Rolling treatment process for one-step forming of w-shaped hinge section steel
Through gas heating, pulse combustion control, descaling system and laminar cooling process, the problems of low efficiency and unstable quality in hinge steel production have been solved, and efficient and green manufacturing of W-shaped hinge steel has been achieved, which is suitable for building curtain walls, automobile manufacturing, civil defense doors and other fields.
Patent Information
- Application Number
- CN202510980364.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-16
- Publication Date
- 2025-09-12
AI Technical Summary
The existing hinge steel production process has problems such as low efficiency, low material utilization, high equipment cost, unstable product quality, and serious environmental pollution, which makes it difficult to meet the efficient and green manufacturing needs of modern industry.
The company adopts gas heating and pulse combustion control technology, combined with a high-pressure descaling system and a three-stage laminar cooling process. Through precision rolling and multi-roller straightening, the W-shaped hinge steel is formed in one step. Combined with high-precision sawing and quality inspection, product quality and production efficiency are ensured.
It realizes efficient production process, improves material utilization, reduces environmental pollution, ensures the dimensional accuracy and mechanical properties of the product, and is suitable for multiple industrial fields.
Smart Images

Figure CN120619047A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rolling processing technology, in particular to a rolling processing technology for one-step forming of W-shaped hinge steel. Background Art
[0002] In the field of modern industrial manufacturing, hinge steel is a key component of many equipment and facilities, and its demand is growing and its performance requirements are constantly improving. The main processes for traditional hinge steel production include forging, stamping and conventional hot rolling. Although the forging process can produce parts with various shapes, it is usually processed one by one, and the production speed is slow. Especially for hinge steel with complex shapes, the forging process is cumbersome and inefficient, and a large amount of scrap is generated, and the raw material utilization rate is low. Although the stamping process can achieve high production efficiency, for large or complex hinge steel, the mold cost of the stamping equipment is high, and the production flexibility is insufficient due to the limitation of the equipment tonnage. At the same time, the stamping process is prone to work hardening, which affects the subsequent processing and performance of the product. Although conventional hot rolling technology has certain advantages in the production of hinge steel, it still has many shortcomings. For example, the heating process often leads to local overheating or overcooling due to unreasonable combustion methods. The workpiece is prone to deformation and uneven performance due to temperature differences, affecting product quality consistency. The descaling effect is poor, and the residual oxide scale not only reduces the surface quality of the product, but may also cause rolling defects. It is difficult to accurately control the cooling speed in the cooling link, and the steel cools unevenly, which is prone to deformation, increased internal stress and other problems, which in turn affect the dimensional accuracy and mechanical properties of the product. In addition, the subsequent straightening, sawing, quality inspection, packaging and warehousing processes lack systematic optimization, the links between each link are not tight enough, and the overall process flow has poor coordination, resulting in the inability to maximize production efficiency and the need to improve product quality stability.
[0003] Existing technologies, whether forging, stamping, or conventional hot rolling, all have significant drawbacks. Forging is inefficient and results in significant waste of raw materials. Stamping is costly, inflexible, and prone to work hardening. Conventional hot rolling suffers from inaccurate control of key steps like heating, descaling, and cooling, making it difficult to ensure product quality stability and dimensional accuracy. Subsequent processes are often poorly connected, leading to poor overall process synergy. These issues have severely impacted the quality and production efficiency of hinge steel products, hindering their widespread application and performance improvement across various industries. The "one-step forming rolling process of W-shaped hinge steel" proposed in this plan has been comprehensively improved and optimized to address the above-mentioned defects. Summary of the Invention
[0004] The main purpose of the present invention is to provide a rolling process for forming W-shaped hinge steel in one step, which can effectively solve the problems in the background technology.
[0005] To achieve the above object, the technical solution adopted by the present invention is: A rolling process for forming a W-shaped hinge steel in one step, comprising: S1. Heating: Gas heating is used, the oxidizing atmosphere can be adjusted, it is weakly oxidizing, low-carbon burners are installed, and pulse combustion control technology is used. The burners are controlled by computer temperature control to make the burners work alternately in different areas of the furnace, and the heating temperature is controlled within the predetermined range; S2. Descaling: Two high-pressure descaling systems are continuously set up during the rough rolling and finishing rolling process to descaling the W-shaped hinge steel and remove the oxide scale; S3, rolling: the descaled W-shaped hinge steel billet is subjected to rough rolling and finish rolling in sequence, and the billet is gradually formed into a W-shaped hinge steel by designing rollers of different shapes; S4. Cooling: A three-stage laminar cooling process is adopted, including one stage cooling, two stage cooling and three stage cooling. The cooling speed of each stage is controlled by adjusting the water volume, water pressure and cooling zone length; S5. Straightening: The cooled W-shaped hinge steel is straightened by a multi-roller straightening machine. The straightening machine has 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness. S6. Sawing: After straightening, the steel section is cut to the specified length using high-precision sawing equipment with an accuracy of ±2mm. Cooling and lubrication are used during sawing. S7. Quality inspection: Carry out comprehensive quality inspection on the W-shaped hinge steel after sawing, including dimensional accuracy, surface quality, mechanical properties and internal structure inspection.
[0006] Preferably, in the heating step, the heating temperature is 1100-1200°C.
[0007] Preferably, the water pressure of the high-pressure descaling system is 15-20 MPa, the nozzles are arranged symmetrically, and form an angle of 45-60 degrees with the surface of the W-shaped hinge steel.
[0008] Preferably, in the rough rolling step, the roller profile of the rough rolling mill is designed to be a groove shape that matches the initial shape of the W-shaped hinge steel, and the roller material is an alloy steel with high hardness and high wear resistance.
[0009] Preferably, in the finishing rolling step, the roller profile design of the finishing mill matches the final shape of the W-shaped hinge steel, the roller diameter and roller body length of the roller are the same as the specifications and dimensions of the W-shaped hinge steel, and a rolling control system is used to control the speed, reduction and position of the roller.
[0010] Preferably, in the three-stage laminar cooling process, the cooling rate of the first stage is 10-15°C / s, the cooling rate of the second stage is 20-25°C / s, and the cooling rate of the third stage is 5-10°C / s.
[0011] Compared with the prior art, the present invention has the following beneficial effects: In the present invention, the one-time forming rolling processing process of the W-shaped hinge steel can realize an efficient production process. From heating, descaling, rolling to cooling, each process is closely connected and has a high degree of automation, which greatly shortens the production cycle, improves production efficiency, and meets the needs of large-scale production. At the same time, there are strict quality control measures in each key step, such as computer temperature control and pulse combustion technology in the heating process, high-pressure system and optimized parameters in the descaling process, precision equipment and precise control in the rolling stage, and three-stage laminar cooling process in the cooling link. These all ensure the dimensional accuracy, cross-sectional shape and surface quality of the product, so that the W-shaped hinge steel can accurately meet the assembly and use requirements in many fields such as building curtain walls, automobile manufacturing, and civil defense doors, reducing production delays and cost increases caused by quality problems.
[0012] The W-shaped hinge steel rolled by the designed process of the present invention has excellent mechanical properties. During the heating and rolling process, the billet is evenly heated and reasonably deformed, and then the precise control of the cooling process promotes the uniform transformation of the internal structure of the steel and refines the grains, thereby significantly improving the strength, toughness, elongation and other mechanical indicators of the steel, enabling it to withstand greater loads, impacts and vibrations, and adapt to complex working conditions such as frequent opening and closing. In addition, its good low-temperature impact performance also expands its application range. It can be used for hinge components of various equipment and facilities in different climatic conditions and extreme environments, such as building doors and windows in cold areas, cabinet doors of outdoor mechanical equipment, etc., providing solid performance support for the wide application of the product.
[0013] The pulse combustion control technology used in the heating process of this invention effectively reduces the emission of nitrogen oxides, which can reduce nitrogen oxide emissions by 30%-50% compared with traditional combustion methods, significantly reducing pollution to the atmospheric environment. The optimized design of the descaling process improves the descaling effect, reduces water resource consumption and wastewater discharge, and reduces production's dependence on water resources and the risk of water pollution. At the same time, the high efficiency and precision of the entire rolling process reduce the waste of raw materials, improve material utilization, and reduce energy consumption. It is in line with the concepts of green manufacturing and sustainable development in modern industry, helps companies reduce environmental pollution control costs and resource procurement costs, and enhances their social image and market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Schematic diagram of the heating and descaling process of the present invention; Figure 2 It is a schematic diagram of the rolling and cooling process of the present invention; Figure 3 Schematic diagram of the post-processing process of the present invention. DETAILED DESCRIPTION
[0015] In order to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the present invention is further described below in conjunction with specific implementation methods.
[0016] like Figure 1 As shown, a rolling process for forming a W-shaped hinge steel in one step includes: S1. Heating: Gas heating is used, the oxidizing atmosphere can be adjusted, it is weakly oxidizing, low-carbon burners are installed, and pulse combustion control technology is used. The burners are controlled by computer temperature control to make the burners work alternately in different areas of the furnace, and the heating temperature is controlled within the predetermined range; S2. Descaling: Two high-pressure descaling systems are continuously set up during the rough rolling and finishing rolling process to descaling the W-shaped hinge steel, remove the oxide scale and prevent secondary oxidation; S3, rolling: the descaled W-shaped hinge steel billet is subjected to rough rolling and finish rolling in sequence, and the billet is gradually formed into a W-shaped hinge steel by designing rollers of different shapes; S4. Cooling: A three-stage laminar cooling process is adopted, including one stage cooling, two stage cooling and three stage cooling. The cooling speed of each stage is controlled by adjusting the water volume, water pressure and cooling zone length to achieve a low turbulence and uniform coverage cooling effect; S5. Straightening: The cooled W-shaped hinge steel is straightened by a multi-roller straightening machine. The straightening machine has 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness.
[0017] S6. Sawing: After straightening, the steel section is cut to the specified length using high-precision sawing equipment with an accuracy of ±2mm. Cooling and lubrication are used during sawing. S7. Quality inspection: Carry out comprehensive quality inspection on the W-shaped hinge steel after sawing, including dimensional accuracy, surface quality, mechanical properties and internal structure inspection.
[0018] Furthermore, in the heating step, the heating temperature is 1100-1200°C, and the gas heating atmosphere is adjusted by precisely controlling the mixing ratio of gas and air and the combustion time to maintain weak oxidizing properties, ensuring that the surface oxidation degree of the W-shaped hinge steel billet is low during the heating process, which is beneficial to subsequent rolling and improvement of product performance.
[0019] Furthermore, the water pressure of the high-pressure descaling system is 15-20 MPa, the nozzle arrangement is symmetrical, and forms an angle of 45-60 degrees with the surface of the W-shaped hinge steel. By optimizing the nozzle spray angle and water flow distribution, the descaling effect is further improved and the water consumption and energy consumption during the descaling process are reduced.
[0020] Furthermore, in the rough rolling step, the roller profile of the rough rolling mill is designed to be a groove shape that matches the initial shape of the W-shaped hinge steel. The roller material is a high-hardness, high-wear-resistant alloy steel. The roller surface is specially treated to improve its wear resistance and impact resistance, ensuring that the W-shaped hinge steel can be uniformly deformed during the rough rolling process to form a good organizational structure and dimensional accuracy.
[0021] Furthermore, in the finishing rolling step, the roller profile of the finishing mill is designed with high mold precision to match the final shape of the W-shaped hinge steel. The roller diameter and roller body length of the roller are optimized according to the specifications and dimensions of the W-shaped hinge steel. At the same time, an advanced rolling control system is used to accurately control the speed, reduction amount and position of the roller to ensure that the dimensional tolerance of the W-shaped hinge steel after finishing rolling is controlled within an extremely small range, meeting the manufacturing requirements of high-precision products.
[0022] Furthermore, in the three-stage laminar cooling process, the cooling rate of the first stage is 10-15°C / s, the cooling rate of the second stage is 20-25°C / s, and the cooling rate of the third stage is 5-10°C / s. By precisely controlling the cooling rate of each stage, precise control of the cooling process of the W-shaped hinge steel is achieved, so that a suitable phase change occurs during the cooling process, a uniform organizational structure and good mechanical properties are obtained, and internal cracks and organizational defects in the steel caused by improper cooling rate are reduced.
[0023] Embodiment 1: This embodiment aims to achieve high-precision forming and surface quality optimization of W-shaped hinge steel for building curtain walls.
[0024] Specifically: This process is used to produce W-shaped hinge steel for building curtain walls. During heating, the heating temperature is precisely set to 1150°C. The mixture ratio of gas and air is strictly controlled to ensure that the oxidizing atmosphere is in an ideal weak oxidizing state. Low-carbon burners are equipped with pulse combustion control technology. The computer intelligently controls the burners to work alternately based on temperature feedback from different areas in the furnace, so that the W-shaped hinge steel billets are evenly heated, effectively reducing the risk of deformation caused by temperature differences. Nitrogen oxide emissions are reduced by 40% compared to traditional combustion methods. In the descaling process, the water pressure of the high-pressure descaling system is set to 18MPa, and the nozzles are arranged symmetrically and at a 50-degree angle to the billet surface. The optimized nozzle layout significantly improves the descaling effect and reduces water consumption by 15%. During the rolling stage, the roughing mill rolls are grooved to match the initial shape of the W-shaped hinge steel. They are made of high-hardness alloy steel and have a special surface treatment to improve their wear and impact resistance. The finishing mill rolls are designed with high mold precision to match the final shape of the W-shaped hinge steel. The roll diameter and roll length are optimized according to the specifications and dimensions of the W-shaped hinge steel. An advanced rolling control system is used to precisely control the roll speed, reduction, and position to ensure that the dimensional tolerance of the W-shaped hinge steel after finish rolling is kept within a very small range, meeting the manufacturing requirements of high-precision products. During cooling, a three-stage laminar cooling process is adopted, including one stage cooling, two stages cooling and three stages cooling. The cooling rate of each stage is controlled by adjusting the water volume, water pressure and cooling zone length to achieve a low turbulence and uniform coverage cooling effect, ensuring that the W-shaped hinge steel is cooled evenly, avoiding local overcooling or insufficient cooling, reducing steel deformation and internal stress, optimizing the phase change process of the steel, and ultimately obtaining good comprehensive mechanical properties; The cooled steel enters the straightening process and is straightened by a multi-roller straightening machine with 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness, avoid subsequent deformation problems, and improve the overall quality and performance stability of the product. After sawing, the steel is cut to a fixed length using high-precision sawing equipment. The sawing accuracy is controlled within ±2mm. Cooling and lubrication measures are used during the sawing process to reduce the impact of sawing heat on the ends of the W-shaped hinge steel, ensuring the quality and dimensional accuracy of the sawn surface, meeting the user's length requirements and subsequent processing needs of the product. In the quality inspection link, a comprehensive quality inspection is carried out on the sawed W-shaped hinge steel , including dimensional accuracy testing, surface quality testing, mechanical properties testing and internal structure testing, etc., using advanced testing equipment and technical means to ensure that product quality meets relevant standards and user requirements, and timely handle and feedback on unqualified products to ensure the quality stability and reliability of factory products. Finally, according to different user needs and transportation conditions, use appropriate packaging methods to package the qualified W-shaped hinge steel. The packaging material has moisture-proof, rust-proof and shock-proof functions to ensure that the quality of the product is not affected during transportation and storage. At the same time, the packaged products are marked and put into storage for easy traceability and deployment of products.
[0025] Embodiment 2: This embodiment is to achieve both lightweight and high strength of W-shaped hinge steel for automobile manufacturing.
[0026] Specifically: This process is used to produce thin-walled W-shaped hinge steel required in the automotive manufacturing field. The heating temperature is controlled at 1100℃. Through precise gas-air ratio adjustment and combustion time control, a weak oxidizing atmosphere is maintained. The low-carbon burner and pulse combustion control technology work together. The computer monitors the temperature distribution in the furnace in real time and optimizes the burner working sequence to ensure uniform heating of the billet and reduce the slight deformation of the material caused by thermal stress. At the same time, nitrogen oxide emissions are reduced by 35%. In the descaling process, the water pressure is set to 15MPa. The nozzle is designed with a special angle of 45 degrees to the billet surface. The high-pressure water flow effectively removes the oxide scale. The optimized descaling system improves descaling efficiency by 20%, laying a good foundation for subsequent precision cutting. During the rolling stage, the roughing mill rolls are grooved to match the initial shape of the W-shaped hinge steel. They are made of high-hardness, high-wear-resistant alloy steel, and their surfaces are finely ground to improve their wear and impact resistance. The finishing mill rolls are designed with high-precision dies that match the final shape of the W-shaped hinge steel. The roll diameter and length are optimized based on the specifications of thin-walled W-shaped hinge steel in the automotive field. An advanced rolling control system is used to precisely control the roll speed, reduction, and position, ensuring that the dimensional tolerance of the W-shaped hinge steel after finish rolling is kept within a very small range, meeting the manufacturing requirements of high-precision products. During the cooling process, a three-stage laminar cooling process is used. By adjusting the water volume, water pressure, and cooling zone length to control the cooling rate, low turbulence and uniform coverage are achieved. This ensures uniform cooling of the W-shaped hinge steel, avoids local overcooling or insufficient cooling, reduces steel deformation and internal stress, optimizes the steel's phase transformation process, and ultimately achieves good comprehensive mechanical properties. The cooled steel enters the straightening process and is straightened by a multi-roller straightening machine with 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness, avoid subsequent deformation problems, and improve the overall quality and performance stability of the product. After sawing, the steel is cut to a fixed length using high-precision sawing equipment. The sawing accuracy is controlled within ±2mm. Cooling and lubrication measures are used during the sawing process to reduce the impact of sawing heat on the ends of the W-shaped hinge steel, ensuring the quality and dimensional accuracy of the sawn surface, meeting the user's length requirements and subsequent processing needs of the product. In the quality inspection link, a comprehensive quality inspection is carried out on the sawed W-shaped hinge steel , including dimensional accuracy testing, surface quality testing, mechanical properties testing and internal structure testing, etc., using advanced testing equipment and technical means to ensure that product quality meets relevant standards and user requirements, and timely handle and feedback on unqualified products to ensure the quality stability and reliability of factory products. Finally, according to different user needs and transportation conditions, use appropriate packaging methods to package the qualified W-shaped hinge steel. The packaging material has moisture-proof, rust-proof and shock-proof functions to ensure that the quality of the product is not affected during transportation and storage. At the same time, the packaged products are marked and put into storage for easy traceability and deployment of products.
[0027] Example 3: This example aims to achieve high load-bearing capacity and impact resistance of W-shaped hinge steel for civil air defense doors.
[0028] Specifically: This process is used to manufacture heavy W-shaped hinge steel for civil air defense doors. The heating temperature is raised to 1200°C, and the gas heating power is enhanced to ensure that the heavy billets are fully heated. The oxidizing atmosphere adjustment system accurately maintains a weak oxidation state. The low-carbon burners and pulse combustion control technology work efficiently together. The computer intelligently controls the burners to operate crosswise in the furnace, eliminating local temperature differences and reducing nitrogen oxide emissions by 45%, providing uniform billets for subsequent rolling of heavy steel. In the descaling process, the water pressure is increased to 20MPa, and the nozzle is at a 60-degree angle to the billet surface. The high-pressure water flow has a strong impact to completely remove the thick oxide scale. The optimized descaling system improves the descaling effect by 25%, preventing the residual oxide scale from affecting subsequent rolling. During the rolling stage, the roughing mill rolls have wide grooves that match the initial shape of the W-shaped hinge steel. The special alloy steel rolls have a surface hardness of HRC62, making them resistant to wear. The finishing mill rolls have a diameter and length that are precisely customized to the heavy specifications of the civil air defense door hinge steel. The advanced rolling control system controls the roll speed, reduction, and position within a very small range, ensuring that the steel dimensional accuracy reaches ±0.5mm and the cross-sectional shape is regular, meeting the high-strength requirements of civil air defense doors. During the cooling process, a three-stage laminar cooling process is used. By adjusting the water volume, water pressure, and cooling zone length to control the cooling rate, low turbulence and uniform coverage are achieved. This ensures uniform cooling of the W-shaped hinge steel, avoids local overcooling or insufficient cooling, reduces steel deformation and internal stress, optimizes the steel's phase transformation process, and ultimately achieves good comprehensive mechanical properties. The cooled steel enters the straightening process and is straightened by a multi-roller straightening machine with 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness, avoid subsequent deformation problems, and improve the overall quality and performance stability of the product. After sawing, the steel is cut to a fixed length using high-precision sawing equipment. The sawing accuracy is controlled within ±2mm. Cooling and lubrication measures are used during the sawing process to reduce the impact of sawing heat on the ends of the W-shaped hinge steel, ensuring the quality and dimensional accuracy of the sawn surface, meeting the user's length requirements and subsequent processing needs of the product. In the quality inspection link, a comprehensive quality inspection is carried out on the sawed W-shaped hinge steel, including dimensional accuracy detection. , surface quality inspection, mechanical property inspection and internal organization inspection, etc., using advanced testing equipment and technical means to ensure that product quality meets relevant standards and user requirements, and timely handle and feedback on unqualified products to ensure the quality stability and reliability of products leaving the factory. Finally, according to different user needs and transportation conditions, use appropriate packaging methods to package the qualified W-shaped hinge steel. The packaging material has moisture-proof, rust-proof and shock-proof functions to ensure that the quality of the product is not affected during transportation and storage. At the same time, the packaged products are marked and put into storage for easy traceability and deployment of products, thereby improving the company's production management level and user satisfaction.
[0029] Embodiment 4: This embodiment aims to achieve high-precision assembly and durability of W-shaped hinge steel for cabinet doors of industrial machinery and equipment.
[0030] Specifically: This process is used to produce medium-sized W-shaped hinged steel for industrial machinery cabinet doors. The heating temperature is set at 1130°C. Through high-precision gas-air ratio adjustment and combustion control procedures, a stable weak oxidizing atmosphere is maintained. The low-carbon burner and pulse combustion control technology work efficiently together. The computer monitors and optimizes the burner working status in real time, ensuring uniform heating of the billet, reducing thermal stress and reducing nitrogen oxide emissions by 38%. During the descaling process, the water pressure is stabilized at 17MPa. The nozzle adopts an optimized spiral arrangement, forming a 55-degree angle with the billet surface. The multi-angle water flow impact improves the descaling efficiency by 18%, providing clean billets for subsequent rolling. During the rolling stage, the roughing mill rolls are designed with a grooved shape that matches the initial shape of the W-shaped hinge steel. They are made of high-hardness alloy steel and have a finely ground surface to improve their wear and impact resistance. The finishing mill rolls are designed with high-precision molds that match the final shape of the W-shaped hinge steel. The roll diameter and roll length are optimized according to the specifications of the W-shaped hinge steel for industrial cabinet doors. At the same time, an advanced rolling control system is used to precisely control the roll speed, reduction, and position to ensure that the dimensional tolerance of the W-shaped hinge steel after finish rolling is controlled within a very small range, meeting the manufacturing requirements of high-precision products. During the cooling process, a three-stage laminar cooling process is used. By adjusting the water volume, water pressure, and cooling zone length to control the cooling rate, low turbulence and uniform coverage are achieved. This ensures uniform cooling of the W-shaped hinge steel, avoids local overcooling or insufficient cooling, reduces steel deformation and internal stress, optimizes the steel's phase transformation process, and ultimately achieves good comprehensive mechanical properties. The cooled steel enters the straightening process and is straightened by a multi-roller straightening machine with 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness, avoid subsequent deformation problems, and improve the overall quality and performance stability of the product. After sawing, the steel is cut to a fixed length using high-precision sawing equipment. The sawing accuracy is controlled within ±2mm. Cooling and lubrication measures are used during the sawing process to reduce the impact of sawing heat on the ends of the W-shaped hinge steel, ensuring the quality and dimensional accuracy of the sawn surface, meeting the user's length requirements and subsequent processing needs of the product. In the quality inspection link, a comprehensive quality inspection is carried out on the sawed W-shaped hinge steel , including dimensional accuracy testing, surface quality testing, mechanical properties testing and internal structure testing, etc., using advanced testing equipment and technical means to ensure that product quality meets relevant standards and user requirements, and timely handle and feedback on unqualified products to ensure the quality stability and reliability of factory products. Finally, according to different user needs and transportation conditions, use appropriate packaging methods to package the qualified W-shaped hinge steel. The packaging material has moisture-proof, rust-proof and shock-proof functions to ensure that the quality of the product is not affected during transportation and storage. At the same time, the packaged products are marked and put into storage for easy traceability and deployment of products.
[0031] Example 5: This example aims to achieve the purpose of achieving corrosion resistance and high impact resistance of W-shaped hinge steel for ship hatches.
[0032] Specifically: This process is used to manufacture corrosion-resistant W-shaped hinge steel for ship hatches. The heating temperature is controlled at 1180°C. A stable, weakly oxidizing atmosphere is maintained through high-precision gas-air ratio adjustment and combustion control procedures. The low-carbon burner and pulse combustion control technology work efficiently together. The computer monitors and optimizes the working status of the burner in real time, ensuring uniform heating of the billet, reducing thermal stress and reducing nitrogen oxide emissions by 42%. In the descaling process, the water pressure is set to 19MPa, and the nozzle uses a special wide-width nozzle, forming a 52-degree angle with the billet surface. The high-pressure water flow fully covers the billet, improving the descaling effect by 22%, removing thick oxide scale and providing a clean surface for subsequent rolling. During the rolling stage, the roughing mill rolls are designed with wide, shallow grooves based on the initial shape of the W-shaped hinge steel for ships. The alloy steel rolls have a surface hardness of HRC60, making them wear-resistant and impact-resistant. The finishing mill rolls have a diameter and length precisely tailored to the corrosion resistance and mechanical requirements of the ship hatch hinge steel. The advanced rolling control system precisely controls the roll speed, reduction, and position within an extremely small range, ensuring a dimensional accuracy of ±0.4mm and a cross-sectional shape that is highly consistent with the design blueprint. During the cooling process, a three-stage laminar cooling process is used. By adjusting the water volume, water pressure, and cooling zone length to control the cooling rate, low turbulence and uniform coverage are achieved. This ensures uniform cooling of the W-shaped hinge steel, avoids local overcooling or insufficient cooling, reduces steel deformation and internal stress, optimizes the steel's phase transformation process, and ultimately achieves good comprehensive mechanical properties. The cooled steel enters the straightening process and is straightened by a multi-roller straightening machine with 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness, avoid subsequent deformation problems, and improve the overall quality and performance stability of the product. After sawing, the steel is cut to a fixed length using high-precision sawing equipment. The sawing accuracy is controlled within ±2mm. Cooling and lubrication measures are used during the sawing process to reduce the impact of sawing heat on the ends of the W-shaped hinge steel, ensuring the quality and dimensional accuracy of the sawn surface, meeting the user's length requirements and subsequent processing needs of the product. In the quality inspection link, a comprehensive quality inspection is carried out on the sawed W-shaped hinge steel , including dimensional accuracy testing, surface quality testing, mechanical properties testing and internal structure testing, etc., using advanced testing equipment and technical means to ensure that product quality meets relevant standards and user requirements, and timely handle and feedback on unqualified products to ensure the quality stability and reliability of factory products. Finally, according to different user needs and transportation conditions, use appropriate packaging methods to package the qualified W-shaped hinge steel. The packaging material has moisture-proof, rust-proof and shock-proof functions to ensure that the quality of the product is not affected during transportation and storage. At the same time, the packaged products are marked and put into storage for easy traceability and deployment of products.
[0033] Each of the above five embodiments starts from a different application field, makes targeted adjustments to the process parameters according to the product characteristics, and elaborates on the specific operations and effects of each step in detail. The connection between the previous and the next is tight and the logic is clear, which fully reflects the wide applicability and operability of this process.
[0034] The basic principles, main features, and advantages of the present invention are shown and described above. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are merely illustrative of the principles of the present invention. Various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention. Such changes and modifications are intended to fall within the scope of the present invention. The scope of protection claimed in the present invention is defined by the appended claims and their equivalents.
Claims
1. A rolling process for forming a W-shaped hinge steel in one step, characterized in that: include: S1. Heating: Gas heating is used, the oxidizing atmosphere can be adjusted, it is weakly oxidizing, low-carbon burners are installed, and pulse combustion control technology is used. The burners are controlled by computer temperature control to make the burners work alternately in different areas of the furnace, and the heating temperature is controlled within the predetermined range; S2. Descaling: Two high-pressure descaling systems are continuously set up during the rough rolling and finishing rolling process to descaling the W-shaped hinge steel and remove the oxide scale; S3, rolling: the descaled W-shaped hinge steel billet is subjected to rough rolling and finish rolling in sequence, and the billet is gradually formed into a W-shaped hinge steel by designing rollers of different shapes; S4. Cooling: A three-stage laminar cooling process is adopted, including one stage cooling, two stage cooling and three stage cooling. The cooling speed of each stage is controlled by adjusting the water volume, water pressure and cooling zone length; S5. Straightening: The cooled W-shaped hinge steel is straightened by a multi-roller straightening machine. The straightening machine has 5-7 rollers. The straightening pressure and speed are adjusted according to the specifications and materials of the W-shaped hinge steel to ensure straightness. S6. Sawing: After straightening, the steel section is cut to the specified length using high-precision sawing equipment with an accuracy of ±2mm. Cooling and lubrication are used during sawing. S7. Quality inspection: Carry out comprehensive quality inspection on the W-shaped hinge steel after sawing, including dimensional accuracy, surface quality, mechanical properties and internal structure inspection.
2. The one-step forming rolling process of the W-shaped hinge steel according to claim 1 is characterized in that: In the heating step, the heating temperature is 1100-1200°C.
3. The one-step forming rolling process of the W-shaped hinge steel according to claim 1 is characterized in that: The water pressure of the high-pressure descaling system is 15-20 MPa, and the nozzles are arranged symmetrically and at an angle of 45-60 degrees to the surface of the W-shaped hinge steel.
4. The one-step forming rolling process of the W-shaped hinge steel according to claim 1 is characterized in that: In the rough rolling step, the roll profile of the rough rolling mill is designed to be a groove shape that matches the initial shape of the W-shaped hinge steel.
5. The one-step forming rolling process of the W-shaped hinge steel according to claim 1 is characterized in that: In the finishing rolling step, the roller profile design of the finishing mill matches the final shape of the W-shaped hinge steel, the roller diameter and roller body length of the roller are the same as the specifications and dimensions of the W-shaped hinge steel, and a rolling control system is used to control the speed, reduction and position of the roller.
6. The one-step forming rolling process of the W-shaped hinge steel according to claim 1 is characterized in that: In the three-stage laminar cooling process, the cooling rate of the first stage is 10-15°C / s, the cooling rate of the second stage is 20-25°C / s, and the cooling rate of the third stage is 5-10°C / s.
Citation Information
Cited By
Manufacturing method of hinge connecting piece of vehicle door hinge
CN120886013A
Water consumption accounting method in steel plate rolling process