Manufacturing method of double-sided micro-nano structure
By strictly designing nano-anti-reflection and micron light-trapping structures based on coupled wave theory, combining electron beam etching and ultra-precision machining, and using imprinting technology to prepare double-sided micro-nanostructures, the problems of high preparation cost, low efficiency and poor stability in existing technologies are solved, and the efficient and low-cost preparation of large-area double-sided micro-nanostructures and stability in extreme environments are achieved.
Patent Information
- Application Number
- CN202510719407.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-30
- Publication Date
- 2025-09-05
AI Technical Summary
Existing technologies make it difficult to efficiently and cost-effectively prepare large-area, mechanically strong, double-sided micro-nanostructures, and it is difficult to maintain stable performance in extreme environments.
The strict coupled wave theory is used to design nano-anti-reflection structures and micron light trapping structures. Combined with electron beam etching and ultra-precision machining, the imprinting process is used to achieve the integrated preparation of double-sided micro-nano structures.
It realizes a large-area double-sided micro-nano structure with low cost, high efficiency and good quality, which has high mechanical strength and stability in extreme environments and is suitable for space environment.
Smart Images

Figure CN120589678A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of metamaterial preparation, and in particular relates to a method for manufacturing a double-sided micro-nano structure. Background Art
[0002] Metamaterials are a class of artificial materials composed of subwavelength-scale artificial structural units. Their physical properties are determined by their structure rather than the constituent materials themselves. Early metamaterial research focused on microwave and radar bands, with typical applications including electromagnetic wave absorbers. These radar metamaterials typically utilize periodic structures to effectively manipulate electromagnetic waves, thereby exhibiting unnatural properties such as a negative refractive index and an electromagnetic band gap.
[0003] With the advancement of nanofabrication technology, researchers have gradually expanded the concept of metamaterials to higher-frequency optical bands, giving rise to the rise of optical metamaterials. Optical metamaterials generally refer to materials with micro- and nanoscale structures incorporated into their surfaces. These precisely designed structures can manipulate the propagation, polarization, phase, and amplitude of incident light, achieving ultra-high absorptivity and empowering satellite structures. Summary of the Invention
[0004] The present invention proposes a method for manufacturing a double-sided micro-nano structure, which absorbs visible light with a high absorption rate.
[0005] The technical solution to realize the present invention is: a method for manufacturing a double-sided micro-nanostructure, comprising the following steps:
[0006] Step 1: construct a double-sided micro-nano structure, which includes a nanometer anti-reflection structure as the front side and a micrometer light-trapping structure as the back side, and a substrate located between the two.
[0007] Step 2: Design of nano-anti-reflection structure:
[0008] Based on the rigorous coupled wave theory, a reflectivity analysis model of the nano-anti-reflection structure is established. According to the reflectivity analysis model of the nano-anti-reflection structure, the mapping relationship between the nano-anti-reflection structure form, characteristic parameters and reflectivity is constructed. Then, combined with the processing technology, the optimal characteristic parameters of the nano-anti-reflection structure are determined.
[0009] Step 3: Design the micron light trapping structure:
[0010] The energy characteristic distribution law of light after passing through the nano-anti-reflection structure is analyzed. The transmittance and transmission direction of each order of light passing through the nano-anti-reflection structure calculated by strict coupling theory are used as input. The light trapping ability of the micron light trapping structure is analyzed in combination with Fresnel's law and Snell's law. Driven by the goal of high absorption rate, the optimal characteristic parameters of the micron light trapping structure are determined, and the absorption rate of the entire double-sided micro-nano structure is calculated.
[0011] Step 4: Based on the optimal characteristic parameters of the nano-anti-reflection structure, an electron beam etching process is used to complete the processing of the nano-anti-reflection structure master.
[0012] Step 5: Based on the optimal characteristic parameters of the micron light trapping structure, the processing of the micron light trapping structure master is completed based on ultra-precision machining.
[0013] Step 6: Use the nano-anti-reflection structure master and the micron light trapping structure master to achieve the integrated manufacturing of double-sided micro-nano structures based on the imprinting process.
[0014] Compared with the prior art, the present invention has the following significant advantages:
[0015] (1) The double-sided micro-nanostructures fabricated using this method have obvious advantages such as low cost, high efficiency, and high quality. Compared with traditional methods, the double-sided micro-nanostructures fabricated using this method can save more than 300% in cost and improve efficiency by more than 200%.
[0016] (2) The double-sided micro-nanostructures produced by this method have high mechanical strength and strong resistance to extreme environments, and can function normally in a space environment. The double-sided micro-nanostructures produced by this method can serve in a space environment for many years.
[0017] (3) Ability to prepare large areas. The area of double-sided micro-nanostructures prepared by this method can be increased by more than 200% compared with traditional methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a flow chart of a double-sided micro-nanostructure manufacturing method of the present invention.
[0019] Figure 2 Schematic diagram of the double-sided micro-nano structure of the present invention.
[0020] Figure 3 Schematic diagram of the double-sided micro-nanostructure imprinting unit of the present invention. DETAILED DESCRIPTION
[0021] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The technical solutions between the various embodiments of the present invention can be combined with each other, but they must be based on the fact that ordinary technicians in this field can implement them. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0023] The following will further introduce the specific implementation methods, as well as the technical difficulties and inventive points of this invention in combination with this design example.
[0024] Combine Figures 1 to 3 The method for manufacturing a double-sided micro-nanostructure according to the present invention comprises the following steps:
[0025] Step 1: construct a double-sided micro-nano structure, which includes a nanometer anti-reflection structure as the front side and a micrometer light-trapping structure as the back side, and a substrate located between the two.
[0026] The nanometer anti-reflection structure is a lattice nano-cone structure, which achieves anti-reflection performance with a reflectivity of less than 0.3% in the visible light band.
[0027] The micron light trapping structure is a dot-matrix pyramid structure. The micron light trapping structure can realize multiple reflection and absorption of visible light, thereby increasing the absorption rate of visible light entering the entire double-sided micro-nano structure.
[0028] The substrate is used to support the nano-anti-reflection structure and the micron light-trapping structure, providing mechanical strength for the entire double-sided micro-nanostructure. Its thickness can be flexibly adjusted according to actual needs.
[0029] Go to step 2.
[0030] Step 2: Design of nano-anti-reflection structure:
[0031] Based on the rigorous coupled wave theory, a reflectivity analysis model of the nano-anti-reflection structure is established. According to the reflectivity analysis model of the nano-anti-reflection structure, the mapping relationship between the nano-anti-reflection structure form, characteristic parameters and reflectivity is constructed. Then, combined with the processing technology, the optimal characteristic parameters of the nano-anti-reflection structure are determined.
[0032] Step 21: Establish a reflectivity analysis model for the nano-anti-reflection structure based on the rigorous coupled wave theory, as follows:
[0033] The nano-anti-reflection structure is layered in the longitudinal direction, and the dielectric constant and electromagnetic field of the structural area are expanded into the form of Fourier series and introduced into the Maxwell equations to construct a set of differential equations. The scattering matrix of each layer is established by matching the boundary conditions between layers. On this basis, a global scattering matrix is constructed to establish the relationship between the incident electric field and the reflected electric field and the transmitted electric field, and the reflectivity and transmittance of each order are calculated.
[0034] Step 211: Dielectric constant ε of the nano-AR structure region r (x, y), the electromagnetic field is expanded into the Fourier series form:
[0035]
[0036] In the above formula, m and n correspond to the Fourier coefficients in the X and Y directions respectively; They correspond to the period of the structure in the X and Y directions respectively; a m,n is the Fourier series coefficient of the dielectric constant, S x (m,n;z) is the Fourier series coefficient of the electric field in the X direction, U x (m,n;z) is the Fourier series coefficient of the magnetic field in the X direction, and j is the imaginary part. x (x,y,z) is the electric field in the X direction, H x (x,y,z) is the magnetic field in the X direction, is the position vector, k x (m,n) is the X-direction wave vector of order m and n, k y (m,n) are the Y-direction wave vectors of order m and n, and (x,y,z) represent the coordinates of any point on the structure.
[0037] Step 212: Substitute the dielectric constant of the structural area and the Fourier series form of the electromagnetic field into Maxwell, and construct a global scattering matrix, and the relationship between the incident electric field and the reflected electric field and the transmitted electric field:
[0038]
[0039] In the above formula, c ref 、c trn are the modal coefficient vectors of the reflected electromagnetic field and the transmitted electromagnetic field, c inc is the modal coefficient vector of the incident electromagnetic field, S G is the global scattering matrix;
[0040] Step 213: Establish a reflectivity analysis model for the nano-anti-reflection structure based on the rigorous coupled wave theory to calculate the reflectivity and transmittance of each order:
[0041] According to the reflectivity analysis model of the nano anti-reflection structure established based on the strict coupled wave theory, it is calculated that the reflectivity of the nano anti-reflection structure is 0.2% to 0.3%, and the transmittance is 99.7% to 99.8%.
[0042] Step 22: Determine a characteristic parameter set of a nano-anti-reflection structure that meets the requirement of a reflectivity lower than 0.3%;
[0043] Step 23: In combination with existing processing technology, determine the optimal nano-anti-reflection structure form and optimal characteristic parameters, including period, aspect ratio and duty cycle.
[0044] The nanometer anti-reflection structure is a lattice nanocone structure with a period of 300-500nm, a height of 600-800nm and a duty cycle of 1; the micrometer light trapping structure is a lattice pyramid structure with the characteristics of a pyramid structure.
[0045] Preferably, the nano anti-reflection structure is a lattice nanocone structure with a period of 400 nm, a height of 600 nm, and a duty cycle of 1.
[0046] Go to step 3.
[0047] Step 3: Design the micron light trapping structure:
[0048] The energy characteristic distribution law of light after passing through the nano-anti-reflection structure is analyzed. The transmittance and transmission direction of each order of light passing through the nano-anti-reflection structure calculated by strict coupling theory are used as input. The light trapping ability of the micron light trapping structure is analyzed in combination with Fresnel's law and Snell's law. Driven by the goal of high absorption rate, the optimal characteristic parameters of the micron light trapping structure are determined, and the absorption rate of the entire double-sided micro-nano structure is calculated.
[0049] Step 31: Let the intensity of the incident light be P in , the transmittance of the nano-anti-reflection structure under any characteristic size is T, then the total intensity of light passing through the i-th nano-anti-reflection structure P i for:
[0050] P i =P in ×T (5)
[0051] Step 32: Let the efficiency of the qth stage transmission be ω i,q , then the intensity P of the qth level transmitted light of the i-th nano-anti-reflection structure is i,q for:
[0052] P i,q =ω i,q ×P i =ω i,q ×P in ×T (6)
[0053] Step 33: According to Fresnel's law, for TE polarized light and TM polarized light, the reflection coefficient and transmission coefficient are:
[0054]
[0055] In the above formula, r s is the reflection coefficient of TE polarized light, r p is the reflection coefficient of TM polarized light, t s is the transmission coefficient of TE polarized light, t p is the transmission coefficient of TM polarized light, n1 and n2 correspond to the refractive index of the first medium and the second medium, respectively, θ1 and θ2 correspond to the incident angle and the refraction angle, respectively.
[0056] Step 34: After passing through the nanometer anti-reflection structure, the intensity P of the reflected light after the qth level of transmitted light passes through the micrometer light trapping structure for the first time i,q,1 for:
[0057] P i,q,1 =P i,q ×|t s / p | 2 (11)
[0058] Among them, t s / p is the transmission coefficient of TE polarized light or TM polarized light.
[0059] Step 35: After passing through the nanometer anti-reflection structure, the intensity P of the reflected light after the qth level of transmitted light passes through the micrometer light trapping structure for the lth time i,q,l for:
[0060] P i,q,l =P i,q,l-1 ×|t s / p | 2 (12)
[0061] In the above formula, P i,q,l-1 is the intensity of the reflected light after the qth transmitted light passes through the nanometer anti-reflection structure and then passes through the micrometer light trapping structure for the l-1th time.
[0062] Step 36: For a cell, the intensity P after passing through the nano-anti-reflection structure and the micron light trapping structure is R for:
[0063]
[0064] Step 37: The absorption rate α of the root after micro-nano coupling is:
[0065]
[0066] The designed micron light trapping structure is a lattice pyramid structure. The characteristic dimensions of the pyramid structure are a bottom width of 300um, a height of 400um, a duty cycle of 1, and an absorption rate of 99.6% for the entire double-sided micro-nano structure.
[0067] Go to step 4.
[0068] Step 4: Based on the optimal characteristic parameters of the nano-AR structure, the nano-AR structure master is processed using an electron beam etching process. This double-sided micro-nanostructured nano-AR structure master is manufactured using an electron beam etching process. Its structure is a lattice-like nanocone with a period of 400nm, a height of 600nm, and a duty cycle of 1. It is made of silicon.
[0069] Go to step 5.
[0070] Step 5: Based on the optimal characteristic parameters of the micron light-trapping structure, the micron light-trapping structure master is fabricated using ultra-precision machining. This double-sided micron-nanostructured micron light-trapping structure master is manufactured using a fly-cut process. It features a lattice pyramid structure with a period of 300 μm, a height of 400 μm, and a duty cycle of 1. The material is polyimide.
[0071] The ultra-precision machining method of the micron light-trapping structure master is one of the following: electric spark wire cutting, diamond fly cutting, fast and slow tool servo, and mold molding.
[0072] Go to step 6.
[0073] Step 6: Use the nano-anti-reflection structure master and the micron light trapping structure master to achieve the integrated manufacturing of double-sided micro-nano structures based on the imprinting process.
[0074] Step 61: Perform anti-sticking treatment on the nano-anti-reflection structure master and the micron light trapping structure master respectively to protect the master in subsequent processes and extend their service life.
[0075] Step 62: Manufacturing an embossing concave mold: Both the nano-anti-reflection structure master and the micron light trapping structure master are convex structures. After anti-sticking treatment, the manufactured master is used to manufacture an embossing concave mold for subsequent embossing.
[0076] Furthermore, the material of the nano-anti-reflection structure mold and the micron light-trapping structure mold is one of polydimethylsiloxane and acrylate; when manufacturing the imprint mold, it is cured and formed based on a thermal curing process, the curing temperature is 80-130°C, and the curing time is 20-30 minutes.
[0077] Step 63: Anti-stick treatment is performed on the embossed die to allow successful demoulding after curing and to prevent damage to the structure during demoulding.
[0078] When performing anti-sticking treatment on the embossing die, first place the nano-anti-reflective structure die and the micron light-trapping structure die in a plasma treatment machine for 5-10 minutes to reduce the surface energy of the die; then soak the nano-anti-reflective structure die and the micron light-trapping structure die in anti-sticking liquid for 20-40 minutes.
[0079] Step 64: Heat the embossing adhesive to sufficiently reduce its viscosity to 50-100 cps so that bubbles can be smoothly discharged from the embossing adhesive during vacuuming.
[0080] The embossing adhesive is polyimide or FR4; the heating temperature is 80-100°C and the heating time is 5-10 minutes.
[0081] Step 65: Place the nano-anti-reflection structure concave mold and the micron light-trapping structure concave mold in a vacuum box for vacuum treatment, and then apply the embossing glue to the nano-anti-reflection structure concave mold and the micron light-trapping structure concave mold respectively, and eliminate the bubbles in the nano-anti-reflection structure concave mold, the micron light-trapping structure concave mold and the embossing glue to ensure that the entire double-sided micro-nano structure is free of bubble defects and has high mechanical strength.
[0082] The nanometer anti-reflection structure concave mold and the micrometer light trapping structure concave mold were placed in a vacuum box and evacuated to -1 MPa for 10 minutes at a time.
[0083] Step 66: Place the micron light trapping structure mold coated with embossing glue on the glass substrate, then add embossing glue until it is flush with the edge of the micron light trapping structure mold, cover it with the nano anti-reflection structure mold, and then cover the upper surface of the nano anti-reflection structure mold with another glass substrate to form a double-sided micro-nano structure embossing unit, as shown in FIG. Figure 3 shown.
[0084] Step 67: Place the double-sided micro-nanostructure imprinting unit in a pneumatic imprinting machine, apply pressure, and maintain the pressure for a period of time to fully fill and shape it.
[0085] Use air pressure equipment for embossing, with an embossing force of 0.2-1MPa and holding pressure for 2-5min.
[0086] Step 68: Take the double-sided micro-nanostructure imprinting unit out of the pneumatic imprinting machine, and place both sides of the double-sided micro-nanostructure imprinting unit under an ultraviolet lamp for irradiation and curing.
[0087] Place both sides of the double-sided micro-nanostructure imprinting unit under UV light for curing. The UV light intensity used for curing is 500-800mw / cm 2 The irradiation time is adjusted according to the thickness of the final double-sided micro-nanostructure product.
[0088] Step 69: Remove the glass substrates on both sides of the double-sided micro-nanostructure imprinting unit, and remove the nano-anti-reflection structure concave mold and the micron light trapping structure concave mold respectively to obtain the final double-sided micro-nanostructure product;
[0089] Step 610: Place the printed double-sided micro-nano structure product in a temperature-controlled box, cover the upper surface with a pressing plate, and adopt a segmented heating and heat preservation method to eliminate its internal stress, fully eliminate its residual stress, and prevent its warping and deformation. The segmented heating and heat preservation method is adopted to eliminate its internal stress, specifically as follows:
[0090] Keep warm at 80-90℃ for 4-6 hours, at 100-110℃ for 1-2 hours, at 120-130℃ for 1-2 hours, at 150-160℃ for 2-3 hours, at 170-180℃ for 2-3 hours, at 190-200℃ for 1-2 hours, and at 200-220℃ for 2-3 hours.
[0091] In summary, the present invention describes a method for manufacturing a double-sided micro-nanostructure, which can achieve high absorption rate in the visible light band in a space environment based on this double-sided micro-nanostructure, thereby enabling some structural components of the satellite and greatly improving the manufacturing efficiency of the satellite's ultra-black structural components. The double-sided micro-nanostructure is composed of three functional structural modules, including a nanoscale anti-reflection structure, a substrate, and a micron-scale light-trapping structure. The nanoscale anti-reflection structure is a lattice nanocone structure that can significantly reduce the interface reflectivity. The micron-scale light-trapping structure is a lattice pyramid structure that increases the absorption of light entering the double-sided micro-nanostructure through multiple reflections. The substrate provides attachment space for the nano-anti-reflection structure and the micron light-trapping structure, and provides mechanical strength to the entire double-sided micro-nanostructure. The double-sided micro-nanostructure is manufactured and formed in an integrated manner based on the imprinting process.
Claims
1. A method for manufacturing a double-sided micro-nano structure, characterized in that: The steps include: Step 1: constructing a double-sided micro-nanostructure, wherein the double-sided micro-nanostructure includes a nanometer anti-reflection structure as the front side and a micrometer light-trapping structure as the back side, and a substrate located between the two; Step 2: Design of nano-anti-reflection structure: A reflectivity analysis model for nano-anti-reflection structures is established based on rigorous coupled wave theory. Based on this model, a mapping relationship between the nano-anti-reflection structure form, characteristic parameters, and reflectivity is constructed. Combined with the processing technology, the optimal characteristic parameters of the nano-anti-reflection structure are determined. Step 3: Design the micron light trapping structure: The energy distribution of light after passing through the nano-anti-reflection structure is analyzed. The transmittance and transmission direction of each order of light passing through the nano-anti-reflection structure calculated by strict coupling theory are used as input. The light trapping ability of the micron light trapping structure is analyzed in combination with Fresnel's law and Snell's law. Driven by the goal of high absorptivity, the optimal characteristic parameters of the micron light trapping structure are determined, and the absorptivity of the entire double-sided micro-nanostructure is calculated. Step 4: Based on the optimal characteristic parameters of the nano-anti-reflection structure, an electron beam etching process is used to complete the processing of the nano-anti-reflection structure master; Step 5: Based on the optimal characteristic parameters of the micron light trapping structure, the micron light trapping structure master is processed by ultra-precision machining; Step 6: Use the nano-anti-reflection structure master and the micron light trapping structure master to achieve the integrated manufacturing of double-sided micro-nano structures based on the imprinting process.
2. The method for manufacturing a double-sided micro-nanostructure according to claim 1, wherein: In step 1, a double-sided micro-nano structure is constructed, wherein the double-sided micro-nano structure includes a nanometer anti-reflection structure as the front side and a micrometer light trapping structure as the back side, as follows: The nanometer anti-reflection structure is a lattice nano-cone structure, which achieves anti-reflection performance with a reflectivity of less than 0.3% in the visible light band. The micron light trapping structure is a dot-matrix pyramid structure. The micron light trapping structure can realize multiple reflection and absorption of visible light, thereby increasing the absorption rate of visible light entering the entire double-sided micro-nano structure. The substrate is used to support the nano-anti-reflection structure and the micron light-trapping structure, providing mechanical strength for the entire double-sided micro-nanostructure. Its thickness can be flexibly adjusted according to actual needs.
3. The method for manufacturing a double-sided micro-nanostructure according to claim 2, wherein: The nano-anti-reflection structure is a lattice nano-cone structure with a period of 300-500nm, a height of 600-800nm, and a duty cycle of 1; the micron light trapping structure is a lattice pyramid structure with characteristic dimensions of a bottom width of 200-300um, a height of 400-500um, and a duty cycle of 1.
4. The method for manufacturing a double-sided micro-nanostructure according to claim 1, wherein: In step 2, the nano anti-reflection structure is designed as follows: Step 21: Establish a reflectivity analysis model for the nano-anti-reflection structure based on rigorous coupled wave theory: The nano-anti-reflection structure is layered in the longitudinal direction, and the dielectric constant and electromagnetic field of the structural area are expanded into Fourier series form and introduced into the Maxwell equations to construct a differential equation system. The scattering matrix of each layer is established by matching the boundary conditions between layers. On this basis, a global scattering matrix is constructed to establish the relationship between the incident electric field and the reflected electric field and the transmitted electric field, and the reflectivity and transmittance of each order are calculated; Step 22: Determine a characteristic parameter set of a nano-anti-reflection structure that meets the requirement of a reflectivity lower than 0.3%; Step 23: In combination with existing processing technology, determine the optimal nano-anti-reflection structure form and optimal characteristic parameters, including period, aspect ratio and duty cycle.
5. The method for manufacturing a double-sided micro-nano structure according to claim 1, wherein: In step 21, a reflectivity analysis model of the nano-anti-reflection structure is established based on the rigorous coupled wave theory, as follows: Step 211: Dielectric constant ε of the nano-AR structure region r (x, y), the electromagnetic field is expanded into the Fourier series form: In the above formula, m and n correspond to the Fourier coefficients in the X and Y directions respectively; They correspond to the period of the structure in the X and Y directions respectively; a m,n is the Fourier series coefficient of the dielectric constant, S x (m,n;z) is the Fourier series coefficient of the electric field in the X direction, U x (m,n;z) is the Fourier series coefficient of the magnetic field in the X direction, j is the imaginary part; E x (x,y,z) is the electric field in the X direction, H x (x,y,z) is the magnetic field in the X direction, is the position vector, k x (m,n) is the X-direction wave vector of order m and n, k y (m,n) are the Y-direction wave vectors of order m and n, and (x,y,z) represent the coordinates of any point on the structure; Step 212: Substitute the dielectric constant of the structural area and the Fourier series form of the electromagnetic field into Maxwell, and construct a global scattering matrix, and the relationship between the incident electric field and the reflected electric field and the transmitted electric field: In the above formula, c ref 、c trn are the modal coefficient vectors of the reflected electromagnetic field and the transmitted electromagnetic field, c inc is the modal coefficient vector of the incident electromagnetic field, S G is the global scattering matrix; Step 213: Establish a reflectivity analysis model for the nano-anti-reflection structure based on the rigorous coupled wave theory to calculate the reflectivity and transmittance of each order: According to the reflectivity analysis model of the nano anti-reflection structure established based on the strict coupled wave theory, it is calculated that the reflectivity of the nano anti-reflection structure is 0.2% to 0.3%, and the transmittance is 99.7% to 99.8%.
6. The method for manufacturing a double-sided micro-nano structure according to claim 1, wherein: In step 3, the micron light trapping structure is designed as follows: Step 31: Let the intensity of the incident light be P in , the transmittance of the nano-anti-reflection structure under any characteristic size is T, then the total intensity of light passing through the i-th nano-anti-reflection structure P i for: P i =P in ×T(5) Step 32: Let the efficiency of the qth stage transmission be ω i,q , then the intensity P of the qth level transmitted light of the i-th nano-anti-reflection structure is i,q for: P i,q =ω i,q ×P i =ω i,q ×P in ×T(6) Step 33: According to Fresnel's law, for TE polarized light and TM polarized light, the reflection coefficient and transmission coefficient are: In the above formula, r s is the reflection coefficient of TE polarized light, r p is the reflection coefficient of TM polarized light, t s is the transmission coefficient of TE polarized light, t p is the transmission coefficient of TM polarized light, n1 and n2 correspond to the refractive index of the first medium and the second medium respectively, θ1 and θ2 correspond to the incident angle and the refraction angle respectively; Step 34: After passing through the nanometer anti-reflection structure, the intensity P of the reflected light after the qth level of transmitted light passes through the micrometer light trapping structure for the first time i,q,1 for: P i,q,1 =P i,q ×|t s / p | 2 (11) Among them, t s / p is the transmission coefficient of TE polarized light or TM polarized light; Step 35: After passing through the nanometer anti-reflection structure, the intensity P of the reflected light after the qth level of transmitted light passes through the micrometer light trapping structure for the lth time i,q,l for: P i,q,l =P i,q,l-1 ×|t s / p | 2 (12) In the above formula, P i,q,l-1 is the intensity of the reflected light after the qth transmitted light passes through the nanometer anti-reflection structure and the l-1th time passes through the micrometer light trapping structure; Step 36: For a cell, the intensity P after passing through the nano-anti-reflection structure and the micron light trapping structure is R for: Step 37: The absorption rate α of the root after micro-nano coupling is:
7. The method for manufacturing a double-sided micro-nano structure according to claim 1, wherein: In step 5, the ultra-precision machining method of the micron-trapped light structure master is one of electric spark wire cutting, diamond fly cutting, fast and slow tool servo, and mold molding.
8. The method for manufacturing a double-sided micro-nanostructure according to claim 1, wherein: In step 6, the nano-anti-reflection structure master and the micron light trapping structure master are used to realize the integrated manufacturing of the double-sided micro-nano structure based on the imprinting process, as follows: Step 61: performing anti-sticking treatment on the nano-anti-reflection structure master and the micron light trapping structure master respectively; Step 62: Manufacturing an embossing concave mold: Both the nano-anti-reflection structure master and the micron light trapping structure master have convex structures. After anti-sticking treatment, the manufactured master is used to manufacture an embossing concave mold for subsequent embossing. Step 63: performing anti-sticking treatment on the embossing die; Step 64: Heating the embossing adhesive to sufficiently reduce its viscosity to 50-100 cps; Step 65: Place the nano-AR structure concave mold and the micron light trapping structure concave mold in a vacuum chamber for vacuum treatment, then apply embossing adhesive to the nano-AR structure concave mold and the micron light trapping structure concave mold, respectively, and eliminate bubbles in the nano-AR structure concave mold, the micron light trapping structure concave mold, and the embossing adhesive; Step 66: Place the micron light-trapping structure mold coated with embossing adhesive on the glass substrate, then add embossing adhesive until it is flush with the edge of the micron light-trapping structure mold, cover it with the nano anti-reflection structure mold, and then cover the upper surface of the nano anti-reflection structure mold with another glass substrate to form a double-sided micro-nano structure embossing unit; Step 67: Place the double-sided micro-nanostructure imprinting unit in a pneumatic imprinting machine, apply pressure, and maintain the pressure for a period of time to fully fill and shape it; Step 68: Take the double-sided micro-nanostructure imprinting unit out of the pneumatic imprinting machine, and place both sides of the double-sided micro-nanostructure imprinting unit under a UV lamp for curing. Step 69: Remove the glass substrates on both sides of the double-sided micro-nanostructure imprinting unit, and remove the nano-anti-reflection structure concave mold and the micron light trapping structure concave mold respectively to obtain the final double-sided micro-nanostructure product; Step 610: Place the printed double-sided micro-nano structure product in a temperature-controlled box, cover the upper surface with a pressing plate, and adopt a segmented heating and heat preservation method to eliminate its internal stress and prevent its warping and deformation.
9. The method for manufacturing a double-sided micro-nanostructure according to claim 8, wherein: In step 62, the material of the nanometer anti-reflection structure concave mold and the micrometer light trapping structure concave mold is one of polydimethylsiloxane and acrylate; when manufacturing the imprint concave mold, it is cured and formed based on a thermal curing process, the curing temperature is 80-130° C., and the curing time is 20-30 minutes; In step 63, when performing anti-sticking treatment on the embossing die, the nanometer anti-reflection structure die and the micrometer light-trapping structure die are first placed in a plasma treatment machine for 5-10 minutes to reduce the surface energy of the die; then the nanometer anti-reflection structure die and the micrometer light-trapping structure die are immersed in anti-sticking liquid for 20-40 minutes; In step 64, the imprinting adhesive is polyimide or FR4; the heating temperature is 80-100° C., and the heating time is 5-10 minutes; In step 65, the nanometer anti-reflection structure concave mold and the micrometer light trapping structure concave mold are placed in a vacuum box and evacuated to -1 MPa for 10 minutes. In step 67, an air pressure device is used for embossing, with an embossing force of 0.2-1 MPa and a holding pressure of 2-5 minutes; In step 68, both sides of the double-sided micro-nanostructure imprinting unit are placed under a UV lamp for curing. The UV lamp used for curing has an intensity of 500-800 mw / cm 2 The irradiation time is adjusted according to the thickness of the final double-sided micro-nanostructure product.
10. The method for manufacturing a double-sided micro-nanostructure according to claim 8, wherein: In step 610, the internal stress is eliminated by heating and keeping warm in sections, as follows: Keep warm at 80-90℃ for 4-6 hours, at 100-110℃ for 1-2 hours, at 120-130℃ for 1-2 hours, at 150-160℃ for 2-3 hours, at 170-180℃ for 2-3 hours, at 190-200℃ for 1-2 hours, and at 200-220℃ for 2-3 hours.