Fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment
The composite coating composed of nano-ceramic pre-dispersion and microcapsule dry powder solves the problems of high energy consumption, insufficient coating durability and poor construction compatibility in the anti-icing technology of wind power and power grid equipment. It achieves the precise release of fluorosilicone oil and improved durability of the coating, and is suitable for the anti-icing of wind power and power grid equipment.
Patent Information
- Application Number
- CN202511119541.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-11
- Publication Date
- 2025-09-26
AI Technical Summary
Existing anti-icing technologies for wind power and power grid equipment have problems such as high energy consumption, insufficient coating durability, and poor construction compatibility. In particular, the release of fluorosilicone oil in coastal wind farms with high humidity and high salt fog is uncontrollable, leading to rapid accumulation of ice.
A composite coating composed of nano-ceramic pre-dispersion and microcapsule dry powder, including a thermal expansion layer and a stress-sensitive layer, is used. A fluorosilicone oil microcapsule coating is formed through electrostatic spraying and photothermal gradient curing, combined with plasma activation treatment to ensure coating adhesion and durability.
The precise release of fluorosilicone oil at low temperatures is achieved. The coating is highly durable in extreme environments, meeting the lifelong maintenance-free requirements of high-voltage insulators. The adhesion of ice is reduced, the coating has strong bonding strength, and the construction process is controllable.
Smart Images

Figure BDA0005542471640000071 
Figure BDA0005542471640000081 
Figure BDA0005542471640000082
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of anti-icing of wind power and power grid equipment, and more particularly to a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment. Background Art
[0002] Current anti-icing technologies for wind turbines and power grid equipment rely primarily on three types of solutions: Thermal deicing technology: This uses resistance heating or hot air to melt ice, but it consumes extremely high amounts of energy, accounting for 15-30% of wind turbine power generation, and cannot cope with extreme freezing rain.
[0003] Chemical coating technology: Mainstream silicone coatings such as PDMS can reduce ice adhesion strength to 50-100kPa, but fluorosilicone oil will quickly lose its hardness and cannot withstand wind and sand abrasion;
[0004] Microcapsule technology: CN113234364A uses paraffin microcapsules to passively release oil, but the low-temperature response is slow and the mechanical strength of the wall material is insufficient.
[0005] Especially in coastal wind farms with high humidity and high salt fog, existing coatings generally have three major defects:
[0006] Fluorosilicone oil release is uncontrollable: Temperature-triggered microcapsules release with lag in the "freezing rain critical zone" between -5 and 0°C, leading to rapid accumulation of ice.
[0007] Insufficient industrial durability: Power grid insulators need to withstand more than 1,000 thermal shock cycles, while traditional fluorocarbon coatings will crack and peel after 200 hot and cold cycles;
[0008] Poor construction compatibility: The curved surface structure of wind turbine blades requires a single-pass coating, but high-solid slurry spraying is prone to clogging the gun, forcing the use of brush coating, resulting in uneven film thickness. Therefore, the present invention provides a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment. Summary of the Invention
[0009] In order to overcome the above-mentioned defects of the prior art, the present invention provides a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment to solve the problems existing in the above-mentioned background technology.
[0010] The present invention provides the following technical solution: a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment, comprising the following independently packaged components:
[0011] Component A - nano-ceramic pre-dispersion: 20-30 parts of methyltrimethoxysilane, 5-8 parts of tetraethoxysilane, 40-60 parts of isopropyl alcohol, and 10-15 parts of silica nanoparticles grafted with perfluoroalkyl groups;
[0012] Component B - microcapsule powder: 25-40 parts of mesoporous alumina microcapsules filled with fluorosilicone oil, 1-4 parts of amino-modified carbon nanotubes, and 2-5 parts of oxygen vacancy defect titanium dioxide photocatalyst;
[0013] The composite wall material is composed of a thermal expansion layer and a stress-sensitive layer from the inside to the outside. The thermal expansion layer is poly (N-vinyl caprolactam) with a thickness of 0.5-1 μm. The stress-sensitive layer is porous alumina with a pore size of 20-100 nm and a porosity of 60-80%. The surface is covered with a polydopamine elastic layer with a thickness of 50-100 nm.
[0014] Furthermore, the fluorosilicone oil contains trifluoropropyl and phenyl modified groups, has a molecular weight of 2000-5000 g / mol, an oxygen vacancy concentration of oxygen vacancy titanium dioxide is ≥1018 cm-3, and the mixing mass ratio of component A to component B is 1:1.
[0015] A construction method for a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment comprises the following steps:
[0016] S1. Substrate treatment: Use white corundum sand to sandblast wind power and power grid equipment, with a sandblasting pressure of 0.6±0.05MPa, to ensure that there is no visual residue on the surface of the equipment, and the roughness is ≤60μm. Immediately after sandblasting, use dry, clean compressed air (pressure 0.4-0.6MPa) to blow the surface for ≥30 seconds to completely remove residual dust. At this time, perform online plasma activation treatment: use an atmospheric pressure plasma jet device or corona discharge device with argon as the working gas to scan the substrate surface after sandblasting and blowing under normal pressure. During the treatment, the spray gun / electrode head is 10-30mm away from the substrate surface, and the moving speed is kept uniform to ensure that the treatment area is fully covered and not missed. The plasma treatment time is controlled within 5-8 minutes. The goal is to significantly increase the surface energy of the substrate to ≥60mN / m to enhance the adhesion of the coating;
[0017] S2. Component pretreatment: Component A was first frozen at -20°C for 24 h and then thawed to room temperature. The carbon nanotubes in component B were vacuum-infused with fluorosilicone oil and then ball-milled with liquid nitrogen to a particle size of ≤45 μm.
[0018] S3 mixing and dispersion: A and B components were mixed in a ratio of 1:1; ultrasonically coupled mechanical stirring was performed at 2500 rpm / 15 min until a slurry was obtained after mixing, ensuring that the slurry viscosity was 150 mPa·s;
[0019] S4. Directional coating: The mixed slurry is sprayed onto wind power and power grid equipment using an electrostatic spraying method with an alternating magnetic field superimposed on the surface, forming a single-pass film with a wet film thickness of 100±10μm.
[0020] S5. Gradient curing: Use near-infrared light to irradiate the spray film of the equipment until the temperature of the coating on the equipment surface is ≥80℃. At this time, perform hot air curing at 110℃-130℃ for 20-40 minutes. At this time, ensure that the coating on the surface of the equipment does not peel off when peeled off with tape, which means that the coating has been cured. At this time, UV irradiation is required for 0-8 minutes to complete the curing.
[0021] Furthermore, after the surface of S1 is polished by sandblasting equipment, compressed air is used to blow the surface for 30 seconds, and the mixed slurry must be completed within 120 minutes. The overdue slurry is discarded after UV curing.
[0022] Furthermore, the online plasma activation treatment of S1 is an atmospheric pressure plasma jet device or a corona discharge device using argon as the working gas, and the surface of the substrate after sandblasting is scanned under normal pressure. The direction of the alternating magnetic field is perpendicular to the substrate surface, and the magnetic induction intensity is optimally 30-60mt, and the carbon tube fluorosilicone oil loading rate is 30-50wt%.
[0023] Technical effects and advantages of the present invention:
[0024] 1. The volume expansion rate of the composite wall material of the thermal expansion layer and the stress-sensitive layer of the present invention at low temperatures triggers the microcapsules to release fluorosilicone oil. At the same time, when ice pressure exists, the polydopamine-coated alumina layer undergoes elastic deformation, synergistically releasing fluorosilicone oil to form a dual-mode anti-icing mechanism.
[0025] 2. The present invention innovates the independent encapsulation of AB components + gradient curing process, breaks the nano-agglomeration by freezing and depolymerizing component A, and stores component B as dry powder, which makes the microcapsules have a long shelf life and are durable in extreme environments. The coating has strong bonding strength, meeting the lifelong maintenance-free requirements of high-voltage insulators.
[0026] 3. The present invention uses electromagnetic-assisted directional spraying and photothermal gradient curing, precise arrangement of microcapsules, and electrostatic atomization superimposed on a vertical magnetic field to achieve a high degree of orientation of the long axis of the microcapsules perpendicular to the substrate, and shorten the oil release path. At the same time, through zero-defect film formation, near-infrared light is used to selectively heat the microcapsules, and then 110℃-130℃ hot air curing and UV curing are used to greatly improve the stability of the equipment coating. DETAILED DESCRIPTION
[0027] The technical solutions in the present invention will be described clearly and completely below. In addition, the forms of the various structures described in the following embodiments are merely examples. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] The present invention provides a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment, comprising the following independently packaged components:
[0029] Component A - nano-ceramic pre-dispersion: 20-30 parts of methyltrimethoxysilane, 5-8 parts of tetraethoxysilane, 40-60 parts of isopropyl alcohol, and 10-15 parts of silica nanoparticles grafted with perfluoroalkyl groups;
[0030] Component B - microcapsule powder: 25-40 parts of mesoporous alumina microcapsules filled with fluorosilicone oil, 1-4 parts of amino-modified carbon nanotubes, and 2-5 parts of oxygen vacancy defect titanium dioxide photocatalyst;
[0031] The composite wall material is composed of a thermal expansion layer and a stress-sensitive layer from the inside to the outside. The thermal expansion layer is poly (N-vinyl caprolactam) with a thickness of 0.5-1 μm. The stress-sensitive layer is porous alumina with a pore size of 20-100 nm and a porosity of 60-80%. The surface is covered with a polydopamine elastic layer with a thickness of 50-100 nm.
[0032] The fluorosilicone oil contains trifluoropropyl and phenyl modified groups, has a molecular weight of 2000-5000 g / mol, an oxygen vacancy concentration of oxygen vacancy titanium dioxide is ≥1018 cm-3, and the mixing mass ratio of component A to component B is 1:1.
[0033] A construction method for a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment comprises the following steps:
[0034] S1. Substrate treatment: Use white corundum sand to sandblast wind power and power grid equipment, with a sandblasting pressure of 0.6±0.05MPa, to ensure that there is no visual residue on the surface of the equipment, and the roughness is ≤60μm. Immediately after sandblasting, use dry, clean compressed air (pressure 0.4-0.6MPa) to blow the surface for ≥30 seconds to completely remove residual dust. At this time, perform online plasma activation treatment: use an atmospheric pressure plasma jet device or corona discharge device with argon as the working gas to scan the substrate surface after sandblasting and blowing under normal pressure. During the treatment, the spray gun / electrode head is 10-30mm away from the substrate surface, and the moving speed is kept uniform to ensure that the treatment area is fully covered and not missed. The plasma treatment time is controlled within 5-8 minutes, and the goal is to significantly increase the surface energy of the substrate to ≥60mN / m to enhance the adhesion of the coating;
[0035] S2. Component pretreatment: Component A was first frozen at -20°C for 24 hours and then thawed to room temperature. The carbon nanotubes in component B were vacuum-injected with fluorosilicone oil and ball-milled with liquid nitrogen to a particle size of ≤45 μm. The amino-modified carbon nanotubes were placed in a vacuum tank and set to -0.1 MPa. At this time, fluorosilicone oil containing phenyl or trifluoropropyl groups with a molecular weight of 3500 g / mol was injected. The mixture was incubated at 60°C for 2 hours and the excess oil was removed by centrifugation to ensure that its loading rate was controlled at 45 wt%;
[0036] S3 mixing and dispersion: A and B components were mixed in a ratio of 1:1; ultrasonically coupled mechanical stirring was performed at 2500 rpm / 15 min until a slurry was obtained after mixing, ensuring that the slurry viscosity was 150 mPa·s;
[0037] S4. Directional coating: The mixed slurry is sprayed onto wind power and power grid equipment using an electrostatic spraying method with an alternating magnetic field superimposed on the surface, forming a single-pass film with a wet film thickness of 100±10μm.
[0038] S5. Gradient curing: Use near-infrared light to irradiate the spray film of the equipment until the temperature of the coating on the equipment surface is ≥80℃. At this time, perform hot air curing at 110℃-130℃ for 20-40 minutes. At this time, ensure that the coating on the surface of the equipment does not peel off when peeled off with tape, which means that the coating has been cured. At this time, UV irradiation is required for 0-8 minutes to complete the curing.
[0039] Among them, after the surface of S1 is polished by sandblasting equipment, compressed air is used to blow the surface for 30 seconds, and the mixed slurry must be completed within 120 minutes. The overdue slurry is discarded after UV curing.
[0040] Among them, the online plasma activation treatment of S1 is an atmospheric pressure plasma jet device or corona discharge device using argon as the working gas, which scans the surface of the substrate after sandblasting under normal pressure. The direction of the alternating magnetic field is perpendicular to the substrate surface, and the magnetic induction intensity is optimally 30-60mt, and the carbon tube fluorosilicone oil loading rate is 30-50wt%.
[0041] In order to verify the effect of microcapsule wall material thickness on oil release efficiency in the present invention, the following experiment was set up:
[0042] Experiment 1: Simulating a 15cm ice layer at -5℃ + 0.3MPa ice pressure. The detection method uses high-speed video recording of oil release response time and fluorescence quantitative analysis:
[0043] Control group 1: The thickness of the thermal expansion layer was set to 0.3 μm, the thickness of the stress sensitive layer was set to 0.2 μm, and the fluorosilicone oil loading rate was set to 60%;
[0044] Control group 2: The thickness of the thermal expansion layer was set to 0.5 μm, the thickness of the stress sensitive layer was set to 0.3 μm, and the fluorosilicone oil loading rate was set to 60%;
[0045] Control group 3: The thickness of the thermal expansion layer was set to 1.2 μm, the thickness of the stress sensitive layer was set to 0.7 μm, and the fluorosilicone oil loading rate was set to 60%;
[0046] Experimental group: The thickness of the thermal expansion layer was set to 0.8 μm, the thickness of the stress sensitive layer was set to 0.5 μm, and the fluorosilicone oil loading rate was set to 60%.
[0047] The following results were obtained through experiments:
[0048] Group Oil release delay time (s) 5-year oil release residual rate Microcapsule breakage rate Control group 1 18 38% 12.5% Control group 2 25 52% 5.8% Control group 3 42 75% 0.3% Experimental group 28 68% 0.4%
[0049] From the above content, it can be seen that the wall thickness of 0.5-1μm specified in claim 1 is the optimal wall thickness. At the same time, the oil release delay time is within 30s, and the microcapsule breakage rate is only 0.4% after 1000 times of -40℃-80℃ thermal shock, so that the oil release will not be too fast, resulting in loss of fluorosilicone oil and shortening the service life.
[0050] In order to verify the effect of carbon nanotube fluorosilicone oil loading rate on secondary oil release in the present invention, the following experiment was set up:
[0051] Experiment 2: The test indicators are the amount of fluorosilicone oil leakage per unit pressure of carbon nanotubes and the residual rate of the carbon nanotube lumen cross-sectional area after 500 hours of salt spray. The detection is carried out using a microfluidic chip and high-speed photography:
[0052] Control group 1: The carbon tube fluorosilicone oil loading rate was set to 30wt% and the ice pressure trigger value was set to 50kPa;
[0053] Control group 2: The carbon tube fluorosilicone oil loading rate was set to 40wt% and the ice pressure trigger value was set to 50kPa;
[0054] Control group 3: The carbon tube fluorosilicone oil loading rate was set to 50wt% and the ice pressure trigger value was set to 50kPa;
[0055] Experimental group: The carbon tube fluorosilicone oil loading rate was set to 45wt% and the ice pressure trigger value was set to 50kPa.
[0056] The following results were obtained through experiments:
[0057]
[0058] In summary, it can be seen that when loading fluorosilicone oil into carbon tubes, the loading rate of 45wt% is the optimal value. At the same time, the oil supply is still high after 25 years, and the clogging rate is lower than that of the control group 3. That is, the method adopted by the experimental group can effectively supply oil while reducing the clogging rate.
[0059] In order to verify the effect of UV irradiation time on the self-cleaning effect of the present invention, the following experiment was set up:
[0060] Experiment 3: The test indicators are the water contact angle after pollutant attachment and the open rate of carbon nanotubes after UV treatment at a wavelength of 365nm. The detection methods include contact angle measurement, scanning electron microscopy, and fluorosilicone oil photodegradation detection.
[0061] Control group 1: UV irradiation duration was set to 0 min, and the pollutants were diesel smoke and sea salt as the pollutant sources;
[0062] Control group 2: UV irradiation duration was set to 2 minutes, and the pollutants were diesel smoke and sea salt as the pollutant sources;
[0063] Control group 3: UV irradiation duration was set to 8 minutes, and the pollutants were diesel smoke and sea salt as the pollutant sources;
[0064] Experimental group: UV irradiation duration was set to 3 minutes, and the pollutants were diesel smoke and sea salt as the pollutant sources:
[0065] The following results were obtained through experiments:
[0066]
[0067] In summary, it can be concluded that 3 minutes of UV irradiation is the optimal time, which makes it easier for blocked carbon tubes to recover, thereby reducing the blockage of external pollutants, and is not likely to cause titanium oxide to decay due to excessive UV irradiation, and will not cause a large amount of photolysis of fluorosilicone oil.
[0068] In order to verify the effect of the aging of the mixed slurry of the present invention on the coating performance, the following experiments were set up:
[0069] Experiment 4: The substrate is a wind turbine blade with a curvature radius of 2m. The test index is to compare the exposed proportion of microcapsules under different wet film thicknesses:
[0070] Control group 1: wet film thickness 80 μm;
[0071] Control group 2: wet film thickness 110 μm;
[0072] Control group 2: wet film thickness 150 μm;
[0073] Experimental group: wet film thickness 100 μm.
[0074] The following results were obtained through experiments:
[0075]
[0076] In summary, it can be seen that 100μm is enough to achieve good results, but the improvement is limited when it exceeds 100μm.
[0077] In order to verify the effect of the alternating magnetic field intensity on the orientation degree of the microcapsules of the present invention, the following experiment was set up:
[0078] Experiment 5: The test indicators are the ratio of the angle between the long axis of the microcapsule and the normal line of the substrate ≤ 10° and the peeling force of a 5mm ice layer at -10°C. The test is carried out by using SEM statistical angle sampling:
[0079] Control group 1: The magnetic field intensity was set to 30 mT, and the direction deviation angle was ≤ 5°;
[0080] Control group 2: The magnetic field intensity was set to 40 mT, and the direction deviation angle was ≤5°;
[0081] Control group 3: The magnetic field intensity was set to 60 mT, and the direction deviation angle was ≤ 5°;
[0082] Experimental group: The magnetic field intensity was set to 50 mT, and the direction deviation angle was ≤5°.
[0083] Group Perpendicular orientation rate Ice adhesion strength (kPa) Microcapsule rupture rate Control group 1 63% 14.2 1.8% Control group 2 75% 10.5 1.2% Control group 3 83% 9.2 5.7% Experimental group 87% 8.7 0.4%
[0084] In summary, it can be seen that 50mT is the optimal magnetic field strength, which greatly reduces the ice adhesion strength. At the same time, the microcapsule rupture rate is also greatly reduced by subjecting the coating to 500 freeze-thaw cycles in a water bath from -40℃ to 60℃ to simulate 25 years of use in a natural environment.
[0085] The present invention realizes that when wind power and power grid equipment encounter freezing rain, the ice layer grows and generates ice pressure, causing the polydopamine-coated aluminum oxide in the stress-sensitive layer to undergo elastic deformation and reduce the pore size. At the same time, due to the decrease in temperature, the thermal expansion layer also shrinks, and then squeezes the inside. Through the cooperation of the thermal expansion layer and the stress-sensitive layer, the fluorosilicone oil seeps out from the inside of the microcapsule and spreads on the coating surface to form an oleophobic layer. When the ice pressure disappears, the carbon tube recovers elastically, causing the tube cavity to generate negative pressure, which partially absorbs the unconsumed fluorosilicone oil on the surface. The oil is replenished to the microcapsule cavity through the carbon tube-microcapsule interface channel to maintain the oil storage capacity.
[0086] When annual maintenance is required, UV irradiation is used to activate oxygen vacancy titanium dioxide on the surface of the equipment to generate active oxygen free radicals to degrade organic pollutants. The decomposed pollutants are peeled off from the surface, and fluorosilicone oil is re-spread. The released fluorosilicone oil fills the micro-cracks in the alumina wall material to achieve self-repair.
[0087] Finally, a few points should be explained: First, in the description of this application, it should be noted that, unless otherwise specified or limited, the terms "mounted," "connected," and "connected" should be understood in a broad sense, and may refer to mechanical or electrical connections, internal communication between two components, or direct connection. "Up," "down," "left," and "right" are only used to indicate relative positional relationships. When the absolute positions of the objects being described change, the relative positional relationships may also change.
[0088] Secondly: Regarding the structures involved in the embodiments of the present disclosure, other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other;
[0089] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment, characterized by: It consists of the following individually packaged components: Component A - nano-ceramic pre-dispersion: 20-30 parts of methyltrimethoxysilane, 5-8 parts of tetraethoxysilane, 40-60 parts of isopropyl alcohol, and 10-15 parts of silica nanoparticles grafted with perfluoroalkyl groups; Component B - microcapsule powder: 25-40 parts of mesoporous alumina microcapsules filled with fluorosilicone oil, 1-4 parts of amino-modified carbon nanotubes, and 2-5 parts of oxygen vacancy defect titanium dioxide photocatalyst; The composite wall material is composed of a thermal expansion layer and a stress-sensitive layer from the inside to the outside. The thermal expansion layer is poly (N-vinyl caprolactam) with a thickness of 0.5-1 μm. The stress-sensitive layer is porous alumina with a pore size of 20-100 nm and a porosity of 60-80%. The surface is covered with a polydopamine elastic layer with a thickness of 50-100 nm.
2. The fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment according to claim 1, characterized in that: The fluorosilicone oil contains trifluoropropyl and phenyl modified groups, has a molecular weight of 2000-5000 g / mol, and the oxygen vacancy concentration of the oxygen vacancy titanium dioxide is ≥10 18 cm -3 The amino density of amino-modified carbon nanotubes is ≥3.2 / nm 2 The mixing mass ratio of component A to component B is 1:10.8-1:1.
5.
3. A construction method for a fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment, characterized by: The following steps are included: S1. Substrate treatment: Use white corundum sand to sandblast wind power and power grid equipment at a sandblasting pressure of 0.6±0.05MPa. Ensure that there is no visual residue on the surface of the equipment and the roughness is ≤60μm. Immediately after sandblasting, use dry, clean compressed air (pressure 0.4-0.6MPa) to blow the surface for ≥30 seconds to completely remove residual dust. At this time, perform online plasma activation treatment. During treatment, the spray gun / electrode head is 10-30mm away from the substrate surface, and the moving speed is kept uniform to ensure that the treatment area is fully covered and not missed. The plasma treatment time is controlled within 5-8 minutes. The goal is to significantly increase the surface energy of the substrate to ≥60mN / m to enhance the adhesion of the coating. S2. Component pretreatment: Component A was first frozen at -20°C for 24 h and then thawed to room temperature. The carbon nanotubes in component B were vacuum-infused with fluorosilicone oil and then ball-milled with liquid nitrogen to a particle size of ≤45 μm. S3 mixing and dispersion: A and B components were mixed in a ratio of 1:1; ultrasonically coupled mechanical stirring was performed at 2500 rpm / 15 min until a slurry was obtained after mixing, ensuring that the slurry viscosity was 150 mPa·s; S4. Directional coating: The mixed slurry is sprayed onto wind power and power grid equipment through electrostatic spraying and superimposing an alternating magnetic field, forming a single-pass film on the surface to complete the equipment coating spraying operation; S5. Gradient curing: Use near-infrared light to irradiate the spray film of the equipment until the temperature of the coating on the equipment surface is ≥80℃. At this time, perform hot air curing at 110℃-130℃ for 20-40min. At this time, ensure that the coating on the surface of the equipment does not peel off when peeled off with tape, which means that the coating has been cured. At this time, UV irradiation is required for 0-8min to activate the titanium dioxide photocatalyst, and complete curing is completed.
4. The fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment according to claim 1, characterized in that: After the surface of S1 is polished by sandblasting equipment, compressed air is used to blow the surface for 30 seconds. The mixed slurry must be completed within 120 minutes. The overdue slurry is discarded after UV curing.
5. The fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment according to claim 1, characterized in that: The online plasma activation treatment in S1 is to use an atmospheric pressure plasma jet device or a corona discharge device using argon as a working gas to perform a scanning treatment on the surface of the substrate after sandblasting and purging under a normal pressure environment.
6. The fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment according to claim 1, characterized in that: The alternating magnetic field is perpendicular to the surface of the substrate, and the magnetic induction intensity is 30-60 mt.
7. The fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment according to claim 1, characterized in that: In the S4, the surface is film-formed in a single pass, and the thickness of the formed wet film is 100±10 μm.
8. The fluorosilicone oil microcapsule anti-icing coating for wind power and power grid equipment according to claim 1, characterized in that: The carbon tube fluorosilicone oil loading rate is 30-50 wt %.
Citation Information
Patent Citations
Pure broad-spectrum radiation refrigeration coating and preparation method and coating layer structure thereof
CN113234364A
Cited By
Epoxy resin / organic silicon composite insulating material with tracking resistance and preparation method of epoxy resin / organic silicon composite insulating material
CN122060287A
Fan blade low-ice-adhesion super-hydrophobic ice-hydrophobic functional layer and preparation method thereof
CN122146163A