Sunlight and thermal radiation multi-adjustment intelligent window and preparation method and application thereof
Through the stacked structure of smart windows, combined with electric field and temperature stimulation, multiple controls of sunlight and thermal radiation are achieved, solving the problems of narrow control band and slow response speed of existing smart windows, achieving high efficiency and energy saving effects, and adapting to various climate zones.
Patent Information
- Application Number
- CN202510886273.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-30
- Publication Date
- 2025-10-28
Smart Images

Figure CN120848062A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of building energy-saving smart window technology, specifically to a smart window with multiple modes of adjustment for sunlight and thermal radiation, its preparation method, and its application. Background Technology
[0002] With the continued growth of global energy consumption, building energy conservation has become an important direction for solving energy problems. Windows, as the primary means of heat exchange between buildings and the external environment, directly affect building energy consumption. However, traditional windows can lead to increased indoor temperatures and cooling loads in summer, and heat loss and increased heating demands in winter, thus increasing building energy consumption. Therefore, developing intelligent windows that can dynamically adjust sunlight and heat radiation is of great significance for achieving building energy conservation.
[0003] Currently, smart window technologies mainly include thermochromic, electrochromic, photochromic, and mechanical color-changing types. Existing smart window technologies generally suffer from the following problems: First, existing technologies mostly focus on optical modulation in a single wavelength band (such as visible light or near-infrared), failing to simultaneously cover the entire wavelength band of sunlight (200-2500nm) and mid-to-far-infrared thermal radiation (8-13μm), resulting in low energy management efficiency; second, response speed and stability are insufficient. For example, the response time of humidity-responsive and thermochromic materials generally exceeds one minute, exhibiting poor cycle stability, easy aging, and significant performance degradation after long-term use; third, high cost and complex manufacturing processes make large-scale application difficult.
[0004] Radiative cooling is a passive cooling technology based on the principle of thermal radiation. It boasts advantages such as energy saving, environmental friendliness, high efficiency, and rapid cooling, and has broad application prospects in various fields. Its core principle is to selectively emit infrared radiation in a specific wavelength band (the atmospheric window band of 8-13 micrometers) to directly transfer heat from an object to outer space near absolute zero (3K), thus achieving highly efficient heat dissipation without external energy input. The key to the radiative cooling process lies in the emissivity of the material surface, i.e., the object's ability to radiate heat outward. Materials with high emissivity (approaching 1) can maximize the conversion of thermal energy into radiative energy. Especially within the target wavelength band, high emissivity designs can overcome the atmospheric absorption barrier for infrared radiation, significantly improving cooling efficiency. Low emissivity materials (approaching 0) are particularly effective in applications requiring heat preservation, insulation, or reduction of thermal signals due to their ability to significantly suppress the loss of thermal radiation energy.
[0005] In building cooling, radiative cooling based on the principle of thermal radiation has shown great application potential. By applying radiative cooling materials or devices to building roofs or exterior walls, infrared radiation can be effectively emitted into the sky, thereby transferring heat away. Therefore, developing a smart window capable of multiple adjustments to sunlight and thermal radiation to achieve building energy conservation is of great significance. Summary of the Invention
[0006] This application provides a smart window with multiple modes of solar radiation and thermal radiation, its preparation method, and its application, aiming to solve the technical problems of existing smart windows, such as narrow control band, slow response speed, and poor energy-saving effect.
[0007] To achieve the above objectives, the present application adopts the following technical solution.
[0008] In a first aspect, this application provides a smart window that allows for multiple adjustments of sunlight and thermal radiation, comprising an outer surface layer, a middle layer, and an inner surface layer stacked sequentially.
[0009] The outer surface layer includes an infrared transparent layer, and an infrared reflective layer and a vanadium dioxide doped layer respectively disposed on two opposite surfaces of the infrared transparent layer;
[0010] The inner surface layer includes a transparent substrate and a conductive layer attached to one side surface of the transparent substrate;
[0011] The intermediate layer is a liquid crystal / polymer dimming layer, with one side of the liquid crystal / polymer dimming layer bonded to the infrared reflective layer and the other side bonded to the conductive layer.
[0012] Preferably, the liquid crystal / polymer dimming layer includes any one of polymer-dispersed liquid crystal, polymer-stabilized liquid crystal, or polymer-dispersed and stabilized liquid crystal.
[0013] Preferably, the transmittance of the liquid crystal / polymer dimming layer can be switched by electric field stimulation;
[0014] Its driving voltage is 5-100V, visible light transmittance change is ≥40%, and response time is ≤1s.
[0015] More preferably, the polymer-dispersed liquid crystal comprises, by mass percentage: liquid crystal phase A 50-80 wt%, polymerizable monomer A 15-48.5 wt%, spacer particles 0.5-2 wt%, and photoinitiator 1 wt%.
[0016] Wherein, the liquid crystal phase A is a room temperature nematic liquid crystal or a mixture thereof; the polymerizable monomer A is a photocurable low-shrinkage monomer;
[0017] and / or,
[0018] The polymer-stabilized liquid crystal comprises, by weight percentage: liquid crystal phase B 68.5–95.5 wt%, polymerizable monomer B 2–30 wt%, spacer particles 0.5–2 wt%, and photoinitiator 1 wt%.
[0019] and / or,
[0020] The polymer-dispersed and stabilized liquid crystal comprises, by mass percentage: liquid crystal phase B 50-80 wt%, polymerizable monomer A 14-40 wt%, polymerizable monomer B 2-10 wt%, spacer particles 0.5-2 wt%, and photoinitiator 0.5-3 wt%.
[0021] Wherein, the liquid crystal phase B includes at least one of cholesteric liquid crystal, inverted liquid crystal, or smectic-cholesteric phase transition liquid crystal, and the polymerizable monomer B is a polymerizable monomer with optical anisotropy.
[0022] More preferably, the polymerizable monomer A includes at least one of trimethylolpropane triacrylate, HDDA, BDDA, PEGDA, IBOA, BMA, Bis-EMA, isocyanate-modified polyurethane-acrylate, or epoxy acrylate.
[0023] The polymerizable monomer B includes any one of 1,4-bis[4-(6-acryloyloxyhexyloxy)phenyl]octanoate (C6M), 1,4-bis[4-(3-acryloyloxypropoxy)phenyl]octanoate (C3M) or 4-(4-acryloyloxybutoxy)vinyl benzoate (C4V);
[0024] The initiator includes any one of Irgacure 1173, Irgacure 184, Irgacure 651, Irgacure 819 or TPO-L;
[0025] The spacer particles include any one of silica microspheres, organopolystyrene microspheres, or surface-modified nanocellulose.
[0026] Preferably, the visible light transmittance of the outer surface layer is ≥50%;
[0027] The infrared transparent layer is a polypropylene film or a polyethylene film; the infrared transmittance of the infrared transparent layer is ≥80%;
[0028] The infrared reflective layer is made of at least one of indium tin oxide, silver nanowires, copper, gold, or graphene.
[0029] Preferably, the doping material of the vanadium dioxide layer includes at least one of tungsten, molybdenum, niobium, or fluorine;
[0030] The doping concentration of the vanadium dioxide layer is 1–5 at%, and the phase transition temperature range is 10–45 °C.
[0031] and / or,
[0032] The transparent substrate is made of at least one of glass, polypropylene, polyethylene, polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polyvinyl chloride, or transparent nylon.
[0033] and / or,
[0034] The conductive layer is made of at least one of indium tin oxide, silver nanowires, graphene, silver, gold, or copper, and the visible light transmittance of the conductive layer is ≥85%.
[0035] A second aspect of this application provides a method for preparing the aforementioned smart window, comprising:
[0036] An infrared reflective layer and a vanadium dioxide-doped layer are deposited on two opposite surfaces of the infrared transparent layer to obtain the outer surface layer.
[0037] A conductive layer is deposited on one surface of a transparent substrate to obtain an inner surface layer;
[0038] A prepolymer is obtained by mixing liquid crystal mixture, polymerizable monomer, initiator and spacer particles. The prepolymer is then extruded between the infrared reflective layer of the outer surface layer and the conductive layer of the inner surface layer through a roll-to-roll process. The prepolymer is then cured by photopolymerization or thermal polymerization to obtain a smart window.
[0039] A third aspect of this application provides the application of the aforementioned intelligent window with multiple modes of solar and thermal radiation adjustment in building windows, vehicle windows, or photovoltaic modules.
[0040] A fourth aspect of this application provides an intelligent temperature control system, which includes the aforementioned intelligent window with multiple adjustments for sunlight and thermal radiation.
[0041] Compared with the prior art, the beneficial effects of this application are as follows:
[0042] The intelligent window of this application can achieve multiple coordinated regulation of sunlight and thermal radiation, with a wide regulation band, fast response speed, and good energy-saving effect. Its regulation band covers the visible light, near-infrared and mid-far-infrared range, and can reversibly change with the ambient temperature. At low temperatures, it presents a transparent, low-emission heat-preserving state, while at high temperatures, it presents a scattering, high-emission heat-dissipating state; it can achieve energy saving all year round and all weather, and is suitable for various climate regions.
[0043] The intelligent window of this application has a light transmission adjustable layer response time of ≤1 second under electric field response; and a light transmittance adjustable response time of ≤10 seconds under temperature stimulation, with a vanadium dioxide doped phase transition response of ≤10 seconds; it can respond quickly to changes in the external environment.
[0044] The smart window of this application exhibits highly efficient energy-saving performance. At high temperatures, it cools the room by using high emissivity and low transmittance, refracting and reflecting most sunlight while absorbing a small portion, significantly reducing heat entering the room and increasing heat loss to the outside; this lowers the indoor temperature and saves energy consumption in the cooling system. At low temperatures, it displays low emissivity and high transmittance, absorbing most sunlight entering the room while reflecting a small portion, reducing heat loss from the interior to the outside, maintaining indoor lighting and temperature, and reducing energy consumption in the heating system. Simulation tests show that compared to ordinary glass, the smart window of this application can reduce indoor temperature by 8-15℃ in summer and improve insulation efficiency by 15-25% in winter.
[0045] Furthermore, this application employs a roll-to-roll process to prepare the liquid crystal layer, resulting in high production efficiency and material utilization.
[0046] It has low production costs and is suitable for large-scale production. Attached Figure Description
[0047] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0048] Figure 1 This is a schematic diagram of the intelligent window for multiple adjustments of sunlight and thermal radiation in this application.
[0049] Figure 2 Microscopic morphology of the infrared reflective layer on the outer surface of the smart window;
[0050] Figure 3 Microscopic morphology of the vanadium dioxide doped layer on the outer surface of the smart window;
[0051] Figure 4 The graph shows the light transmittance test results of the smart window in Example 1 in the transparent and scattering states;
[0052] Figure 5 The emissivity curve of the smart window in Example 1 in the 8-14μm range is shown.
[0053] Figure 6 The graph shows the light transmittance test results of the smart window in Example 2 in the transparent state (low temperature 25°C) and the scattering state (high temperature 50°C);
[0054] Figure 7 This is a cross-sectional topographic view of the intermediate layer PD&SLC of the smart window in Example 3. Detailed Implementation
[0055] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.
[0056] In the following description of this embodiment, the terms "including", "comprising", "having", and "containing" are all open-ended terms, meaning that they include but are not limited to.
[0057] In the following description of this embodiment, the term "and / or" is used to describe the association relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, B existing alone, and A and B existing simultaneously. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.
[0058] In the following description of this embodiment, the term "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0059] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms "a" and "the" as used in the embodiments of this application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.
[0060] Those skilled in the art should understand that, in the following description of the embodiments of this application, the sequence of numbers does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.
[0061] Those skilled in the art will understand that the numerical ranges in the embodiments of this application should be understood as each intermediate value between the upper and lower limits of the specifically disclosed range. Each smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this application. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0062] Unless otherwise stated, the technical / scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains. While this application describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this application. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0063] Firstly, this application provides a smart window with multiple modes for adjusting sunlight and thermal radiation, the structure of which is as follows: Figure 1 As shown, it includes an outer surface layer, a middle layer, and an inner surface layer stacked in sequence;
[0064] The outer surface layer includes an infrared transparent layer, and an infrared reflective layer and a vanadium dioxide doped layer respectively disposed on two opposite surfaces of the infrared transparent layer; wherein, the vanadium dioxide doped layer is a vanadium dioxide nanoparticle layer;
[0065] The inner surface layer includes a transparent substrate and a conductive layer attached to one side surface of the transparent substrate;
[0066] The intermediate layer is a liquid crystal / polymer dimming layer, with one side of the liquid crystal / polymer dimming layer bonded to the infrared reflective layer and the other side bonded to the conductive layer.
[0067] In this application, the liquid crystal / polymer dimming layer includes any one of polymer-dispersed liquid crystal, polymer-stabilized liquid crystal, or a combination of polymer-dispersed and stabilized liquid crystal. The liquid crystal / polymer dimming layer can switch its transmittance through electric field stimulation; its driving voltage is 5–100V, with a visible light transmittance change ≥40% and a response time ≤1s; more preferably, its driving voltage is 5–30V, with a visible light transmittance change ≥65% and a response time ≤0.5s.
[0068] Furthermore, when the liquid crystal / polymer dimming layer is a polymer-dispersed liquid crystal, its raw materials, by mass percentage, include: liquid crystal phase A 50-80 wt%, polymerizable monomer A 15-48.5 wt%, spacer particles 0.5-2 wt%, and photoinitiator 1 wt%. The driving voltage of the polymer-dispersed liquid crystal is 1-20V, the threshold voltage is 5-100V, the transmittance of visible light in the transmitted state is ≥65%, the transmittance of visible light in the scattered state is ≤15%, the change in visible light transmittance is ≥50%, the response time is ≤1s, and the thickness is 5-100μm.
[0069] Wherein, the liquid crystal phase A is a room temperature nematic liquid crystal or a mixture thereof, which may be any one of Merck E7, E8, E44, TL213, ZLI-4792, DIC SLC-1717, SLC-1011 or GXP-6033 liquid crystals; or, it may be a mixed liquid crystal composed of liquid crystal monomers of 5CB, 6CB, 5TB or 7CB.
[0070] The polymerizable monomer A is a photocurable low-shrinkage monomer, comprising at least one of the following compounds:
[0071] Trifunctional acrylate monomers, such as trimethylolpropane triacrylate;
[0072] Difunctional acrylates / methacrylates, such as HDDA, BDDA or PEGDA;
[0073] Monofunctional acrylates or methacrylates, such as IBOA, BMA or Bis-EMA;
[0074] Alternatively, isocyanate-modified polyurethane-acrylate or epoxy acrylate.
[0075] Furthermore, when the liquid crystal / polymer dimming layer is a polymer-stabilized liquid crystal, its raw materials, by mass percentage, include: liquid crystal phase B 68.5-95.5 wt%, polymerizable monomer B 2-30 wt%, spacer particles 0.5-2 wt%, and photoinitiator 1 wt%.
[0076] The polymer-stabilized liquid crystal can be electrically driven or temperature-regulated. The electrically driven type has a driving voltage of 1-20V, a threshold voltage of 5-100V, a visible light transmittance of ≥65% in the transmitted state, a visible light transmittance of ≤15% in the scattered state, a visible light transmittance change of ≥50%, a response time of ≤1s, and a thickness of 5-200μm. The temperature-regulated type has a visible light transmittance of ≥65% in the transmitted state, a visible light transmittance of ≤10% in the scattered state, a visible light transmittance change of ≥55%, a response time of ≤10s, and a thickness of 5-200μm.
[0077] When the liquid crystal / polymer dimming layer is a polymer-dispersed and stabilized liquid crystal, its raw materials, by mass percentage, include: liquid crystal phase B 50-80wt%, polymerizable monomer A 14-40wt%, polymerizable monomer B 2-10wt%, spacer particles 0.5-2wt%, and photoinitiator 0.5-3wt%.
[0078] The polymer-dispersed and stabilized liquid crystal can be electrically driven or temperature-regulated. The electrically driven type has a driving voltage of 1-20V, a threshold voltage of 5-80V, a visible light transmittance of ≥65% in the transmitted state, a visible light transmittance of ≤15% in the scattered state, a visible light transmittance change of ≥50%, a response time of ≤0.5s, and a thickness of 5-50μm. The temperature-regulated type has a visible light transmittance of ≥65% in the transmitted state, a visible light transmittance of ≤10% in the scattered state, a visible light transmittance change of ≥55%, a response time of ≤10s, and a thickness of 5-50μm.
[0079] In this application, the liquid crystal phase B includes at least one of cholesteric liquid crystal, inverted liquid crystal, or smectic-cholesteric phase transition liquid crystal. The cholesteric liquid crystal can be prepared by blending nematic mother liquors such as E7, E8, 5CB, GXP-6033, GXP-6022 with chiral dopants R811, S811, or CB15, wherein the amount of chiral dopant is 2-30 wt% of the amount of the nematic mother liquor, or by using existing commercially available cholesteric liquid crystal mixtures such as Merck BL-006 or HC-5000 series; the inverted liquid crystal can be selected from GXV-7822-180 or GXV-7822-179; the smectic-cholesteric phase transition liquid crystal can be prepared by blending nematic liquid crystal mother liquor with smectic liquid crystal molecules such as 8CB, 8OCB, 9CB, or 10CB, wherein chiral molecules such as S811 or R811 may also be added. The amount of nematic liquid crystal mother liquor used is 40-80 wt%, the amount of smectic liquid crystal molecules is 8-50 wt%, and the amount of chiral molecules is 0-30 wt%, by mass percentage.
[0080] In this application, the polymerizable monomer B is an optically anisotropic polymerizable monomer, including any one of 1,4-bis[4-(6-acryloyloxyhexyloxy)phenyl]octanoate (C6M), 1,4-bis[4-(3-acryloyloxypropoxy)phenyl]octanoate (C3M), or 4-(4-acryloyloxybutoxy)vinyl benzoate (C4V).
[0081] The initiator includes any one of Irgacure 1173, Irgacure 184, Irgacure 651, Irgacure 819 or TPO-L;
[0082] The spacer particles include any one of silica microspheres, organopolystyrene microspheres, or surface-modified nanocellulose.
[0083] In this application, the visible light transmittance of the outer surface layer is ≥50%. The infrared transparent layer in the outer surface layer is a polypropylene film or a polyethylene film with an infrared transmittance ≥80% and a thickness of 0.1–1 mm; preferably, it is a polypropylene film with a thickness of 0.3–0.6 mm.
[0084] In the outer surface layer, the infrared reflective layer is used to reflect mid- and far-infrared thermal radiation. Its material is selected from at least one of indium tin oxide, silver nanowires, copper, gold, or graphene, and its thickness is 20-100 nm with a sheet resistance of 10-200 Ω / sq. Preferably, it is silver nanowires or indium tin oxide, and more preferably, its thickness is 20-80 nm.
[0085] In the outer surface layer, a vanadium dioxide nanoparticle layer is used to regulate the infrared transmission and low infrared reflection states below the phase transition point, and the infrared reflection and low infrared transmission states above the phase transition point. The doping material includes at least one of tungsten, molybdenum, niobium, or fluorine, with a doping concentration of 1–5 at%, and a phase transition temperature range of 10–45°C. Tungsten is preferred as the doping material, with the phase transition temperature adjusted to 18–45°C and a doping concentration of 1–2 at%.
[0086] In this application, the inner surface layer is used to provide structural support and electrical drive. The transparent substrate of the inner surface layer is made of at least one of glass, polypropylene, polyethylene, polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polyvinyl chloride, or transparent nylon, and has a thickness of 0.5-20 mm; preferably polyethylene terephthalate, with a thickness preferably of 0.1-0.3 mm.
[0087] In the inner surface layer, the conductive layer is made of at least one of indium tin oxide, silver nanowires, graphene, silver, gold, or copper, with a visible light transmittance ≥85%, a sheet resistance of 10–200 Ω / sq, and a thickness of 20–100 nm. Preferably, it is indium tin oxide, with a thickness of 20–50 nm and a sheet resistance ≤100 Ω / sq.
[0088] The intelligent window of this application has an intermediate layer of PDLC, PSLC, or PD&SLC that reversibly switches the orientation of liquid crystal molecules or the phase state of liquid crystal through electric field or temperature stimulation, dynamically adjusting visible light transmission (transparent state → scattering state); the vanadium dioxide doped outer surface layer can switch near-infrared transmittance at phase transition temperature to achieve high transmittance at low temperature, allowing heat to enter; and low transmittance at high temperature, reducing heat entry; the infrared reflective layer reflects indoor thermal radiation (heat preservation) at low temperature, and forms a Fabry-Perot resonant cavity with the infrared emitting layer through the vanadium dioxide doped layer to achieve high emissivity and dissipate heat at high temperature.
[0089] Based on this, the smart window of this application can achieve multiple coordinated regulation of sunlight and thermal radiation, with a wide regulation band, fast response speed, and good energy-saving effect. Its regulation band covers the visible light, near-infrared, and mid-far-infrared range, and can reversibly change with the ambient temperature. At low temperatures, it presents a transparent, low-emission heat-preserving state, while at high temperatures, it presents a scattering, high-emission heat-dissipating state; it can achieve energy saving all year round and all weather, and is suitable for various climate regions.
[0090] The smart window of this application exhibits highly efficient energy-saving performance. At high temperatures, it cools the room by using high emissivity and low transmittance, refracting and reflecting most sunlight while absorbing a small portion, significantly reducing heat entering the room and increasing heat loss to the outside; this lowers the indoor temperature and saves energy consumption in the cooling system. At low temperatures, it displays low emissivity and high transmittance, absorbing most sunlight entering the room while reflecting a small portion, reducing heat loss from the interior to the outside, maintaining indoor lighting and temperature, and reducing energy consumption in the heating system. Simulation tests show that compared to ordinary glass, the smart window of this application can reduce indoor temperature by 8-15℃ in summer and improve insulation efficiency by 15-25% in winter.
[0091] Meanwhile, the smart window of this application can respond quickly to changes in the external environment. Under electric field response, the light transmission adjustable layer response time is ≤1 second; while under temperature stimulation, the light transmittance adjustable response time is ≤10 seconds, and the vanadium dioxide doped phase transition response is ≤10 seconds.
[0092] Secondly, this application provides a method for preparing the aforementioned smart window, comprising:
[0093] An infrared reflective layer and a vanadium dioxide nanoparticle layer are deposited on two opposite surfaces of the infrared transparent layer to obtain the outer surface layer.
[0094] Specifically, an infrared reflective layer and a low-phase-transition-temperature doped vanadium dioxide nanoparticle layer are deposited on both sides of the infrared transparent layer by magnetron sputtering, blade coating, spraying, or spin coating.
[0095] A conductive layer is deposited on one surface of a transparent substrate to obtain an inner surface layer;
[0096] Specifically, conductive layers are prepared on transparent substrates using methods such as thermal evaporation, magnetron sputtering, blade coating, spraying, or spin coating.
[0097] A prepolymer is obtained by mixing liquid crystal mixture, polymerizable monomer, initiator and spacer particles. The prepolymer is then extruded between the infrared reflective layer of the outer surface layer and the conductive layer of the inner surface layer through a roll-to-roll process. The prepolymer is then cured by photopolymerization or thermal polymerization to obtain a smart window.
[0098] This application uses a roll-to-roll process to prepare the liquid crystal layer, which has high production efficiency and material utilization, low production cost, and is suitable for large-scale production.
[0099] The smart window of this application can achieve multiple coordinated control of sunlight and heat radiation. It has a wide control band, fast response speed and good energy saving effect. It can be used in building windows, vehicle windows or photovoltaic modules.
[0100] This application also provides an intelligent temperature control system, which includes the aforementioned intelligent window for multi-modal adjustment of sunlight and thermal radiation. The intelligent temperature control system can achieve dual regulation of solar energy and thermal radiation through the intelligent window, thereby enabling temperature management.
[0101] The present application will be further described below through specific embodiments.
[0102] Example 1
[0103] This embodiment provides a method for preparing a smart window with a polymer-dispersed liquid crystal as the liquid crystal / polymer dimming layer, including:
[0104] 1. Preparation of outer surface layer:
[0105] S1. A 0.5 mm thick polypropylene film was cleaned with acetone, ethanol and deionized water respectively and then dried with nitrogen. The film was then treated in a plasma cleaner with a power of 50 W for 3 min to obtain an infrared transparent layer.
[0106] S2, an ITO layer with a thickness of 50 nm and a sheet resistance of 30 Ω / sq is deposited by magnetron sputtering on one surface of a polypropylene film.
[0107] S3, add 4g of vanadium dioxide doped with 2at% tungsten (phase transition temperature 25℃) and 500mg of polyvinylpyrrolidone to 40mL of ethanol, stir at room temperature for 24 hours, and take 200μL of the supernatant; drop the supernatant onto another surface of the polypropylene film for spin coating at 1000rpm, and let it air dry to obtain the outer surface layer.
[0108] 2. Preparation of the inner surface layer:
[0109] S1. Clean 0.5mm thick PET with acetone, ethanol and deionized water respectively, then dry with nitrogen, and treat with 50W power in a plasma cleaner for 3 minutes to make a transparent substrate.
[0110] S2, silver nanowires with a diameter of 70 nm and a length of 45 μm were dispersed in ethanol to prepare a silver nanowire dispersion with a solid content of 5 mg / mL; the dispersion was spin-coated onto a PET surface at 1000 rpm for 30 s, and then dried on a hot plate at 80 °C for 2 minutes to obtain the inner surface layer.
[0111] 3. Smart Window Preparation:
[0112] S1. Mix the following raw materials thoroughly to prepare a prepolymer solution. It comprises, by mass percentage:
[0113] Mixed liquid crystal E870 wt%, a mixture of isoborneol acrylate IBOA and 1,4-butanediol diacrylate BDDA in a mass ratio of 4:1 28.5 wt%, Irgacure 65 11.0 wt%, and polystyrene microspheres with a diameter of 20 μm 0.5 wt%;
[0114] S2, the prepolymer liquid is coated between the infrared reflective layer of the outer surface layer and the conductive layer of the inner surface layer, and the thickness is controlled to 20 μm by roller extrusion. It is then applied using a wavelength of 365 nm and an energy density of 7.5 mw / cm². 2 The film is cured by ultraviolet radiation for 20 minutes to form a PDLC film with a thickness of 20 μm, thus obtaining the smart window.
[0115] Example 2
[0116] This embodiment provides a method for preparing a smart window with a polymer-stabilized liquid crystal layer as the liquid crystal / polymer dimming layer, including:
[0117] 1. Preparation of outer surface layer:
[0118] S1. A 0.5 mm thick polypropylene film was cleaned with acetone, ethanol and deionized water respectively and then dried with nitrogen. The film was then treated in a plasma cleaner with a power of 50 W for 3 min to obtain an infrared transparent layer.
[0119] S2, a silver layer with a thickness of 30 nm and a sheet resistance of 50 Ω / sq is deposited by magnetron sputtering on one surface of a polypropylene film as an infrared reflective layer.
[0120] S3, add 2g of vanadium dioxide doped with 2at% tungsten (phase transition temperature 25℃) and 200mg of polymethyl methacrylate to 20mL of ethanol, stir at room temperature for 24 hours, and take 200μL of the supernatant; drop the supernatant onto another surface of the polypropylene film for spin coating at 1000rpm, and let it air dry to obtain the outer surface layer.
[0121] 2. Preparation of the inner surface layer:
[0122] S1. Clean the PP film with a thickness of 0.5mm with acetone, ethanol and deionized water respectively, then dry it with nitrogen, and treat it in a plasma cleaner with a power of 50W for 3 minutes to make a transparent substrate.
[0123] S2, under nitrogen protection, silver was deposited on one surface of a PP film using a magnetron sputtering coating machine to obtain an inner surface layer. The DC sputtering power was 100W, the working pressure was 1.0Pa, the coating time was 3 minutes, and the film was then annealed at 120℃ for 30 minutes.
[0124] 3. Smart Window Preparation:
[0125] S1. Mix the following raw materials thoroughly to prepare a prepolymer solution. It comprises, by mass percentage:
[0126] The mixture consisted of 95.5 wt% of a 4:1 mixture of liquid crystals E8 and 8CB, 3.0 wt% of C6M, 1.0 wt% of Irgacure 65, and 0.5 wt% of silica microspheres with a diameter of 30 μm.
[0127] S2, the above prepolymer liquid is coated between the infrared reflective layer on the outer surface layer and the conductive layer on the inner surface layer, and the thickness is controlled to 30μm by roller extrusion. It is then tested with a wavelength of 365nm and an energy density of 5mw / cm². 2 The film is cured by ultraviolet radiation for 15 minutes to form a PSLC film with a thickness of 30 μm, thus obtaining the smart window.
[0128] Example 3
[0129] This embodiment provides a method for preparing a smart window where the liquid crystal / polymer dimming layer is a polymer-dispersed and stabilized liquid crystal layer, including:
[0130] 1. Preparation of outer surface layer:
[0131] S1. A 0.5 mm thick polypropylene film was cleaned with acetone, ethanol and deionized water respectively and then dried with nitrogen. The film was then treated in a plasma cleaner with a power of 50 W for 3 min to obtain an infrared transparent layer.
[0132] S2, a silver layer with a thickness of 25 nm and a sheet resistance of 80 Ω / sq is deposited by magnetron sputtering on one surface of a polypropylene film as an infrared reflective layer.
[0133] S3, add 4g of vanadium dioxide doped with 1.5at% tungsten (phase transition temperature 30℃) and 40mg of polymethyl methacrylate to 40mL of ethanol, stir at room temperature for 24 hours, and take 200μL of the supernatant; drop the supernatant onto another surface of the polypropylene film for spin coating at 1000rpm, and dry it on a hot table at 50℃ to obtain the outer surface layer.
[0134] 2. Preparation of the inner surface layer:
[0135] S1. Clean a 0.5mm thick quartz glass sheet with acetone, ethanol and deionized water respectively, then dry it with nitrogen gas, and treat it in a plasma cleaner with a power of 50W for 3 minutes to make a transparent substrate.
[0136] S2, using a vacuum coating machine, silver is deposited on one surface of a quartz glass slide to obtain an inner surface layer. The deposition rate is... Vacuum degree <10 -5 The silver plating time is 200 seconds; after plating, the film is annealed in a vacuum at a temperature of 120°C for 30 minutes.
[0137] 3. Smart Window Preparation:
[0138] S1. Mix the following raw materials thoroughly to prepare a prepolymer solution. It comprises, by mass percentage:
[0139] The mixture consisted of 65.5 wt% of a mixture of E8 and 8CB liquid crystals in a 4:1 mass ratio, 3.0 wt% of C6M, 30 wt% of a mixture of isoborneol acrylate IBOA and 1,4-butanediol diacrylate BDDA in a 4:1 mass ratio, 1.0 wt% of Irgacure 65, and 0.5 wt% of silica microspheres with a diameter of 20 μm.
[0140] S2, the prepolymer liquid is coated between the infrared reflective layer on the outer surface and the conductive layer on the inner surface, and the thickness is controlled to 20 μm by roller extrusion. It is then tested with a wavelength of 365 nm and an energy density of 5 mw / cm². 2 It was cured by ultraviolet irradiation for 40 seconds, and then cured with a wavelength of 365nm and an energy density of 0.5mw / cm². 2 The film was cured by ultraviolet radiation for 15 minutes to obtain a PD&SLC film with a thickness of 20 μm, thus obtaining the smart window.
[0141] The outer surface layer of Example 1 was observed on both sides using a field emission scanning electron microscope (Regulus 8220) and an energy dispersive spectroscopy (EDS) instrument. The results are as follows: Figure 2 and Figure 3 As shown. Among them, Figure 2 The left image is a SEM image of the infrared reflective layer. Figure 2 The right image shows the EDS diagram of the infrared reflective layer; Figure 3 The left image is a SEM image of the vanadium dioxide doped layer. Figure 3 The middle image is the EDS diagram of the vanadium dioxide doped layer with V. Figure 3 The right figure shows the EDS diagram of W element in the vanadium dioxide doped layer.
[0142] from Figure 2 and Figure 3As can be seen, the elemental signals are distributed in a dotted pattern throughout the image, without any obvious large particle agglomeration or segregation, indicating that uniform silver nanowire layers and tungsten-doped vanadium dioxide layers have been deposited on both sides of the outer surface layer, with good dispersion.
[0143] The light transmittance of the smart window in Example 1 was measured using a variable-temperature UV-Vis-NIR spectrophotometer in both the transparent and scattering states. The test wavelengths were 300-2500 nm. The results are as follows: Figure 4 As shown. From Figure 4 It can be seen that there is a significant difference in transmittance between the visible light band and the near-infrared light band. The difference in ΔT in the visible light band is close to 70%, presenting a high contrast. It allows sunlight energy input at low temperatures and blocks sunlight at high temperatures, thus realizing the dimming performance of the thermochromic smart window.
[0144] The emissivity curves of the smart window in Example 1 in the 8-14 μm range were measured using a Fourier transform infrared spectrometer, and the results are as follows: Figure 5 As shown. From Figure 5 It can be seen that the emissivity of the sample changes significantly with increasing temperature. It is in a high emissivity state at high temperature and maintains a medium emissivity at room temperature, showing thermally tunable emissivity. When heated, it automatically enhances mid-infrared radiation, which helps with spontaneous heat dissipation. At low temperature, it reduces radiation and reduces heat loss, proving that the material has a reversible and high-amplitude temperature-sensitive emissivity regulation capability in the atmospheric window band.
[0145] The light transmittance of the smart window in Example 2 was measured using a variable-temperature UV-Vis-NIR spectrophotometer in both the transparent state (low temperature 25℃) and the scattering state (high temperature 50℃). The test wavelengths were 300-2500nm. The test results are as follows: Figure 6 As shown. From Figure 6 It can be seen that the transmittance in the visible light region is stable at 70% at 25℃ and remains at an extremely low transmittance of <10% at 50℃, with the sample exhibiting strong scattering and visible light modulation amplitude close to 60%. In the near-infrared region, the transparent state maintains a high transmittance of 60%-70%, which is beneficial for obtaining heat from sunlight during winter heating. In the scattering state, the transmittance drops to 10%, significantly weakening near-infrared radiation, thus achieving the effect of blocking solar radiation in hot conditions and maintaining high transmittance at low temperatures to achieve adaptive energy-saving effect.
[0146] The cross-sectional morphology of the intermediate PD & SLC layer in Example 3 was observed using a field emission scanning electron microscope (Regulus 8220), as shown below. Figure 7 As shown. Figure 7 This indicates that the intermediate PD&SLC film of Example 3 has a highly porous layered structure inside, and there is also a vertical network inside the pores, which realizes the construction of polymer dispersion and stable liquid crystal system and improves light scattering and dimming performance.
[0147] Although this application has been described in detail in this specification with general descriptions and specific embodiments, some modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, such modifications or improvements made without departing from the spirit of this application are all within the scope of protection claimed in this application.
Claims
1. A smart window with multiple modes for adjusting sunlight and thermal radiation, characterized in that, It includes an outer surface layer, a middle layer, and an inner surface layer that are stacked in sequence; The outer surface layer includes an infrared transparent layer, and an infrared reflective layer and a vanadium dioxide doped layer respectively disposed on two opposite surfaces of the infrared transparent layer; The inner surface layer includes a transparent substrate and a conductive layer attached to one side surface of the transparent substrate; The intermediate layer is a liquid crystal / polymer dimming layer, with one side of the liquid crystal / polymer dimming layer bonded to the infrared reflective layer and the other side bonded to the conductive layer.
2. The smart window according to claim 1, characterized in that, The liquid crystal / polymer dimming layer includes any one of polymer-dispersed liquid crystal, polymer-stabilized liquid crystal, or polymer-dispersed and stabilized liquid crystal.
3. The smart window according to claim 1, characterized in that, The transmittance of the liquid crystal / polymer dimming layer can be switched by electric field stimulation; Its driving voltage is 5-100V, visible light transmittance change is ≥40%, and response time is ≤1s.
4. The smart window according to claim 2, characterized in that, The polymer-dispersed liquid crystal comprises, by mass percentage: liquid crystal phase A 50-80 wt%, polymerizable monomer A 15-48.5 wt%, spacer particles 0.5-2 wt%, and photoinitiator 1 wt%. Wherein, the liquid crystal phase A is a room temperature nematic liquid crystal or a mixture thereof; the polymerizable monomer A is a photocurable low-shrinkage monomer; And / or, The polymer-stabilized liquid crystal comprises, by mass percentage: liquid crystal phase B 68.5–95.5 wt%, polymerizable monomer B 2–30 wt%, spacer particles 0.5–2 wt%, and photoinitiator 1 wt%. And / or, The polymer-dispersed and stabilized liquid crystal comprises, by mass percentage: liquid crystal phase B 50-80 wt%, polymerizable monomer A 14-40 wt%, polymerizable monomer B 2-10 wt%, spacer particles 0.5-2 wt%, and photoinitiator 0.5-3 wt%. Wherein, the liquid crystal phase B includes at least one of cholesteric liquid crystal, inverted liquid crystal, or smectic-cholesteric phase transition liquid crystal, and the polymerizable monomer B is a polymerizable monomer with optical anisotropy.
5. The smart window according to claim 4, characterized in that, The polymerizable monomer A includes at least one of trimethylolpropane triacrylate, HDDA, BDDA, PEGDA, IBOA, BMA, Bis-EMA, isocyanate-modified polyurethane-acrylate, or epoxy acrylate. The polymerizable monomer B includes any one of 1,4-bis[4-(6-acryloyloxyhexyloxy)phenyl]octanoate, 1,4-bis[4-(3-acryloyloxypropoxy)phenyl]octanoate, or 4-(4-acryloyloxybutoxy)vinyl benzoate. The initiator includes any one of Irgacure 1173, Irgacure 184, Irgacure 651, Irgacure 819 or TPO-L; The spacer particles include any one of silica microspheres, organopolystyrene microspheres, or surface-modified nanocellulose.
6. The smart window according to claim 1, characterized in that, The visible light transmittance of the outer surface layer is ≥50%; The infrared transparent layer is a polypropylene film or a polyethylene film; the infrared transmittance of the infrared transparent layer is ≥80%; The infrared reflective layer is made of at least one of indium tin oxide, silver nanowires, copper, gold, or graphene.
7. The smart window according to claim 1, characterized in that, The doping material of the vanadium dioxide layer includes at least one of tungsten, molybdenum, niobium or fluorine. The doping concentration of the vanadium dioxide layer is 1–5 at%, and the phase transition temperature range is 10–45 °C. And / or, The transparent substrate is made of at least one of glass, polypropylene, polyethylene, polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polyvinyl chloride, or transparent nylon. And / or, The conductive layer is made of at least one of indium tin oxide, silver nanowires, graphene, silver, gold, or copper, and the visible light transmittance of the conductive layer is ≥85%.
8. The method for preparing the smart window according to claim 1, characterized in that, include: An infrared reflective layer and a vanadium dioxide-doped layer are deposited on two opposite surfaces of the infrared transparent layer to obtain the outer surface layer. A conductive layer is deposited on one surface of a transparent substrate to obtain an inner surface layer; A prepolymer is obtained by mixing liquid crystal mixture, polymerizable monomer, initiator and spacer particles. The prepolymer is then extruded between the infrared reflective layer of the outer surface layer and the conductive layer of the inner surface layer through a roll-to-roll process. The prepolymer is then cured by photopolymerization or thermal polymerization to obtain a smart window.
9. The application of the intelligent window with multiple modes of solar radiation and thermal radiation as described in any one of claims 1-7 in building windows, vehicle windows, or photovoltaic modules.
10. An intelligent temperature control system, characterized in that, It includes the intelligent window with multiple modes of adjustment of sunlight and thermal radiation as described in any one of claims 1-7.
Citation Information
Cited By
Self-adaptive heat dissipation electronic heat management composite material as well as preparation method and application thereof
CN122213479A
An adaptive heat dissipation electronic thermal management composite material and preparation method and use thereof
CN122213479B