the metal salt is 1:1 to 1:

3.

5. The method for preparing an amorphous nickel-cobalt-iron phosphate anode catalyst according to claim 1, characterized in that: The reaction time is 1 to 3 hours; The drying temperature is 50-80°C.

6. Use of the amorphous nickel-cobalt-iron phosphate anode catalyst obtained by the preparation method according to any one of claims 1 to 5 in anion exchange membrane water electrolysis to produce hydrogen, characterized in that: The application comprises the following steps: grinding an amorphous nickel-cobalt-iron-phosphate anode catalyst, a ball milling medium, and a solvent, adding the ground amorphous nickel-cobalt-iron-phosphate slurry into a mixed solvent containing an ionomer, and performing ultrasonic dispersion to obtain an amorphous nickel-cobalt-iron-phosphate anode catalyst dispersion; A nickel felt substrate or an anion exchange membrane is placed on a heating plate for heating, and an amorphous nickel cobalt iron phosphate anode catalyst dispersion is sprayed on the nickel felt substrate or the anion exchange membrane to form a catalyst-coated substrate membrane electrode or a catalyst-coated membrane membrane electrode; the catalyst-coated substrate membrane electrode or the catalyst-coated membrane membrane electrode is hot-pressed to serve as the anode of an anion exchange membrane water electrolysis hydrogen production device.

7. The use according to claim 6, characterized in that: The grinding of the amorphous nickel-cobalt-iron phosphate anode catalyst, ball milling media and solvent comprises: using a four-stage series ball milling device, the rotation speed of each stage ball mill is 700-800 rpm, and the ball milling time of each stage is 4-6 minutes.

8. The use according to claim 6, characterized in that: The mass ratio of the amorphous nickel cobalt iron phosphate anode catalyst, ball milling beads, and solvent is 1:(30-50):(4-6); The mass ratio of the ionomer to the amorphous nickel cobalt iron phosphate anode catalyst in the amorphous nickel cobalt iron phosphate catalyst dispersion is 1:(3-5); The mixed solvent consists of isopropyl alcohol and water, and the volume ratio of water to isopropyl alcohol is 1:(1-3); the mass concentration of the amorphous nickel cobalt iron phosphate catalyst dispersion is 7.5-15 mg / mL.

9. The use according to claim 6, characterized in that: The nickel felt substrate or the anion exchange membrane is placed on a heating plate and heated at a temperature of 60-80°C.

10. The use according to claim 6, characterized in that: The amorphous nickel cobalt iron phosphate anode catalyst dispersion is sprayed on the nickel felt substrate or the anion exchange membrane at a spraying rate of 0.11 ml / time; The sprayed catalyst-coated substrate membrane electrode or catalyst-coated membrane electrode is hot-pressed at a temperature of 100-160° C., a time of 5-30 minutes, and a pressure of 50-100 kPa.

Citation Information

Cited By

  • Multi-metal phosphate solid solution catalyst as well as preparation method and application thereof

    CN120920033A

  • Preparation method of carbon-carbon composite fiber material

    CN121575584A

  • High-stability crystalline NiFePO4 catalyst, preparation method and application thereof, and AEM electrolytic bath

    CN121823517A

  • High-stability crystalline ni-fe-po4 catalyst, preparation method and application thereof, and aem electrolytic cell

    CN121823517B